Wire rod XYL82B for prestressed steel strand with specification of 16mm and production method of wire rod XYL82B

By adopting the billet-fired material production method and the rolling and cooling control process, the strength and plasticity of the 16mm specification prestressed steel strands are improved, and the problem of high production cost of high-strength strands in the existing technology is solved, and the Low-cost and high-efficiency production meets the high-strength stranded wire requirements of Φ21.6mm specification 1860MPa level.

CN118880168APending Publication Date: 2024-11-01HUNAN VALIN XIANGTAN IRON & STEEL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410909028.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to produce high-strength, uniformly structured 16mm specification prestressed steel strands for 16mm specifications at low cost, and the production cost is relatively high, making it difficult to meet the high-strength strand requirements of Φ21.6mm specifications of 1860MPa.

Method used

The production method of square billet-fired material is adopted to improve the silicon content component system, combine it with the controlled rolling and cold control process to ensure the strength and plasticity of the strips. The strength of hot-rolled strips is achieved through converter smelting, LF refining, continuous casting and rolling processes. It reaches 1200~1250MPa, meeting the requirements of high-strength stranded wire.

Benefits of technology

The low-cost production of high-strength 16mm specification prestressed steel strands is achieved. The cost is 300-500 yuan/ton lower than that of the second fire material, and the energy consumption and environmental problems caused by the second fire billet are avoided, which improves the Production efficiency and product competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880168A_ABST
    Figure CN118880168A_ABST
Patent Text Reader

Abstract

The invention provides a steel wire rod XYL82B for a prestressed steel strand with the specification of 16 mm and a production method. The steel wire rod XYL82B comprises the following chemical components in percentage by weight: 0.80-0.85% of C, 0.40-0.60% of Si, 0.70-0.80% of Mn, 0.20-0.25% of Cr, less than or equal to 0.015% of P, less than or equal to 0.010% of S, less than or equal to 0.10% of Ni, less than or equal to 0.10% of Cu, less than or equal to 0.02% of Al, less than or equal to 0.002% of O, less than or equal to 0.005% of N, less than or equal to 0.0100% of Sn, less than or equal to 0.0100% of As and the balance of Fe and inevitable impurities. According to the method, a square billet of 180 * 180mm < 2 > and a fire material are adopted for rolling the specification of phi 16mm, a reasonably-designed component system and advanced smelting and controlled rolling and controlled cooling processes are mainly adopted, generation of abnormal structures of the wire rod is effectively inhibited, meanwhile, the tensile strength and sorbite rate of the wire rod are improved, the plasticity of the wire rod is improved, and meanwhile, waste heat of the wire rod enters a heat preservation vestibule, so that online aging is achieved. The strength of the wire rod reaches 1200 MPa or above, and the requirement for producing 1860 MPa grade 21.6 mm steel strands is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel smelting, and specifically relates to a wire rod XYL82B for prestressed steel strands with a specification of 16 mm and a production method thereof. Background Art

[0002] XYL82B wire rod is the raw material for high-strength steel strand deep processing products. It is used to make Φ21.6mm specification 1860MPa grade mining steel strand. The cold working reduction rate of each part is above 80%. It is 100% inspected from beginning to end during the drawing and twisting process. Under high stress, any defect is a source of breakage. Therefore, it is extremely difficult to achieve a very low wire breakage rate, which is also the main sign of success. The main technical features of XYL82B wire rod are large cross-section, high strength and high cold drawing performance. Improving strength, product homogenization, and ensuring that the wire rod has a good high cold drawing effect are the difficulties in the research and development of this product. At present, many wire rod manufacturers have done a lot of research, but they can only use two-fire material forming process or strengthen with alloy elements such as V, Nb, Ti to ensure product quality, and the production cost is relatively high. Therefore, it is urgent to find a method for producing high-strength steel strand wire rod XYL82B with stable performance and uniform structure using one-fired steel rolling, which has low production cost and large diameter φ16mm mining steel strand wire rod. Summary of the invention

[0003] To achieve the above-mentioned purpose, the present invention provides a 16mm specification prestressed steel strand wire rod XYL82B and a production method, which solves the problems existing in the prior art.

[0004] The present invention provides a production method for a wire rod for a 16mm prestressed steel strand, which uses a square billet-fired material to produce a Φ16mm prestressed steel strand wire rod, mainly adopting a component system with an appropriate increase in silicon content to improve the strength of the wire rod and improve the strength and plasticity of the wire rod, and adopting a reasonable controlled rolling and controlled cooling process to ensure the troostitization rate of the wire rod, while ensuring the strength of the steel wire and improving the plasticity of the wire rod. The strength of the hot-rolled wire rod reaches 1200-1250MPa, which meets the use requirements of making a Φ21.6 specification 1860MPa grade high-strength strand, and the cost of the square billet-fired material is low.

[0005] The present invention adopts 180*180mm2 square billet and one-stage hot-rolled material to produce XYL82B hot-rolled wire rod. The parent material is not subjected to billet opening, lead bath or salt bath heat treatment, and the single wire strength of the stranded wire can meet the requirement of 1860MPa standard steel stranded wire.

[0006] The technical solution of the present invention is:

[0007] A wire rod XYL82B for prestressed steel strands with a specification of 16 mm, the chemical composition and weight percentage of the wire rod XYL82B are: C: 0.80-0.85%, Si: 0.40-0.60%, Mn: 0.70-0.80%, Cr: 0.20-0.25%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.02%, O≤0.002%, N≤0.005%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

[0008] In the above scheme, the strength of the wire rod XYL82B reaches above 1200MPa.

[0009] In the above scheme, the wire rod XYL82B meets the technical requirements for producing high-strength steel wire with a specification of Φ21.6mm and a strength level of 1860MPa.

[0010] A production method of 16mm prestressed steel strand wire rod XYL82B, comprising the following steps:

[0011] Converter smelting: The converter adopts double slag method, and the steel tapping adopts slide plate to block the slag;

[0012] LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system;

[0013] Continuous casting: adopts full-process protection pouring, constant casting speed production, low superheat pouring, using crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology, and combined with the strong cooling process of water cooling + gas mist cooling in the secondary cooling zone;

[0014] Rolling: The rolling adopts walking beam heating furnace, and the finishing rolling adopts "8+4" mode, that is, 8-stand finishing rolling unit and 4-stand sizing unit rolling. The wire rod size is measured in real time by online diameter gauge, and the Stelmor air cooling line is used for cooling, and the insulation corridor is used for insulation.

[0015] Preferably, the casting speed during the continuous casting process is controlled at 1.55-1.6 m / min, and the superheat is stabilized at 20-30°C.

[0016] It is further preferred that square billets with a cross-section of 180*180mm2 are used in the continuous casting process, the electromagnetic stirring current of the crystallizer is 400A, the frequency is 3.5Hz, the end electromagnetic stirring current is 700A, the frequency is 10Hz, the total reduction is 25mm, and the water volume of the continuous casting secondary cooling water is 0.45L / Kg.

[0017] More preferably, the steel billet after continuous casting is slowly cooled for 24 hours and then hot rolled.

[0018] Further preferably, the main process parameters of the rolling are: heating in the heating furnace for one stage at 1000°C, heating in the second stage at 1150-1160°C, soaking section at 1180°C, finishing mill at 890°C, warping mill at 920°C, wire laying at 840-860°C; roller speed at 0.5 m / s; total heating time in the heating furnace at 120-150 min.

[0019] Further preferably, the air cooling parameters of the Stelmore air cooling line are: 17 fans, each fan has an air volume of 200,000 m3 / h and an air pressure of 3000Pa.

[0020] Further preferably, the process parameters of the insulation corridor are: temperature entering the insulation corridor is 450-550°C, and the insulation time is more than 180 minutes.

[0021] The principle of the present invention is as follows: high Si content can improve the strength of the wire rod, improve the elastic limit and fatigue strength of the steel, and have a certain promoting effect on reducing the spacing between the sorbite lamellae; Cr content can greatly improve the strength of the wire rod, and chromium can improve the stability of austenite, shift the C curve to the right, reduce the critical cooling rate, and improve the hardenability of the steel, thereby further reducing the probability of network carbon formation; Mn can improve the strength of the steel without affecting the shrinkage of the material; Al can refine the grains and improve the strength. In addition, by increasing the diameter of the wire rod, the drawing compression rate is increased, and the strength of the stranded wire is improved.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention adopts a square billet-fired material to produce a Φ16mm specification 82 grade hot-rolled wire rod, and adopts an advanced controlled rolling and controlled cooling process to ensure the sorbitization rate of the wire rod, ensure the strength of the steel wire while improving the plasticity of the wire rod, and realize online aging, so that the strength of the hot-rolled wire rod reaches more than 1200MPa, which meets the use requirements of making a Φ21.6 specification 1860MPa high-strength stranded wire;

[0024] 2. The present invention adopts square billet one-fired material to produce XYL82B ultra-high strength stranded wire steel, and the cost is 300-500 yuan / ton lower than that of two-fired material, and 150-250 yuan / ton lower than that of micro-alloyed wire rod. The product is highly competitive, and there is no energy consumption generated by two-fired billet opening and environmental problems caused by heat treatment waste liquid. It can be shipped and used as soon as it comes off the production line, thereby improving production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 This is the metallographic structure (500 times) of Example 1;

[0027] Figure 2 This is the metallographic structure (500 times) diagram of Example 2. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0030] The chemical composition and weight percentage of the wire rod for prestressed steel strand with a specification of 16 mm described in the present invention are: C: 0.80-0.85%, Si: 0.40-0.60%, Mn: 0.70-0.80%, Cr: 0.20-0.25%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.02%, O≤0.002%, N≤0.005%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

[0031] The production process is: BOF (converter) → LF refining → 180*180mm2 continuous casting → slow cooling of billet → high-speed wire rolling.

[0032] Special molten iron and clean scrap steel are used for steelmaking; constant pulling speed, low superheat pouring, strong cooling process, electromagnetic stirring of crystallizer, electromagnetic stirring at the end, light and heavy pressure reduction and full protection pouring are adopted for continuous casting; after the billet is slowly cooled, reasonable controlled rolling and controlled cooling process is adopted for rolling.

[0033] The chemical composition and weight percentage of the wire rod XYL82B are: C: 0.82%, Si: 0.51%, Mn: 0.75%, Cr: 0.23%, P: 0.007%, S: 0.006%, Ni: 0.03%, Cu: 0.02%, Al: 0.02%, O: 0.0016%, N: 0.004%, Sn: 0.0015%, As: 0.0041%, and the balance is iron and unavoidable impurities; or C: 0.83%, Si: 0.52%, Mn: 0.76%, Cr: 0.21%, P: 0.009%, S: 0.008%, Ni: 0.02%, Cu: 0.03%, Al: 0.02%, O: 0.0014%, N: 0.004%, Sn: 0.0016%, As: 0.0048%, and the balance is iron and unavoidable impurities.

[0034] The wire rod strength reaches above 1200 MPa.

[0035] The wire rod meets the technical requirements for producing high-strength stranded wire with a specification of Φ21.6 mm and a strength level of 1860 MPa.

[0036] A method for producing a wire rod for a 16 mm prestressed steel strand comprises the following steps:

[0037] Converter smelting: In order to control harmful residual elements, special molten iron is selected, and the S content of the molten iron is reduced through molten iron pretreatment.

[0038] The converter adopts the double slag method to effectively reduce the phosphorus content, and the slide plate is used to block the slag during steel discharge to prevent slag from falling from the converter, thereby controlling the purity of the molten steel from the source.

[0039] LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system.

[0040] Continuous casting: Continuous casting adopts 180*180mm2 section for production, adopts integral tundish for full protection casting, the continuous casting furnace pulling speed is controlled at 1.55~1.6m / min, the superheat is stable at 20~30℃, the crystallizer, the end electromagnetic stirring, the light and heavy pressure reduction technology are used, and the continuous casting secondary cooling section water cooling plus aerosol cooling is adopted to reduce the columnar crystal area, increase the equiaxed crystal area, prevent the development of columnar crystals, reduce the component segregation of molten steel during solidification, and improve the core and surface quality of continuous casting billet. Specific parameters: crystallizer electromagnetic stirring current 400A, frequency 3.5Hz, end electromagnetic stirring current 700A, frequency 10Hz, total pressure reduction 25mm, continuous casting secondary cooling water specific water volume 0.45L / Kg.

[0041] Slow cooling of steel billet: After slow cooling of steel billet for 24 hours, hot rolling is carried out;

[0042] Rolling: A walking beam heating furnace is used, with a total of 30 rolling mills. The finishing rolling adopts the "8+4" mode, i.e., 8-stand finishing rolling mill and 4-stand sizing mill. The wire rod size is measured in real time through an online diameter gauge to ensure that the wire rod size accuracy reaches Class C accuracy. The main process parameters of the rolling are: heating furnace heating stage 1000℃, heating stage 2 1150℃, soaking stage 1180℃, finishing mill 890℃, warping mill 920℃, wire laying 840℃~860℃; roller speed 0.5m / s; total heating time of the heating furnace 120~150min. The air cooling parameters of the Stelmor air cooling line are: a total of 17 fans are turned on, each fan has a rated air volume of 200,000 m3 / h, and an air pressure of 3000Pa.

[0043] Embodiment 1:

[0044] A method for producing a wire rod XYL82B for a 16mm prestressed steel strand, wherein the chemical composition and weight percentage of the wire rod XYL82B are: C: 0.82%, Si: 0.51%, Mn: 0.75%, Cr: 0.23%, P: 0.007%, S: 0.006%, Ni: 0.03%, Cu: 0.02%, Al: 0.02%, O: 0.0016%, N: 0.004%, Sn: 0.0015%, As: 0.0041%, and the remainder is iron and unavoidable impurities.

[0045] Converter smelting: In order to control harmful residual elements, special molten iron is selected, and the S content of the molten iron is reduced through molten iron pretreatment.

[0046] The converter adopts the double slag method to effectively reduce the phosphorus content, and the slide plate is used to block the slag during steel discharge to prevent slag from falling from the converter, thereby controlling the purity of the molten steel from the source.

[0047] LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system.

[0048] Continuous casting: Continuous casting adopts 180*180mm2 section for production, adopts integral tundish for full protection casting, the continuous casting furnace pulling speed is controlled at 1.55m / min, the superheat is stable at 22~36℃, the crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology are used, and the continuous casting secondary cooling section water cooling plus aerosol cooling is adopted to reduce the columnar crystal area, increase the equiaxed crystal area, prevent the development of columnar crystals, reduce the component segregation of molten steel during solidification, and improve the core and surface quality of continuous casting billet. Specific parameters: crystallizer electromagnetic stirring current 400A, frequency 3.5Hz, end electromagnetic stirring current 700A, frequency 10Hz, total pressure reduction 25mm, continuous casting secondary cooling water specific water volume 0.45L / Kg.

[0049] Slow cooling of steel billet: After slow cooling of steel billet for 24 hours, hot rolling is carried out;

[0050] Rolling process parameters: heating furnace heating stage 1000℃, heating stage 2 1160℃, equalizing stage 1180℃, finishing mill 890℃, warping mill 920℃, spinning 850℃; roller speed 0.5m / s; total heating time of heating furnace 138min. Air cooling parameters: the first 17 fans are all running at full load, the rated air volume of each fan is 200,000 m3 / h, and the air pressure is 3000Pa. Rapid strong cooling is achieved through the Stelmor air cooling line, which suppresses abnormal structures such as martensite. The temperature entering the insulation corridor is 500-550℃, and the insulation time is 195 minutes. A sorbite structure with high strength and good plasticity is generated. The sorbite structure content reaches 85%, such as Figure 1 shown.

[0051] The tensile strength of the ultra-high strength wire rod XYL82B produced in Example 1 is 1220MPa, the network carbide is evenly distributed, the network carbon level is ≤1.0, and no martensite appears. The 21.6mm specification 1860Mpa grade steel wire made by the wire rod has an actual strength of 1901MPa for the finished single wire.

[0052] Example 2

[0053] A wire rod XYL82B for prestressed steel strands with a specification of 16 mm. The difference between this embodiment 2 and embodiment 1 is that the chemical composition and weight percentage of the wire rod XYL82B are: C: 0.83%, Si: 0.52%, Mn: 0.76%, Cr: 0.21%, P: 0.009%, S: 0.008%, Ni: 0.02%, Cu: 0.03%, Al: 0.02%, O: 0.0014%, N: 0.004%, Sn: 0.0016%, As: 0.0048%, and the remainder is iron and unavoidable impurities.

[0054] In the production process of manufacturing wire rods in this embodiment 2, the superheat of the tundish is controlled at 25°C, the continuous casting speed is controlled at 1.6m / min, the electromagnetic stirring current of the crystallizer is 400A, and the frequency is 3.5Hz. The terminal electromagnetic stirring current is 700A, the frequency is 10Hz, and the total reduction is 25mm. Rolling process parameters: heating furnace heating stage 1000°C, heating stage 2 1160°C, equalizing stage 1180°C, entering finishing mill temperature 890°C, entering warping machine temperature 920°C, spinning temperature 850°C; roller speed 0.5m / s; total heating time of the heating furnace 131min, air cooling parameters are: the first 17 fans are running at full load, each fan has a rated air volume of 200,000 m3 / h, and an air pressure of 3000Pa. The temperature entering the insulation corridor is 450-550°C, and the insulation time is 190 minutes. Under this process, the sorbite content of the rolled wire rod reaches 85%, such as Figure 2 shown.

[0055] The tensile strength of the ultra-high strength wire rod XYL82B produced in Example 2 is 1234MPa, the network carbide is evenly distributed, the network carbon level is ≤1.0, and no martensite appears. The 21.6mm specification 1860Mpa grade steel wire made by the wire rod has an actual strength of 1910MPa for the finished single wire.

[0056]

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A 16mm prestressed steel strand wire rod XYL82B, characterized in that: The chemical composition of the wire rod and its weight percentage are: C: 0.80-0.85%, Si: 0.40-0.60%, Mn: 0.70-0.80%, Cr: 0.20-0.25%, P≤0.015%, S≤0.010%, Ni≤0.10%, Cu≤0.10%, Al≤0.02%, O≤0.002%, N≤0.005%, Sn≤0.0100%, As≤0.0100%, and the rest are Fe and unavoidable impurities.

2. A 16mm prestressed steel strand wire rod XYL82B according to claim 1, characterized in that: The wire rod strength reaches above 1200 MPa.

3. A 16mm prestressed steel strand wire rod XYL82B according to claim 1, characterized in that: The wire rod meets the technical requirements for producing high-strength prestressed steel strands with a specification of Φ21.6 mm and a strength level of 1860 MPa.

4. A method for producing a 16 mm prestressed steel strand wire rod XYL82B according to any one of claims 1 to 3, characterized in that: The following steps are involved: Converter smelting: special molten iron is used, the converter adopts double slag method, and the steel tapping uses slide plate to block slag; LF refining: LF refining uses aluminum particles for diffusion deoxidation, the white slag time is kept above 20 minutes, and the slag system adopts a ternary slag system; Continuous casting: adopts full-process protection pouring, constant casting speed production, low superheat pouring, using crystallizer, end electromagnetic stirring, light and heavy pressure reduction technology, and combined with the strong cooling process of water cooling + gas mist cooling in the secondary cooling zone; Rolling: The rolling adopts walking beam heating furnace, and the finishing rolling adopts "8+4" mode, that is, 8-stand finishing rolling unit and 4-stand sizing unit rolling. The wire rod size is measured in real time by online diameter gauge, and the wire rod is cooled by Stelmor air cooling line and kept warm in insulation corridor.

5. The method for producing the 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: The casting speed of the continuous casting furnace is 1.55-1.6 m / min, and the superheat is stabilized at 20-30°C.

6. The method for producing the 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: In the continuous casting process, square billets with a cross-section of 180*180mm2 are used for production. The electromagnetic stirring current of the crystallizer is 400A, the frequency is 3.5HZ, the terminal electromagnetic stirring current is 700A, the frequency is 10Hz, the total reduction is 25mm, and the water volume of the continuous casting secondary cooling water is 0.45L / Kg.

7. The method for producing the 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: The continuous cast steel billet is slowly cooled for 24 hours and then hot rolled.

8. The method for producing the 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: The main process parameters of the rolling are: heating furnace heating stage 1000℃, heating stage 2 1150-1160℃, soaking stage 1180℃, finishing mill 890℃, warping mill 920℃, spinning 840℃-860℃; roller speed 0.5m / s; total heating time in the heating furnace 120-150min.

9. The method for producing the 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: The air cooling parameters of the Stelmore air cooling line are: 17 fans, each with a rated air volume of 200,000 m3 / h and an air pressure of 3000Pa.

10. The method for producing a 16mm prestressed steel strand wire rod XYL82B according to claim 4, characterized in that: The process parameters of the insulation corridor are: the temperature entering the insulation corridor is 450-550°C, and the insulation time is more than 180 minutes.

Citation Information

Cited By

  • Steel wire rod for 2000MPa-grade prestressed steel with large specification of 15mm and preparation method of steel wire rod

    CN122013054A