Wire rod for low-nitrogen prestressed steel wire, manufacturing method of wire rod and manufacturing method of steel wire
By strictly controlling the chemical composition and smelting process of low-nitrogen prestressed steel wire rods, combined with surface treatment and controlled cooling drawing, the problem that existing wire rods cannot meet the performance requirements of high-quality steel wires has been solved, and the manufacture of high-strength and high-plasticity low-nitrogen prestressed steel wires has been achieved.
Patent Information
- Application Number
- CN202410963822.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
AI Technical Summary
The existing 12.5mm wire rods cannot meet the requirements for chemical composition, impurities and gas content of high-quality steel wire, resulting in insufficient performance of the steel wire in high-quality construction projects.
By controlling the content of elements such as carbon, silicon, manganese, phosphorus, and sulfur, and by adopting specific smelting and processing procedures, such as KR stirred pre-desulfurization, top and bottom blowing converter steelmaking, LF refining, RH furnace refining, continuous casting and high-speed wire rolling, the gas content and impurities are strictly controlled to ensure the purity of molten steel. Combined with surface treatment and controlled cooling drawing processes, low-nitrogen prestressed steel wire rods are prepared.
The prepared 12.5mm wire rod and 7.0mm prestressed steel wire have excellent strength, plasticity and resistance to hydrogen embrittlement, meeting the mechanical property requirements of high-quality steel wire. They have high tensile strength, excellent reduction of area and torsional properties.
Smart Images

Figure BDA0004951140490000081 
Figure BDA0004951140490000082 
Figure BDA0004951140490000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of steel wire production, and in particular relates to a wire rod for low-nitrogen prestressed steel wire and a manufacturing method thereof and a steel wire manufacturing method. Background Art
[0002] With the development of infrastructure construction, various large-scale bridges, high-pressure water supply projects and other construction projects have entered high-quality construction. The track plates of high-speed railways, bridge cables, high-pressure water supply pipelines and other structures have higher and higher requirements for the quality indicators of steel wires used. The existing 12.5mm wire rods for manufacturing steel wires do not meet the requirements of construction projects in terms of chemical composition, impurity and gas content, and internal organizational state. This requires a high-quality wire rod with the same diameter to produce high-quality steel wire. Summary of the invention
[0003] In view of this, the present invention aims to provide a wire rod for low-nitrogen prestressed steel wire, a method for manufacturing the wire rod, and a method for manufacturing the steel wire.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A wire rod for low-nitrogen prestressed steel wire, wherein the weight percentages of the wire rod components are: C: 0.79%-0.83%, Si: 0.20%-0.30%, Mn: 0.70%-0.85%, P: ≤0.015%, S: ≤0.015%, Cr: 0.20%-0.30%, Ni: ≤0.10%, Cu: ≤0.20%, O≤0.003%, H≤0.0003%, N≤0.003%, and the rest are Fe and unavoidable impurities.
[0006] Carbon (C): Carbon is the key element that determines the strength and plasticity of wire rod. In low-carbon steel wire rod, the carbon content is low, commonly known as soft wire, mainly used for drawing blanks or building materials. As the carbon content increases, the wire rod gradually changes to medium and high carbon steel wire rod, commonly known as hard wire. High carbon steel wire rod is mainly used to make high-strength steel wire, such as: prestressed concrete steel wire, bridge cable wire and other high-performance steel wire products.
[0007] Silicon (Si) and manganese (Mn): These two elements contribute to the strength and plasticity of the wire rod. They are usually added to steel in a certain proportion to improve the mechanical properties of the steel.
[0008] Phosphorus (P) and sulfur (S): Phosphorus and sulfur are generally regarded as harmful elements in steel because they increase the brittleness of steel. Therefore, in high-quality wire rods, the content of phosphorus and sulfur is strictly controlled.
[0009] Other trace elements: such as chromium (Cr) and other alloying elements can further improve the crystal structure of the wire rod, making the mechanical properties of the wire rod more uniform, and improving toughness and plasticity. At the same time, it can improve the corrosion resistance of the product, but the content of alloying elements must be strictly and scientifically controlled. The content of alloying elements has a significant impact on the organization and performance of the wire rod.
[0010] Gas content: The content of gases such as hydrogen (H), nitrogen (N), and oxygen (O) will harm the quality of the wire rod and affect the comprehensive mechanical properties of the steel. Excessive gas content will reduce the plasticity and toughness of the wire rod and increase its brittleness, so it needs to be strictly controlled.
[0011] Further, the following steps are included:
[0012] S1, molten iron pretreatment process:
[0013] Limestone and fluorite desulfurizers are added to the molten iron tank, and the S content in the molten iron is ≤0.018% through KR stirring pre-desulfurization, and the composition stability temperature is not less than 1300℃. After the slag is cleaned, it is sent to the steelmaking process;
[0014] S2, converter steelmaking process:
[0015] The converter adopts a top-bottom combined blowing converter, argon is blown at the bottom during the whole smelting process, top lance oxygen supply controls slag making, C content is controlled to be ≥0.45% when tapping, P content is controlled to be ≤0.015% when tapping, the order of alloy addition after tapping is: ferrosilicon, silicon-manganese alloy, steelmaking carburizer, tapping time is 5-7min, converter tapping temperature is 1585℃±10℃, argon gate outlet average is 1500℃±10℃, and then the ladle is transferred to the LF refining furnace process;
[0016] S3, LF refining process:
[0017] Control the ladle entry temperature ≥1490℃, slag basicity 1.8~2.3, soft blowing time ≥10min, LF makes reducing slag, argon blowing and stirring at the bottom of the ladle during the whole process, refining leaving the station temperature 1570℃, and total power-on time ≤45min;
[0018] S4, RH furnace refining process,
[0019] RH deep treatment: cycle ≤35min, vacuum ≤200pa, deep vacuum 12-15min, lifting gas setting 1300~1400Nl / min, temperature ≥1548℃ at the beginning of treatment, RH does not deoxidize or heat up, RH net cycle time 10min-12min; total time from the end of molten steel treatment to ladle pouring ≤30min, calming time 15-20min, achieving nitrogen content N≤0.0030%;
[0020] S5. Continuous casting process
[0021] The ingot is a square billet with a specification of 150mm×150mm. The actual temperature of the continuous casting station is below 1500℃, the superheat of molten steel is ≤30℃, and the casting is fully protected from the tundish to the crystallizer. The billet drawing speed is 1.9-2.1m / min, and the crystallizer and the end are electromagnetically stirred. The secondary cooling water volume is 1.2L / Kg. The tundish is purged with argon when the pouring and ladle changing furnace are started. The purging time is not less than 2min. Argon is passed through the ladle during the pouring process. The tundish adopts high liquid level casting, and the liquid level height is required to be ≥700mm. The ingot is slowly cooled in the slow cooling stack, and the slow cooling time is ≥72 hours.
[0022] S5, high-speed wire rolling process
[0023] The obtained continuous casting billet is sent to the steel rolling heating furnace. The heating furnace is divided into three sections. The temperature of the preheating section is 880±30℃, the heating section is 1120±30℃, and the soaking section is 1150±20℃. The furnace time is 2-3 hours. After the billet leaves the heating furnace, it is descaled under high pressure, and the water pressure is ≥17MPa; the billet enters the first rolling mill at an inlet temperature of 1020±10℃, and the finishing rolling inlet temperature is 920±20℃, and the wire laying temperature is 860±10℃. The rolling specification is φ12.5mm;
[0024] S6, Cooling Control Process
[0025] S7, Wire rod finishing process
[0026] Ensure that the head and tail of the wire rod are not penetrated by water and the defective parts should be cut off cleanly, and the cutting amount of the head and tail should be guaranteed to be ≥4 turns.
[0027] Furthermore, in S2, the strong argon ladle is pre-blown with argon for ≥2 min, the steel-out process is blown with argon for ≥3 min, and the argon station is blown with argon for ≥3 min to prevent the molten steel from being violently stirred and absorbing nitrogen.
[0028] Furthermore, in S3, the recarburizer adopts a low-nitrogen recarburizer, such as adjusting the carbon after the power-on is completed, and the soft argon blowing time after the carbon adjustment is completed is ≥5 minutes.
[0029] Further, step 1, wire rod surface treatment process:
[0030] After the wire rod is inspected and accepted for surface quality, mechanical properties, chemical composition, and metallographic structure, it is sent to the surface treatment process. The surface treatment process flow is: wire rod - pickling - water washing - high-pressure water washing - dip coating phosphating layer - water washing - boronization - drying - resting for 24 hours - drawing process;
[0031] Step 2, wire drawing process:
[0032] Temperature controlled drawing, online drawing temperature does not exceed 130 degrees.
[0033] Further, in step 1, the pickling is carried out by sulfuric acid pickling, with a concentration of 8%-18%, a temperature ≥50, ferrous sulfate ≤250g / L, and a pickling time of 8-20 minutes according to the oxidation state of the wire rod surface;
[0034] The wire rod is treated with phosphide coating at a total acidity of 45-70 points, free acidity of 3-10 points, nitric acid ≥ 21g / L, total zinc content ≥ 8g / L, free phosphoric acid ≥ 8g / L, ferrous content ≤ 10g / L, and a temperature of 70-85℃ to ensure that the wire rod coating thickness is ≥ 12g / m2;
[0035] Boron coating treatment on the surface: hydrolyze sodium tetraborate, and carry out boronization treatment at a Baume degree of 3-8 at a temperature of ≥80°C and a time of ≥3min, so that a uniform lubricating carrier is obtained on the surface of the wire rod;
[0036] The wire rods are left to air dry or in a drying oven for 24 hours.
[0037] Furthermore, in step 2, the surface-treated wire rod is sent to the drawing process, and 6 drawing passes are carried out on a computer-controlled steel wire special production line, making full use of the cooling system to achieve cold-controlled drawing of the steel wire during the entire plastic deformation process, ensuring that the temperature of the steel wire does not exceed 130°C during the drawing process, and using a calcium-sodium based mixed lubricant.
[0038] The invention has the advantages and positive effects that the wire rod manufactured by the method has a specification of 12.5 mm, a tensile strength range of 1160 MPa-1220 MPa, a cross-sectional shrinkage rate of ≥32%, and a post-fracture elongation rate of ≥10%. The 7.0 mm prestressed steel wire produced by the wire rod through surface treatment and controlled cold drawing has excellent strength, elastic and toughness comprehensive mechanical properties, a tensile strength range of 1600 MPa-1670 MPa, a torsion number of ≥10 times, a cross-sectional shrinkage rate of ≥30%, and a hydrogen embrittlement resistance performance of ≥100 hours. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundancy, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.
[0040] The invention comprises a wire rod for low-nitrogen prestressed steel wire, wherein the weight percentages of the components of the wire rod are: C: 0.79%-0.83%, Si: 0.20%-0.30%, Mn: 0.70%-0.85%, P: ≤0.015%, S: ≤0.015%, Cr: 0.20%-0.30%, Ni: ≤0.10%, Cu: ≤0.20%, O≤0.003%, H≤0.0003%, N≤0.003%, and the rest are Fe and unavoidable impurities.
[0041] The manufacturing method of the wire rod comprises the following steps:
[0042] S1, molten iron pretreatment process:
[0043] Limestone and fluorite desulfurizers are added to the molten iron tank, and the S content in the molten iron is ≤0.018% through KR stirring pre-desulfurization, and the composition stability temperature is not less than 1300℃. After the slag is cleaned, it is sent to the steelmaking process;
[0044] S2, converter steelmaking process:
[0045] The converter adopts a 140-ton converter with top and bottom double blowing. All the scrap steel in the converter is refined material, and the rest is molten iron. Argon is blown at the bottom throughout the smelting process to improve the stirring force of the molten pool. The top gun supplies oxygen to control slag formation. The C content is controlled at ≥0.45% during steel tapping, and the P content is controlled at ≤0.015% during steel tapping. The smelting process focuses on nitrogen control. All spot blowing secondary treatments must be preceded by hood lowering treatment. The air permeability and cleanliness of the ladle must be checked before steel tapping. The strong argon ladle is pre-blown for ≥2 minutes, and the argon is blown for ≥3 minutes during steel tapping. Argon is blown at the station for ≥3min to prevent the molten steel from violently turning and absorbing nitrogen; the order of adding alloys after steelmaking is: ferrosilicon → silicon-manganese alloy → steelmaking carburizer, no deoxidizer is added, carburizer is used for carburization, deoxidation and alloying, the alloy recovery rate is required to be calculated, the composition is controlled as required, and the amount of alloy used for refining and fine-tuning is reduced. The steelmaking time is 5-7min, the converter steelmaking temperature is 1585℃±10℃, and the average argon gate outlet is 1500℃±10℃, and then the ladle is transferred to the LF refining furnace process;
[0046] S3, LF refining process:
[0047] Control the ladle entry temperature ≥1490℃, slag basicity 1.8~2.3, soft blowing time ≥10min, LF makes reducing slag, LF refining ensures white slag making effect, argon blowing and stirring at the bottom of the ladle during the whole process, and adjust the molten steel composition and temperature to the target requirements. The temperature drop value during RH refining should be considered, the refining leaving station temperature is 1570℃, no heating or cooling operations should be performed in the RH refining station, the refining process should be operated with a slight positive pressure to avoid repeated heating, the total power-on time ≤45min, and the recarburizer should use a low-nitrogen recarburizer. If the carbon is adjusted after the power-on, the soft argon blowing time after the carbon adjustment is ≥5min, and the ladle covering agent should use carbonized rice husks. After adjusting the composition, the chemical composition of the molten steel is uniform and stable, ensuring that the reduction of inclusions and gas content in the steel meets the standards, the LF furnace composition meets the target value requirements, and RH furnace refining is carried out;
[0048] S4, RH furnace refining process,
[0049] RH deep treatment: cycle ≤35min, vacuum ≤200pa, deep vacuum 12-15min, lifting gas setting 1300~1400Nl / min, temperature ≥1548℃ at the beginning of treatment, the principle requirement for starting the machine to change the ladle is ≥1563℃, the principle requirement for continuous casting is ≥1548℃, the temperature of the vacuum tank refractory material is >1100℃, ensure that there is no residual steel in the vacuum tank, and deal with the residual steel and residue at the suction nozzle. The RH treatment process is affected by factors such as equipment and steam pressure. The process temperature is lower than the continuous casting station temperature, and the treatment is stopped. RH does not deoxidize or heat up. After adjusting the alloy, the RH net cycle time is 10min-12min; sampling is carried out after 3min of circulation to ensure that the sample is full and to fine-tune the composition; the total time from the end of molten steel treatment to the start of ladle casting is ≤30min, and the calming time is 15-20min, achieving a nitrogen content N≤0.0030%, which is far higher than the international standard of 0.0070%, and improving the internal purity of steel.
[0050] S5. Continuous casting process
[0051] The billet is a square billet with a specification of 150mm×150mm. The actual temperature of the continuous casting station is below 1500℃, the superheat of the molten steel is ≤30℃, and the casting is protected from the tundish to the crystallizer. The casting speed is 1.9~2.1m / min, and the casting speed is constant. The casting speed is 1.9~2.1m / min. The crystallizer and the end are electromagnetically stirred. The secondary cooling water volume is 1.2L / Kg. The sealing of the external casing is ensured during the continuous casting process. The tundish is purged with argon when pouring and changing the ladle furnace. The purging time is not less than 2min. Argon is passed through the ladle during the pouring process. Confirm electromagnetic stirring before pouring. In normal production, the casing is not allowed to float above the liquid surface for casting. If the protective casing is severely eroded or the length is insufficient, it must be replaced in time. It is forbidden to lift the ladle to check the slag at the end. The sealing of the casing is strictly tested. If there is air inhalation, find out the cause and deal with it in time. The tundish adopts high liquid level casting, and the liquid level height is required to be ≥700mm. Carbonized rice husks are required to be added evenly to ensure that the molten steel is not exposed to the liquid surface. In the middle and late stages of the casting, the furnace is required to measure the slag thickness of the tundish. If the slag thickness is ≥80mm, slag removal is required. Aluminum carbon nozzles must be used for casting to ensure that the nozzle is aligned with the crystallizer and the nozzle insertion depth is 80-120mm. The liquid level fluctuation of the cleaner should be ≤±3mm. The temperature gun should be calibrated once every 4 hours, and the temperature of the calibrated gun should be recorded. The temperature gun of the continuous casting tundish should be kept away from the tundish after the temperature measurement is completed. It is forbidden to be in a heated state for a long time. The ingot is slowly cooled in the slow cooling stack, and the slow cooling time is ≥72 hours.
[0052] S5, high-speed wire rolling process
[0053] The obtained continuous casting billet is sent to the steel rolling heating furnace. The heating furnace is divided into three sections, with the preheating section temperature of 880±30℃, the heating section temperature of 1120±30℃, and the soaking section temperature of 1150±20℃. The furnace time is 2-3 hours. After the billet leaves the heating furnace, high-pressure descaling is carried out, and the water pressure is ≥17MPa; it is required to ensure the descaling effect, that is, after descaling, there should be no visible residual primary iron oxide scale on the surface of the billet. The billet enters the first rolling mill at an inlet temperature of 1020±10℃, the finishing rolling inlet temperature is 920±20℃, and the wire laying temperature is 860±10℃. The rolling specification is φ12.5mm.
[0054] S6, Cooling Control Process
[0055] After the wire rod passes through the spinning machine, it is evenly spread on the Stelmor roller for air cooling. There are 11 fans in the production line. Fans No. 1 to 5 are turned on at 100% power, No. 6 is turned on at 80% power, No. 7-10 is turned on at 100% power, and No. 11 is turned on at 50% power in April and September; 100% power is turned on in May-August, and closed in March and October. In actual production, the fans should be appropriately increased or decreased according to the actual performance indicators of the wire rod, and the air volume should be adjusted to control the cooling speed and stabilize the organization and performance of the wire rod. The speed of the first section of the roller is 0.70-0.80m / s, and the speed increase of the remaining sections is set at 2-5%. Along the direction of the wire rod travel, 1-12 insulation covers are opened in April and September, and 13-16 are closed. All insulation covers are opened from May to August, and 1-10 insulation covers are opened in March and October, and 11-16 are closed.
[0056] S7, Wire rod finishing process
[0057] Ensure that the head and tail of the wire rod are not penetrated by water and the defective parts should be cut off cleanly. The cutting amount of the head and tail should be guaranteed to be ≥4 circles. Scratches and other defects are not allowed on the surface of the wire rod.
[0058] We used the above method to obtain 4 furnace products, namely Examples 1-4, and used the conventional method (without RH furnace refining process) to obtain Comparative Examples 1-6. Their chemical compositions and mechanical properties are as follows
[0059] Table 1 Chemical composition of 12.5 mm wire rods of the embodiments and comparative examples
[0060]
[0061]
[0062] Table 2 Mechanical properties of 12.5 mm wire rods of the embodiments and comparative examples
[0063] The specification of the wire rod manufactured in this application is 12.5mm, the tensile strength is as high as 1160MPa-1220MPa, the cross-sectional shrinkage rate is ≥32%, and the elongation after fracture is ≥10%. The metallographic structure of the wire rod should be mainly sorbite structure, the sorbite content should be ≥90%, the harmful structures such as central martensite and network cementite should not be greater than level 1.5, and the depth of the total decarburization layer (ferrite + transition layer) on one side of the wire rod should not be greater than 1.0D% (D is the nominal diameter of the wire rod). The non-metallic inclusions of the wire rod are controlled to be no higher than level 1.5 for A, C, B, D, and Ds, and the austenite grain size is 7 to 9). Various mechanical indicators are significantly better than similar products.
[0064] The manufacturing method of the steel wire using the above-mentioned wire rod mainly comprises the following steps:
[0065] Step 1, wire rod surface treatment process:
[0066] After the wire rod is inspected and accepted for surface quality, mechanical properties, chemical composition, and metallographic structure, it is sent to the surface treatment process. The surface treatment process flow is: wire rod - pickling - water washing - high-pressure water washing - dip coating phosphating layer - water washing - boronization - drying - resting for 24 hours - drawing process;
[0067] The pickling adopts sulfuric acid pickling with a concentration of 8%-18%, a temperature ≥50, and ferrous sulfate ≤250g / L. The pickling time is 8-20 minutes according to the oxidation state of the wire rod surface. The pickling solution inhibitor is used. On the one hand, it purifies the working environment, and more importantly, effectively controls the intrusion of hydrogen atoms into the material.
[0068] The phosphating mother liquor is made of zinc nitrate Zn(NO3)2, phosphoric acid H3PO4, zinc oxide ZnO and water. The parameters are density ≥1.35g / L, zinc content ≥100g / L, FA (free acid) ≥240g / L, TA (total acid) ≥700 points. The normal working wire rod is treated with phosphating coating under the conditions of total acidity 45-70 points, free acidity 3-10 points, nitric acid ≥21g / L, total zinc content ≥8g / L, free phosphoric acid ≥8g / L, ferrous content ≤10g / L, and temperature 70-85℃ to ensure that the wire rod coating thickness is ≥12g / m2. Moreover, the phosphating film is uniform and dense and firmly combined with the matrix, with very strong plastic surface finish and ductility. The surface phosphating film of the finished product has good homogeneity and strong grip. It not only plays a role in surface passivation and rust prevention for steel wire, but also effectively overcomes the tendency of hydrogen embrittlement sensitivity.
[0069] The surface is treated with boron coating. Sodium tetraborate is hydrolyzed to a Baume degree of 3-8. Boron treatment is carried out at a temperature of ≥80°C and a time of ≥3min to obtain a uniform lubricating carrier on the surface of the wire rod.
[0070] The wire rod is kept stationary for 24 hours for air drying or baking treatment to further diffuse the internal gas of the wire rod and promote aging, thus ensuring that the wire rod used in the wire drawing process has good toughness indicators.
[0071] Step 2, wire drawing process:
[0072] Temperature controlled drawing, online drawing temperature does not exceed 130 degrees;
[0073] The wire rod after surface treatment is sent to the drawing process, and 6 drawing passes are carried out on the computer-controlled steel wire special production line. The complete and reliable reel water cooling, air cooling and wire drawing die cooling system are fully utilized to realize the cold-controlled drawing of the steel wire during the plastic deformation process, ensuring that the temperature of the steel wire does not exceed 130℃ during the drawing process. At the same time, the calcium-sodium mixed lubricant is used to ensure not only the smooth drawing of the steel wire during the production process, but also the surface quality of the steel wire after it is ejected from the die. The production line is equipped with a self-developed rotary die drawing device, which not only improves the surface quality of the steel wire, but also strictly controls the ovality of the steel wire surface. In order to strengthen the internal quality control of the steel wire in the drawing process, our production line is equipped with an online automatic temperature collection control system for each drawing pass, and the temperature of each coil of steel wire is measured and recorded in time during the production process. As long as the temperature exceeds the internal control requirements, the machine will be stopped immediately and the machine will continue to be produced after proper treatment. In order to timely discover hidden dangers such as wire rod and drawing friction damage, we are equipped with an online eddy current flaw detection alarm system to fully guarantee the internal and external quality of the company.
[0074] (3) Steel wire product test results
[0075] The tensile strength of the products is between 1600MPa and 1670MPa, the yield strength ratio is ≥80%, and the dispersion of the tensile strength is within 70MPa. The torsion performance is good, the steel wire (at L0 = 210mm) is twisted for no less than 10 turns at 7.0mm, the torsion fracture is flat, and there are no defects on the surface of the steel wire. The samples taken from the production batch are tested for hydrogen embrittlement sensitivity of the steel wire, and the results meet the time index requirements of the relevant standards and projects for hydrogen embrittlement sensitivity test, and meet the qualified indicators. Before and after the wire rod drawing and denaturation, the gas content in the steel is basically unchanged.
[0076] The 7.0 mm prestressed steel wire produced by the method has excellent strength, elasticity and toughness comprehensive mechanical properties, the tensile strength of the steel wire ranges from 1600 MPa to 1670 MPa, the number of torsion times is ≥10 times, the cross-sectional shrinkage rate is ≥30%, and the hydrogen embrittlement resistance is ≥100 hours.
[0077] The embodiments of the present invention are described in detail above, but the contents described are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A low-nitrogen prestressed steel wire wire rod, characterized in that: The weight percentages of the wire rod components are: C: 0.79%-0.83%, Si: 0.20%-0.30%, Mn: 0.70%-0.85%, P: ≤0.015%, S: ≤0.015%, Cr: 0.20%-0.30%, Ni: ≤0.10%, Cu: ≤0.20%, O≤0.003%, H≤0.0003%, N≤0.003%, and the rest are Fe and unavoidable impurities.
2. The method for manufacturing the wire rod according to claim 1, characterized in that: Including the following processes: S1, molten iron pretreatment process: Limestone and fluorite desulfurizers are added to the molten iron tank, and the S content in the molten iron is ≤0.018% through KR stirring pre-desulfurization, and the composition stability temperature is not less than 1300℃. After the slag is cleaned, it is sent to the steelmaking process; S2, converter steelmaking process: The converter adopts a top-bottom combined blowing converter, argon is blown at the bottom during the whole smelting process, top lance oxygen supply controls slag making, C content is controlled to be ≥0.45% and P content is controlled to be ≤0.015% during steel tapping, the order of alloy addition after steel tapping is: ferrosilicon, silicon-manganese alloy, steelmaking carburizer, steel tapping time is 5-7min, converter tapping temperature is 1585℃±10℃, argon gate outlet averages 1500℃±10℃, and then the ladle is transferred to the LF refining furnace process; S3, LF refining process: Control the ladle entry temperature ≥1490℃, slag basicity 1.8~2.3, soft blowing time ≥10min, LF makes reducing slag, argon blowing and stirring at the bottom of the ladle during the whole process, refining leaving the station temperature 1570℃, and total power-on time ≤45min; S4, RH furnace refining process, RH deep treatment: cycle ≤35min, vacuum ≤200pa, deep vacuum 12-15min, lifting gas setting 1300~1400Nl / min, temperature ≥1548℃ at the beginning of treatment, RH does not deoxidize or heat up, RH net cycle time 10min-12min; total time from the end of molten steel treatment to ladle pouring ≤30min, calming time 15-20min, achieving nitrogen content N≤0.0030%; S5. Continuous casting process The ingot is a square billet with a specification of 150mm×150mm. The actual temperature of the continuous casting station is below 1500℃, the superheat of molten steel is ≤30℃, and the casting is fully protected from the tundish to the crystallizer. The billet drawing speed is 1.9-2.1m / min, and the crystallizer and the end are electromagnetically stirred. The secondary cooling water volume is 1.2L / Kg. The tundish is purged with argon when the pouring and ladle changing furnace are started. The purging time is not less than 2min. Argon is passed through the ladle during the pouring process. The tundish adopts high liquid level casting, and the liquid level height is required to be ≥700mm. The ingot is slowly cooled in the slow cooling stack, and the slow cooling time is ≥72 hours. S5, high-speed wire rolling process The obtained continuous casting billet is sent to the steel rolling heating furnace. The heating furnace is divided into three sections. The temperature of the preheating section is 880±30℃, the heating section is 1120±30℃, and the soaking section is 1150±20℃. The furnace time is 2-3 hours. After the billet leaves the heating furnace, high-pressure descaling is carried out, and the water pressure is ≥17MPa; the billet enters the first rolling mill with an inlet temperature of 1020±10℃, and the inlet temperature of the finishing rolling is 920±20℃, the wire laying temperature is 860±10℃, and the rolling specification is φ12.5mm; S6, Cooling Control Process S7, Wire rod finishing process Ensure that the head and tail of the wire rod are not penetrated by water and the defective parts should be cut off cleanly, and the cutting amount of the head and tail should be guaranteed to be ≥4 turns.
3. The method for manufacturing wire rod according to claim 2, characterized in that: In S2, the strong argon ladle is pre-blown with argon for ≥2 minutes, the steel-out process is blown with argon for ≥3 minutes, and the argon station is blown with argon for ≥3 minutes to prevent the molten steel from being violently stirred and absorbing nitrogen.
4. The method for manufacturing a wire rod according to claim 2, characterized in that: In S3, the recarburizer adopts a low-nitrogen recarburizer. If the carbon is adjusted after the power is turned on, the soft argon blowing time shall be ≥5min after the carbon adjustment.
5. A method for manufacturing steel wire using the wire rod according to claim 2, characterized in that: Step 1, wire rod surface treatment process: After the wire rod is inspected and accepted for surface quality, mechanical properties, chemical composition, and metallographic structure, it is sent to the surface treatment process. The surface treatment process flow is: wire rod - pickling - water washing - high-pressure water washing - dip coating phosphating layer - water washing - boronization - drying - resting for 24 hours - drawing process; Step 2, wire drawing process: Temperature controlled drawing, online drawing temperature does not exceed 130 degrees.
6. The method for manufacturing a steel wire according to claim 5, characterized in that: In step 1, pickling is carried out by sulfuric acid pickling, with a concentration of 8%-18%, a temperature ≥50, ferrous sulfate ≤250g / L, and a pickling time of 8-20 minutes according to the oxidation state of the wire rod surface; The wire rod is treated with phosphide coating at a total acidity of 45-70 points, free acidity of 3-10 points, nitric acid ≥ 21g / L, total zinc content ≥ 8g / L, free phosphoric acid ≥ 8g / L, ferrous content ≤ 10g / L, and a temperature of 70-85℃ to ensure that the wire rod coating thickness is ≥ 12g / m2; Boron coating treatment on the surface: hydrolyze sodium tetraborate, and carry out boronization treatment at a Baume degree of 3-8 at a temperature of ≥80°C and a time of ≥3min, so that a uniform lubricating carrier is obtained on the surface of the wire rod; The wire rods are left to air dry or in a drying oven for 24 hours.
7. The method for manufacturing a steel wire according to claim 5, characterized in that: In step 2, the surface treated wire rod is sent to the drawing process and drawn six times on a computer-controlled steel wire production line. The cooling system is fully utilized to achieve cold-controlled drawing of the steel wire during the entire plastic deformation process, ensuring that the temperature of the steel wire does not exceed 130°C during the drawing process. At the same time, a calcium-sodium based mixed lubricant is used.
Citation Information
Cited By
2230 Mpa steel strand for prestressed concrete and preparation method of 2230 Mpa steel strand
CN121555904A
A 2230mpa steel strand for prestressed concrete and a method for manufacturing the same
CN121555904B