Low-density low-temperature steel and preparation method thereof
By controlling the Al content and heat treatment parameters, low-density and low-temperature steel is formed, which solves the problems of high density and low yield strength of traditional low-temperature steel, and achieves the improvement of low-temperature performance and production efficiency, meeting the needs of lightweight materials in the fields of aerospace and other fields.
Patent Information
- Application Number
- CN202411023613.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional low-temperature steel has high density and low yield strength, which is difficult to meet the demand for lightweight materials in the fields of aerospace, deep-sea exploration, etc., and has high production costs and high manufacturing difficulties.
By controlling the Al content, the density of low-temperature steel is reduced, and the heating temperature, insulation time and cooling rate are accurately adjusted during the heat treatment process, forming a uniform FeMnAlC steel with a matrix phase of austenite, improving the low-temperature performance.
The density reduction and low-temperature performance improvement of low-density steel is achieved, meeting the needs of lightweight materials, reducing production costs and improving production efficiency.
Smart Images

Figure CN118880184A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of low-temperature steel preparation, and in particular to low-density low-temperature steel and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the development of industry, low-temperature steel is increasingly used in aerospace, deep-sea exploration, cryogenic storage and other fields. Traditional low-temperature steel contains more alloying elements, usually including Fe, Al, Ni, Cr, Mn, C, etc., which makes its composition complex. This not only increases the difficulty of manufacturing, but also increases the production cost. Due to the large number of alloying elements and complex composition of low-temperature steel, its manufacturing quality is easily affected by process operations. For example, melting temperature, type and amount of refining agent, heat treatment process, etc. will have a significant impact on its performance. This requires strict control of each process link in the manufacturing process, which in turn increases the difficulty of production.
[0003] In addition, in the fields of aerospace, deep sea exploration, etc., in order to ensure mechanical properties, the density of low-temperature steel is usually large. Taking the commonly used nickel-based low-temperature steel as an example, its density is 8.2g / cm 3 However, although this density can meet certain mechanical performance requirements, it increases the weight and cannot meet the demand for lightweight materials in aerospace, deep-sea exploration and other fields.
[0004] Therefore, it is necessary to provide a low-density low-temperature steel with simple composition, low density and good low-temperature performance. Summary of the invention
[0005] In order to solve the problems of high density and low yield strength of conventional low-temperature steel in the prior art, the present invention provides a low-density low-temperature steel and a preparation method thereof.
[0006] In the present invention, Al is the main element for achieving density reduction. For every 1% of Al added, the density of the low-temperature steel is reduced by 1.3%, thereby reducing the density of the low-temperature steel by controlling the amount of Al added. In addition, precise control of the Al content can also improve the low-temperature performance of the low-temperature steel, so that it still has excellent toughness and brittle fracture resistance at low temperatures of -10°C to -196°C. The present invention can not only meet the demand for lightweight materials in specific fields, but also reduce production costs and improve production efficiency.
[0007] To achieve the above objectives, the specific technical solutions of the present invention are as follows.
[0008] The first aspect of the present invention provides a low-density low-temperature steel, wherein the low-density low-temperature steel is prepared from the following raw materials in terms of mass percentage:
[0009] Mn 20% to 30%, C 0.5% to 1.5%, Al 5% to 12%, and the balance is Fe, totaling 100%.
[0010] The present invention can refine the grains, improve the strength and hardness, and effectively improve the low-temperature performance of the low-density low-temperature steel by precisely controlling the Al content in the low-density low-temperature steel. If the Al content is too high, it will lead to a decrease in welding performance and work hardening ability, so it is necessary to accurately control the Al content. The low-density low-temperature steel in the present invention has excellent toughness and brittle fracture resistance at low temperatures of -10°C to -196°C.
[0011] In another preferred embodiment, the density of the low-density low-temperature steel is 6.5 g / cm 3 ~7.02g / cm 3 .
[0012] In another preferred embodiment, the yield strength of the low-density low-temperature steel at -150°C is 1135.2 MPa to 1173.9 MPa.
[0013] In another preferred embodiment, the low-density low-temperature steel is obtained by performing a primary heat treatment at 1100°C to 1200°C and a secondary heat treatment at 900°C to 1000°C.
[0014] During the heat treatment process, when the heat treatment temperature is too high, the grains in the steel will grow rapidly, resulting in a decrease in the mechanical properties of the steel, especially the plasticity and toughness will be significantly reduced. At the same time, the microstructure of the material will become uneven, thus affecting its overall performance. Excessive temperature may also lead to unfavorable structural transformation in the steel, such as high-temperature ferrite transformation. Therefore, during the preparation process, the heat treatment temperature needs to be controlled.
[0015] The second aspect of the present invention provides a method for preparing low-density low-temperature steel, wherein the low-density low-temperature steel is the low-density low-temperature steel provided by the first aspect of the present invention, comprising the following steps:
[0016] The raw materials are mixed to obtain mixed powder, and the mixed powder is ball-milled under a protective atmosphere to obtain a nanocomposite powder slurry;
[0017] The nanocomposite powder slurry is melted to make the elements evenly mixed, and the melted nanocomposite powder slurry is poured to obtain a steel ingot;
[0018] After the steel ingot is hot rolled, it is subjected to a primary heat treatment at 1100°C to 1200°C, and then subjected to a secondary heat treatment at 900°C to 1000°C to obtain low-density low-temperature steel.
[0019] In another preferred embodiment, the specific process of the heat treatment is as follows:
[0020] The hot rolled steel ingot is first heated to 1100°C ~ 1200°C, kept warm for 1 ~ 2 hours, cooled to room temperature at a rate of 7°C / min, then heated to 900°C ~ 1000°C, kept warm for 1 ~ 2 hours, and then water-cooled to room temperature.
[0021] Too long a holding time will also cause grain growth, which will lead to a decrease in the mechanical properties of the steel, especially plasticity and toughness. Steel with too short a holding time may show large fluctuations and instability in mechanical properties due to uneven structure and defects. Too fast a cooling rate will cause large structural stresses in the steel during the cooling process, which may cause deformation or cracking of the steel during subsequent use. Too fast a cooling rate may also promote the formation of brittle phases, such as ordered phases such as B2 and DO3. These brittle phases will significantly reduce the plasticity and toughness of the steel.
[0022] Therefore, the present invention optimizes the microstructure of FeMnAlC steel by controlling the heating temperature, holding time and cooling rate, so that the obtained low-density low-temperature steel has austenite as the matrix phase and a uniform structure, which can effectively eliminate segregation, thereby maintaining good low-temperature toughness and other mechanical properties of the low-density low-temperature steel. In addition, ferrite will also precipitate, thereby further improving the strength of the matrix and the improvement of low-temperature performance.
[0023] In another preferred embodiment, before the mixed powder is ball-milled, the mixed powder is further mixed with ethanol; the mass percentage of the ethanol is 70% to 80%;
[0024] The mass ratio of the ethanol to the mixed powder is 1-1.5:8.5-9. In the subsequent preparation process, all the ethanol is evaporated.
[0025] In another preferred embodiment, the ball milling time is 9 h to 10 h.
[0026] In another preferred embodiment, the smelting temperature is 1600° C. to 1700° C., and the smelting time is 2 h to 3 h.
[0027] In another preferred embodiment, the specific process of hot rolling is:
[0028] Heat the steel ingot to 1150℃~1250℃, keep it warm for 2h~3h; hot roll it at 960℃~1120℃, and then water cool it to room temperature.
[0029] In another preferred embodiment, the protective atmosphere is argon.
[0030] In another preferred embodiment, the ball milling medium is stearic acid.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) The present invention can effectively reduce the density of low-temperature steel by precisely controlling the Al content, compared with the traditional low-temperature steel of 8.2g / cm 3 The density of the low temperature steel in the present invention can be reduced to 6.5g / cm 3 This is mainly because Al is the main element for achieving density reduction. For every 1% of Al added, the density of the low-temperature steel decreases by 1.3%, so the density of the low-temperature steel can be reduced by controlling the amount of Al added. In addition, precise control of the Al content can also improve the low-temperature performance of the low-temperature steel, so that it still has excellent toughness and brittle fracture resistance at low temperatures of -10°C to -196°C. The low-density low-temperature steel in the present invention has broader application prospects in aerospace, deep-sea exploration, low-temperature storage and other fields, especially in fields that require lightweight materials, such as automobile manufacturing, shipbuilding, etc.
[0033] (2) The present invention not only ensures that the low-temperature steel can still maintain good toughness and other mechanical properties under low-temperature environment by controlling the heat treatment process parameters, but also optimizes the microstructure of FeMnAlC steel, so that the obtained low-density low-temperature steel has austenite as the matrix phase and a uniform structure, which can effectively eliminate segregation, thereby maintaining good low-temperature toughness and other mechanical properties of the low-density low-temperature steel. At the same time, the preparation method is simple and easy, with high production efficiency, which is conducive to reducing production costs. Due to the reduction in the types and contents of alloy elements, the procurement cost of raw materials is also controlled, further improving economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a low-temperature tensile test diagram of the low-temperature, low-density, low-temperature steel in Examples 1 to 3 of the present invention at -150°C.
[0035] Figure 2 These are microscopic morphology images of the low-temperature, low-density, low-temperature steels at -150°C in Examples 1 to 3 of the present invention; wherein A is the microscopic morphology image of the low-temperature, low-density, low-temperature steel at -150°C in Example 1, B is the microscopic morphology image of the low-temperature, low-density, low-temperature steel at -150°C in Example 2, and C is the microscopic morphology image of the low-temperature, low-density, low-temperature steel at -150°C in Example 3.
[0036] Figure 3 This is a low-temperature impact test diagram of the low-temperature, low-density, low-temperature steel in Examples 1 to 3 of the present invention at -196°C.
[0037] Figure 4It is a microscopic morphology of the low-temperature, low-density, low-temperature steel in Examples 1 to 3 of the present invention at a low-temperature impact fracture at -196°C; wherein A is a microscopic morphology of the low-temperature, low-density, low-temperature steel in Example 1 at a low-temperature impact fracture at -196°C, B is a microscopic morphology of the low-temperature, low-density, low-temperature steel in Example 2 at a low-temperature impact fracture at -196°C, and C is a microscopic morphology of the low-temperature, low-density, low-temperature steel in Example 3 at a low-temperature impact fracture at -196°C. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0039] Unless otherwise specified, the experimental methods described in the following examples are all conventional methods; the reagents and materials described are all commercially available unless otherwise specified.
[0040] Traditional cryogenic steels usually have a high density, which is not conducive to reducing equipment weight and energy consumption. This shortcoming is particularly prominent in fields that require lightweight materials, such as aerospace and deep-sea exploration. Due to the above reasons, traditional cryogenic steels have problems such as high density and low yield strength, making it difficult to meet the use requirements in specific environments.
[0041] In order to reduce the types of alloying elements in low-temperature steel, the prior art uses Fe, Mn, Al and C to prepare low-density low-temperature steel, wherein the Al content reaches 21% to 25%, that is, the density is reduced by increasing the Al content, and a heat treatment process is performed at 1100 to 1200°C to obtain low-density low-temperature steel. Although the density of the low-temperature steel prepared by this method is lower than that of traditional low-temperature steel, its yield strength at room temperature is about 700MPa, and it cannot guarantee a good yield strength in a low-temperature environment of -10 to -196°C.
[0042] The present invention can refine the grains, improve the strength and hardness while reducing the density by precisely controlling the Al content in the low-density low-temperature steel, thereby effectively improving the low-temperature performance of the low-density low-temperature steel. If the Al content is too high, the welding performance and work hardening ability will be reduced, so the Al content needs to be precisely controlled. The low-density low-temperature steel in the present invention has excellent toughness and brittle fracture resistance in a low temperature environment of -10 to -196°C. During the heat treatment process, when the heat treatment temperature is too high, the grains in the steel will grow rapidly, resulting in a decrease in the mechanical properties of the steel, especially the plasticity and toughness will be significantly reduced. At the same time, the microstructure of the material is also made uneven, thereby affecting its overall performance. Excessive temperature may also cause adverse structural transformations in the steel, such as high-temperature ferrite transformation. Too long a holding time will also cause grain growth, resulting in a decrease in the mechanical properties of the steel, especially plasticity and toughness. Steel with too short a holding time may show large fluctuations and instability in mechanical properties due to uneven structure and defects. Too fast a cooling rate will cause greater structural stress in the steel during the cooling process, which may cause deformation or cracking of the steel during subsequent use. Too fast a cooling rate may also promote the formation of brittle phases, such as ordered phases such as B2 and DO3. These brittle phases will significantly reduce the plasticity and toughness of the steel.
[0043] Therefore, the present invention optimizes the microstructure of FeMnAlC steel by controlling the heating temperature, holding time and cooling rate, so that the obtained low-density low-temperature steel has austenite as the matrix phase and a uniform structure, which can effectively eliminate segregation, thereby maintaining good low-temperature toughness and other mechanical properties of the low-density low-temperature steel. In addition, ferrite will also precipitate, thereby further improving the strength of the matrix and the improvement of low-temperature performance.
[0044] A low-density, low-temperature steel and a preparation method thereof are described in detail below.
[0045] The iron powder in the following examples has a particle size of 50 μm and a purity of 99.9%; the aluminum powder has a particle size of 30 μm and a purity of 99.9%; the manganese powder has a particle size of 150 μm and a purity of 99.9%; the carbon powder has a particle size of 20 μm and a purity of 99.5%; and the nano-cerium powder has a particle size of 30 nm and a purity of 99.5%.
[0046] Example 1
[0047] A low-density low-temperature steel, wherein the low-density low-temperature steel is prepared from the following raw materials in terms of mass percentage:
[0048] Mn 24.68wt%, Al 6.43wt%, C 0.83wt%, and the balance is Fe, totaling 100%.
[0049] The method for preparing the low-density low-temperature steel comprises the following steps:
[0050] S1. Mix the raw materials to obtain nanocomposite powder, mix the nanocomposite powder with 70% ethanol at a mass ratio of 1:8.5, use stearic acid as a ball milling medium, and perform ball milling for 10 hours to obtain a nanocomposite powder slurry; before ball milling, the ball milling tank must be evacuated and argon gas must be introduced as a protective atmosphere;
[0051] S2, placing the nanocomposite powder slurry in a melting furnace, and melting it at a high temperature of 1700°C for 3 hours to ensure that all elements are fully mixed;
[0052] S3, melting the smelted nanocomposite powder slurry in a high-frequency vacuum induction furnace with an argon protective atmosphere and casting it into an iron mold to obtain a steel ingot;
[0053] S4, heating the steel ingot to 1250°C, keeping it at this temperature for 3 hours, hot rolling it at 1120°C, and then water cooling it to room temperature;
[0054] S5. The hot-rolled steel is heated to 1200°C, kept at this temperature for 2 hours, then oil-cooled to room temperature, then heated to 1000°C, kept at this temperature for 2 hours, and then water-cooled to room temperature to obtain low-density low-temperature steel.
[0055] Example 2
[0056] A low-density low-temperature steel, the raw materials are reduced iron powder, aluminum powder, manganese powder, carbon powder and nano-cerium powder, and the mass percentage of the elements in each raw material is:
[0057] Mn 24.44wt%, Al 8.44wt%, C 0.85wt%, and the balance is Fe, totaling 100%.
[0058] The method for preparing the low-density low-temperature steel comprises the following steps:
[0059] S1. Mix the raw materials according to the mass percentage of the elements to obtain nanocomposite powder. After mixing the nanocomposite powder with ethanol, use stearic acid as a ball milling medium and perform ball milling for 10 hours to obtain a nanocomposite powder slurry; before ball milling, the ball milling tank must be evacuated and argon gas must be introduced as a protective atmosphere;
[0060] S2, placing the nanocomposite powder slurry in a melting furnace, and melting it at a high temperature of 1700°C for 2 hours to ensure that all elements are fully mixed;
[0061] S3, melting the smelted nanocomposite powder slurry in a high-frequency vacuum induction furnace with an argon protective atmosphere and casting it into an iron mold to obtain a steel ingot;
[0062] S4, heating the steel ingot to 1250°C, keeping it at this temperature for 2 hours, hot rolling it at 1020°C, and then water cooling it to room temperature;
[0063] S5. The hot-rolled steel is heated to 1200°C, kept at this temperature for 1 hour, then oil-cooled to room temperature, then heated to 1000°C, kept at this temperature for 2 hours, and then water-cooled to room temperature to obtain low-density low-temperature steel.
[0064] Example 3
[0065] A low-density low-temperature steel, the raw materials are reduced iron powder, aluminum powder, manganese powder, carbon powder and nano-cerium powder, and the mass percentage of the elements in each raw material is:
[0066] Mn 24.5wt%, Al 10.28wt%, C 0.86wt%, and the balance is Fe, totaling 100%.
[0067] The method for preparing the low-density low-temperature steel comprises the following steps:
[0068] S1. Mix the raw materials according to the mass percentage of the elements to obtain nanocomposite powder. After mixing the nanocomposite powder with ethanol, use stearic acid as a ball milling medium and perform ball milling for 10 hours to obtain a nanocomposite powder slurry; before ball milling, the ball milling tank must be evacuated and argon gas must be introduced as a protective atmosphere;
[0069] S2, placing the nanocomposite powder slurry in a melting furnace, and melting it at a high temperature of 1600°C for 2 hours to ensure that all elements are fully mixed;
[0070] S3, melting the smelted nanocomposite powder slurry in a high-frequency vacuum induction furnace with an argon protective atmosphere and casting it into an iron mold to obtain a steel ingot;
[0071] S4, heating the steel ingot to 1150°C, keeping it at that temperature for 2h, hot rolling it at 960°C, and then water cooling it to room temperature;
[0072] S5. The hot-rolled steel is heated to 1100°C, kept at this temperature for 1 hour, then oil-cooled to room temperature, then heated to 900°C, kept at this temperature for 1 hour, and then water-cooled to room temperature to obtain low-density low-temperature steel.
[0073] The low temperature and low density steels in the above-mentioned Examples 1 to 3 were subjected to mechanical property tests and microstructure observations.
[0074] 1. Low temperature and low density The density of low temperature steel
[0075] The density of the low-density and low-temperature steels in Examples 1 to 3 was measured, and the results are shown in Table 1.
[0076] Table 1 Density of low-density low-temperature steel in Examples 1 to 3
[0077] Group <![CDATA[Density (g / cm 3 )]]> Example 1 <![CDATA[7.02g / cm 3 ]]> Example 2 <![CDATA[6.76g / cm 3 ]]> Example 3 <![CDATA[6.5g / cm 3 ]]>
[0078] From the results in Table 1, it can be seen that the density of the low-temperature and low-density low-temperature steel in the present invention is 8.2 g / cm compared with the traditional nickel-based low-temperature steel. 3 The density of the steel is reduced by 16.8% to 20.7%. It can be seen that the present invention can effectively reduce the density of warm steel by precisely controlling the amount of Al added, and is beneficial to reducing the weight of equipment and reducing energy consumption, and can meet the requirements of lightweight materials for aerospace, deep-sea exploration, etc.
[0079] 2. Performance of low temperature and low density low temperature steel
[0080] 1) The low temperature and low density low temperature steels in Examples 1 to 3 were subjected to low temperature tensile tests at -150°C. The results are as follows: Figure 1 shown.
[0081] from Figure 1 It can be seen that the yield strength of the low-density low-temperature steel in Example 1 is 1173.9 MPa, and the elongation is 48.9%. The yield strength of the low-density low-temperature steel in Example 2 is 1135.2 MPa, and the elongation is 52.4%. The yield strength of the low-density low-temperature steel in Example 2 is 1335.5 MPa, and the elongation is 27.4%. The strength and plasticity are both good, indicating that when the metal material is subjected to external force, it can absorb more energy before breaking and can maintain good strength and ductility at the same time.
[0082] It can be seen that the low-temperature, low-density, low-temperature steel in the present invention not only has a lower density, but also has good strength and ductility at low temperatures. This is mainly due to controlling the content of Al in the low-density low-temperature steel, which can refine the grains, improve strength and hardness, and effectively improve the low-temperature performance of the low-density low-temperature steel. If the Al content is too high, it will lead to a decrease in welding performance and work hardening ability, so it is necessary to accurately control the Al content. In addition, during the preparation process, the microstructure of the FeMnAlC steel is optimized by controlling the heating temperature, the holding time and the cooling rate, so that the obtained low-density low-temperature steel has austenite as the matrix phase and a uniform structure, which can effectively eliminate segregation, thereby enabling the low-density low-temperature steel to maintain good low-temperature toughness and other mechanical properties.
[0083] Figure 2 The microscopic morphology of the low-temperature tensile fracture of the low-density low-temperature steel in Examples 1 to 3 of the present invention is shown in FIG. Figure 2 It can be seen that the fracture surfaces of the low-density and low-temperature steels of Examples 1 and 2 show large and deep dimples, which are ductile fractures, while Example 3 shows cleavage fractures.
[0084] Figure 3 This is a low-temperature impact test diagram of the low-density low-temperature steel in Examples 1 to 3 of the present invention. Figure 3It can be seen that the low-density low-temperature steel in Example 1 has the best impact toughness. This is because the nanoscale subcrystalline structure produced by the interaction of twins and dislocations in austenitic steel can make it have excellent toughness at low temperatures.
[0085] Figure 4 The microscopic morphology of the low-temperature impact fracture of the low-density low-temperature steel in Examples 1 to 3 of the present invention is shown in FIG. Figure 4 It can be seen that the fracture surface of the low-density low-temperature steel in Example 1 is covered by large dimples near the tip of the V-notch and in the center of the fracture surface, and these large dimples show a rugged morphology, which means relatively large plastic deformation and ductile fracture. Examples 2 and 3 show cleavage fracture.
[0086] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalent technologies, the present invention is also intended to include these changes and variations. The above-described embodiments are only preferred embodiments for fully illustrating the present invention, and their protection scope is not limited thereto. Equivalent substitutions or changes made by those skilled in the art on the basis of the present invention are all within the protection scope of the present invention, and the protection scope of the present invention shall be subject to the claims.
Claims
1. A low-density low-temperature steel, characterized in that: The low-density low-temperature steel is prepared from the following raw materials in terms of mass percentage: Mn 20% to 30%, C 0.5% to 1.5%, Al 5% to 12%, and the balance is Fe, totaling 100%.
2. The low-density low-temperature steel according to claim 1, characterized in that: The density of the low-density low-temperature steel is 6.5 g / cm 3 ~7.02g / cm 3 .
3. The low-density low-temperature steel according to claim 1, characterized in that: The yield strength of the low-density low-temperature steel at -150°C is 1135.2MPa to 1173.9MPa.
4. The low-density low-temperature steel according to claim 1, characterized in that: The low-density low-temperature steel is obtained by performing a primary heat treatment at 1100°C to 1200°C and then performing a secondary heat treatment at 900°C to 1000°C.
5. A method for preparing low-density low-temperature steel according to any one of claims 1 to 4, characterized in that: The following steps are involved: The raw materials are mixed to obtain mixed powder, which is ball-milled, smelted, hot-rolled, and then subjected to a primary heat treatment at 1100°C to 1200°C and a secondary heat treatment at 900°C to 1000°C to obtain low-density low-temperature steel.
6. The preparation method according to claim 5, characterized in that: The specific process of the heat treatment is as follows: The hot rolled steel ingot is first heated to 1100°C ~ 1200°C, kept warm for 1h ~ 2h, cooled to room temperature at a rate of 7°C / min ~ 9°C / min, then heated to 900°C ~ 1000°C, kept warm for 1h ~ 2h, and then water-cooled to room temperature.
7. The preparation method according to claim 5, characterized in that: Before the mixed powder is ball-milled, the mixed powder is mixed with ethanol; The mass percentage of the ethanol is 70% to 80%; The mass ratio of the ethanol to the mixed powder is 1-1.5:8.5-9.
8. The preparation method according to claim 5, characterized in that: The ball milling time is 9h to 10h.
9. The preparation method according to claim 5, characterized in that: The smelting temperature is 1600° C. to 1700° C., and the smelting time is 2 h to 3 h.
10. The preparation method according to claim 5, characterized in that: The specific process of hot rolling is: Heat the steel ingot to 1150℃~1250℃, keep it warm for 2h~3h; hot roll it at 960℃~1120℃, and then water cool it to room temperature.
Citation Information
Cited By
Ultrahigh-strength and ultrahigh-plasticity heterogeneous low-density steel, preparation method and processing equipment thereof
CN119876736A
Ultrahigh-manganese austenite wear-resistant steel as well as preparation method and application thereof