Stainless steel material resistant to high-temperature molten chlorine salt corrosion

By adding Nb and Mo to AFA steel to form Laves phase and Al oxide layer, the problems of instability of nitrate molten salt and the corrosion properties of the material to molten chloride salt are solved, and the corrosion resistance and cost-effectiveness of stainless steel materials are significantly improved. Next generation solar photothermal power generation technology.

CN118880185APending Publication Date: 2024-11-01SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411264404.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The nitrate molten salt used in existing CSP systems is unstable at high temperatures, resulting in NOx pollution and corrosion problems, which cannot meet the needs of next-generation solar thermal power generation for heat transfer/heat storage media, and common materials have strong corrosion to molten chloride salt. limits its application.

Method used

Nb and Mo are added to AFA steel to form Laves phase Fe2 (Nb, Mo) and Al and O to form an oxide layer, thereby improving the material's corrosion resistance against high-temperature molten chloride.

Benefits of technology

It significantly improves the corrosion resistance of stainless steel materials, reduces costs, and significantly reduces the corrosion depth and rate under the same conditions, achieving long-term corrosion resistance at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880185A_ABST
    Figure CN118880185A_ABST
Patent Text Reader

Abstract

The invention discloses a stainless steel material resistant to high-temperature molten chlorine salt corrosion, which is characterized in that Nb and Mo are added into AFA steel, Laves phase Fe2 (Nb, Mo) is formed by gathering Nb and Mo, and an oxide layer is formed by Al and O, so that the stainless steel material is well protected, the high-temperature molten chlorine salt corrosion resistance is obtained, and the application of the AFA steel as a structural material in a next-generation solar photo-thermal power station is promoted. The stainless steel material has the advantages of being good in corrosion resistance, low in cost, mature in technology and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal protection, and more specifically, relates to a stainless steel material resistant to high-temperature molten chloride salt corrosion. Background Art

[0002] Solar thermal power generation (CSP) technology is one of the most promising power generation technologies in future renewable energy systems. In existing CSP power plants, molten nitrate is often used as a heat transfer / heat storage medium. However, when the temperature of molten nitrate exceeds 565°C, the nitrate will decompose and emit NOx pollutants, which cannot meet the demand for heat transfer and storage media in the next generation of solar thermal power generation. It is known that the key to improving the efficiency of any thermal cycle is to increase the operating temperature of the system. In the TES / HTF (heat transfer / heat storage) system of the next generation CSP, a higher service temperature (600-800°C) can effectively increase the conversion efficiency, but molten nitrate is unstable at this temperature, so it is necessary to find a new molten salt with higher stability to replace molten nitrate. In view of the advantages of chloride molten salt such as good heat transfer and storage performance, low price, and rich content, molten chloride salt is considered to be one of the candidate salts in the next generation CSP. However, molten chloride salt has been proven to be highly corrosive to most common structural materials, limiting its application in CSP. At present, the methods for mitigating corrosion mainly include thermal purification, chemical purification and electrochemical purification, improvement and treatment of structural materials, etc. In terms of structural material composition design, others have studied the addition of Nb-Mo and other alloying elements to Hastelloy alloys with a high Ni content. Based on the known chloride corrosion resistance of Ni, only Mo was found to be resistant to chloride corrosion.

[0003] Nickel-based alloys show relatively better corrosion resistance than stainless steel, but the price of nickel-based alloys also increases with the increase of nickel content. AFA steel is an Al-containing austenitic steel, mainly containing Fe-Cr-Ni-Al. The composite effect of a certain amount of Ni and other trace alloying elements jointly improves its chloride corrosion resistance. It can have the same or even better resistance to molten chloride corrosion as Ni-based alloys while reducing costs, and realize large-scale industrial application. At the same time, the third component effect of Al and Cr will lead to the diffusion of Al and the formation of oxides with O to prevent the deepening of corrosion. In addition, the formed Fe2(Nb,Mo)Laves phase can further inhibit corrosion. Summary of the invention

[0004] An object of the present invention is to solve at least the above problems and / or disadvantages and to provide at least the advantages which will be described hereinafter.

[0005] In order to achieve these purposes and other advantages according to the present invention, a stainless steel material resistant to high temperature molten chloride corrosion is provided, comprising: adding Nb and Mo to AFA steel, forming Laves phase Fe2 (Nb, Mo) by aggregation of Nb and Mo, and forming an oxide layer with Al and O to obtain high temperature molten chloride corrosion resistance.

[0006] Preferably, the elements of the stainless steel material include Fe, Cr, Ni, Al, Mo, Nb and C.

[0007] Preferably, the percentage of Fe is 52-59wt.%, the percentage of Cr is 14-16wt.%, the percentage of Ni is 18-27wt.%, the percentage of Al is 2-3wt.%, the percentage of Mo is 2-4wt.%, the percentage of Nb is 1-2wt.%, and the percentage of C is 0.08wt.%.

[0008] A method for preparing a stainless steel material resistant to high temperature molten chloride corrosion comprises the following steps:

[0009] First, clean the crucible and weigh the raw materials in proportion: Fe, Cr, Ni, Mo, Al, Nb and C. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1450-1600℃ and the cavity pressure is less than 10 -4 Pa; first fully melt the raw materials into liquid to ensure uniform composition, then wait for 3 minutes for the sample to cool and solidify into a solid, flip the ingot and continue smelting; repeat this 3-4 times to form an ingot with relatively uniform composition; then pass through the heating furnace, first heat to 800℃, heating rate 100℃ / h, keep warm for 1-2h. Then heat to 1200℃ at a heating rate of 100℃ / h, keep warm for 1 hour and start forging. The steel ingot is forged at 1200℃ at a forging ratio of 3:1, and then air-cooled to obtain stainless steel material.

[0010] Preferably, the stainless steel material corrosion performance testing method comprises:

[0011] In a glove box, a stainless steel material sample is placed in a quartz tube, and mixed chloride salt is added into the quartz tube through a long-necked funnel so that the mixed chloride salt completely covers the stainless steel material sample; the quartz tube is sealed in a vacuum containing the stainless steel material sample and the mixed chloride salt, and the sealing is tested with ethanol; the quartz tube is placed in a muffle furnace for an immersion experiment, and after the stainless steel material sample is naturally cooled in the furnace, the stainless steel material sample is taken out of the quartz tube, and then cleaned with deionized water and alcohol to remove residual salt, and finally dried in air to obtain a stainless steel material sample corroded by high-temperature molten chloride salt.

[0012] Preferably, the mixed chloride salt is a mixture of NaCl, MgCl2 and KCl, wherein the amount of NaCl accounts for 30.2%, the amount of MgCl2 accounts for 47.1%, and the amount of KCl accounts for 22.7%.

[0013] Preferably, the ratio of the weight of the mixed chloride salt to the surface area of ​​the stainless steel material is 4×10 4 g / m -2 ~6×10 4 g / m -2 .

[0014] Preferably, the vacuum degree of the quartz tube sealed in the vacuum containing the stainless steel material sample and the mixed chloride salt is greater than 0.1 Pa.

[0015] Preferably, the static immersion temperature of the quartz tube in the muffle furnace is 600° C. to 700° C.; and the immersion time of the quartz tube in the muffle furnace is 200 h to 800 h.

[0016] The invention discloses an application of a stainless steel material resistant to corrosion by high-temperature molten chloride salts. The stainless steel material is applied to the structural material of chloride molten salt in solar thermal power generation technology.

[0017] The present invention includes at least the following beneficial effects: The present invention provides a stainless steel material resistant to high-temperature molten chloride corrosion. Under high-temperature corrosion, the outward diffusion of Fe and the aggregation of Al and oxygen in the corrosion layer lead to the generation of vacancies, which promote the aggregation of Nb and Mo to produce the second phase - Laves phase Fe2 (Nb, Mo). The AFA steel of the present invention has the advantages of good corrosion resistance, low cost, and mature technology. Compared with conventional stainless steel, the Laves phase formed in the AFA steel caused by the addition of Nb-Mo can effectively improve the corrosion resistance to molten chloride. Under the same corrosion conditions, the corrosion depth of traditional stainless steel after 100 hours of corrosion is as high as more than 100 microns, and the Ni-based alloy also reaches 40-50μm. The corrosion depth of the stainless steel material of the present invention is less than 40μm after 200 hours of corrosion, and the corrosion depth can be as low as 16.1μm after 200 hours of corrosion. In addition, the corrosion rate is also greatly reduced, and the corrosion depth of 25Ni-AFA steel after 800 hours of corrosion does not exceed 100 microns.

[0018] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a cross-sectional morphology diagram of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 200 hours;

[0020] Figure 2 This is a cross-sectional morphology of the stainless steel sample in Example 1 after being corroded in a molten mixed chloride salt for 400 hours;

[0021] Figure 3 This is a cross-sectional morphology diagram of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 600 hours;

[0022] Figure 4 This is a cross-sectional morphology diagram of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 800 hours;

[0023] Figure 5 This is an EDS line scan image of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 200 hours;

[0024] Figure 6 This is an EDS line scan image of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 400 hours;

[0025] Figure 7 This is an EDS line scan image of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 600 hours;

[0026] Figure 8 This is an EDS line scan image of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 800 hours;

[0027] Fig. 9 This is a microscopic morphology of the stainless steel sample in Example 1 after being corroded in a molten mixed chloride salt for 200 hours;

[0028] Fig.10 This is a microscopic morphology of the stainless steel sample in Example 1 after being corroded in a molten mixed chloride salt for 400 hours;

[0029] Fig.11 This is a microscopic morphology of the stainless steel sample in Example 1 after being corroded in a molten mixed chloride salt for 600 hours;

[0030] Fig.12 This is a microscopic morphology of the stainless steel sample in Example 1 after being corroded in a molten mixed chloride salt for 800 hours;

[0031] Fig.13 This is a cross-sectional morphology diagram of the stainless steel material sample in Example 2 after being corroded in a molten mixed chloride salt for 200 hours;

[0032] Fig.14 This is a cross-sectional morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 400 hours;

[0033] Fig.15This is a cross-sectional morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 600 hours;

[0034] Fig.16 This is a cross-sectional morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 800 hours;

[0035] Fig.17 This is an EDS line scan image of the stainless steel material sample in Example 2 after being corroded in a molten mixed chloride salt for 200 hours;

[0036] Fig.18 This is an EDS line scan image of the stainless steel material sample in Example 1 after being corroded in a molten mixed chloride salt for 400 hours;

[0037] Fig.19 This is an EDS line scan of the stainless steel material sample in Example 2 after being corroded in a molten mixed chloride salt for 600 hours;

[0038] Fig. 20 This is an EDS line scan of the stainless steel material sample in Example 2 after being corroded in a molten mixed chloride salt for 800 hours;

[0039] Fig.21 This is a microscopic morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 200 hours;

[0040] Fig. 22 This is a microscopic morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 400 hours;

[0041] Fig.23 This is a microscopic morphology of the stainless steel sample in Example 2 after being corroded in a molten mixed chloride salt for 600 hours;

[0042] Fig.24 This is a microscopic morphology of the stainless steel material sample in Example 2 after being corroded in molten mixed chloride salt for 800 hours. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0044] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0045] Example 1

[0046] This embodiment provides a stainless steel material resistant to high temperature molten chloride corrosion, the stainless steel material comprising: 58.36% Fe, 14.21% Cr, 19.25% Ni, 2.66% Al, 3.62% Mo, 1.8% Nb, 0.08% C;

[0047] The preparation method of the stainless steel material of this embodiment includes:

[0048] First, clean the crucible and prepare the metal raw materials Fe, Cr, Ni, Mo, Al, Nb and C according to different weight ratios. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1500°C and the cavity pressure is less than 10 -4 Pa. First, fully melt the material into liquid to ensure uniform composition, then wait for 3 minutes for the sample to cool and solidify into a solid, flip the ingot, and continue smelting. Repeat this 4 times to form an ingot with relatively uniform composition. Then pass through the heating furnace, first heat to 800℃, heating rate 100℃ / h, and keep warm for 2h. Then heat to 1200℃ at a heating rate of 100℃ / h, keep warm for 1 hour and start forging. The steel ingot is forged at 1200℃ at a forging ratio of 3:1, and then air-cooled to obtain stainless steel material.

[0049] Example 2

[0050] This embodiment provides a stainless steel material resistant to high temperature molten chloride corrosion, the stainless steel material comprising: 51.02% Fe, 14.11% Cr, 26.67% Ni, 2.76% Al, 3.55% Mo, 1.81% Nb, 0.08% C;

[0051] The preparation method of the stainless steel material of this embodiment includes:

[0052] First, clean the crucible and prepare the metal raw materials Fe, Cr, Ni, Mo, Al, Nb and C according to different weight ratios. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1500°C and the cavity pressure is less than 10 -4 Pa. First, fully melt the material into liquid to ensure uniform composition, then wait for 3 minutes for the sample to cool and solidify into a solid, flip the ingot, and continue smelting. Repeat this 4 times to form an ingot with relatively uniform composition. Then pass through the heating furnace, first heat to 800℃, heating rate 100℃ / h, and keep warm for 2h. Then heat to 1200℃ at a heating rate of 100℃ / h, keep warm for 1 hour and start forging. The steel ingot is forged at 1200℃ at a forging ratio of 3:1, and then air-cooled to obtain stainless steel material.

[0053] Example 3

[0054] In order to improve the corrosion resistance of stainless steel to high-temperature molten chloride salts, Si is added to the stainless steel, and a NiCrMoTi layer is laser clad on the surface of the stainless steel. The specific embodiment process is as follows:

[0055] Compared with Example 1, in this embodiment, Si is added to the stainless steel material, and a NiCrMoTi layer is laser clad on the surface of the stainless steel material, wherein the proportion of each element in the stainless steel material is adjusted to: 56.86% Fe, 14.21% Cr, 19.25% Ni, 2.66% Al, 3.62% Mo, 1.8% Nb, 0.08% C, and the percentage of Si is 1.50wt.%; the preparation method of the stainless steel material in this embodiment is:

[0056] First, clean the crucible and prepare the metal raw materials Fe, Cr, Ni, Mo, Al, Nb, C and Si according to different weight ratios. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1500°C and the cavity pressure is less than 10 -4 Pa. First, fully melt the material into liquid to ensure uniform composition, then wait for 3 minutes for the sample to cool and solidify into a solid, flip the ingot, and continue smelting. Repeat this 4 times to form an ingot with relatively uniform composition. Then pass through the heating furnace, first heat to 800°C, heating rate 100°C / h, and keep warm for 2h. Then heat to 1200°C at a heating rate of 100°C / h, keep warm for 1 hour and start forging. The steel ingot is forged at 1200°C at a forging ratio of 3:1, and then air-cooled to obtain stainless steel material

[0057] The specific method of laser cladding a NiCrMoTi layer on the surface of a stainless steel material includes: mixing Ni powder, Cr powder, Mo powder and Ti powder in a mass ratio of 2:1:0.5:0.2 to obtain a mixed powder;

[0058] The surface of the stainless steel material is preheated to 600°C, and a continuous fiber laser with a laser wavelength of 1080nm is used for laser cladding. The mixed powder is fed in a coaxial powder feeding manner, and the continuous fiber laser is used for laser irradiation on the surface of the preheated stainless steel material to obtain a NiCrMoTi layer by cladding on the surface of the stainless steel material. The laser cladding process parameters are: laser output power P=1200W, laser scanning speed of 10mm / s, spot diameter of 2mm, powder feeding amount of 10g / min, and high-purity argon is used as protective gas to protect the molten pool during the laser cladding process, and the argon flow rate is 15L / min.

[0059] Example 4

[0060] In order to improve the corrosion resistance of stainless steel to high-temperature molten chloride salts, Si is added to the stainless steel, and a NiCrMoTi layer is laser clad on the surface of the stainless steel. The specific embodiment process is as follows:

[0061] Compared with Example 2, the present embodiment is different in that Si is added to the stainless steel material in the present embodiment, and a NiCrMoTi layer is laser clad on the surface of the stainless steel material, wherein the proportion of each element in the stainless steel material is adjusted to: 48.02% Fe, 14.11% Cr, 26.67% Ni, 2.76% Al, 3.55% Mo, 1.81% Nb, 0.08% C, and the percentage of Si is 3.0wt.%; the preparation method of the stainless steel material in the present embodiment is:

[0062] First, clean the crucible and prepare the metal raw materials Fe, Cr, Ni, Mo, Al, Nb, C and Si according to different weight ratios. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1500°C and the cavity pressure is less than 10 -4 Pa. First, fully melt the material into liquid to ensure uniform composition, then wait for 3 minutes for the sample to cool and solidify into a solid, flip the ingot, and continue smelting. Repeat this 4 times to form an ingot with relatively uniform composition. Then pass through the heating furnace, first heat to 800℃, heating rate 100℃ / h, and keep warm for 2h. Then heat to 1200℃ at a heating rate of 100℃ / h, keep warm for 1 hour and start forging. The steel ingot is forged at 1200℃ at a forging ratio of 3:1, and then air-cooled to obtain stainless steel material.

[0063] The specific method of laser cladding a NiCrMoTi layer on the surface of a stainless steel material comprises: mixing Ni powder, Cr powder, Mo powder and Ti powder in a mass ratio of 5:2:1:0.2 to obtain a mixed powder;

[0064] The surface of the stainless steel material is preheated to 800°C, and a continuous fiber laser with a laser wavelength of 1080nm is used for laser cladding. The mixed powder is fed in a coaxial powder feeding manner, and the continuous fiber laser is used for laser irradiation on the surface of the preheated stainless steel material to obtain a NiCrMoTi layer by cladding on the surface of the stainless steel material. The laser cladding process parameters are as follows: laser output power of 1200W, laser scanning speed of 10mm / s, spot diameter of 5mm, powder feeding amount of 15g / min, and high-purity argon is used as protective gas to protect the molten pool during the laser cladding process, and the argon flow rate is 15L / min.

[0065] Comparative Example 1

[0066] The proportion and preparation method of the stainless steel material in this comparative example are the same as those in Example 2, except that a NiCrMoTi layer is laser clad on the surface of the stainless steel material in this comparative example, and the method of laser cladding the NiCrMoTi layer is the same as that in Example 4.

[0067] Comparative Example 2

[0068] The proportion and preparation method of the stainless steel material in this comparative example are the same as those in Example 4, except that the NiCrMoTi layer is not laser clad on the surface of the stainless steel in this comparative example.

[0069] The stainless steel materials resistant to high temperature molten chloride corrosion of Example 1, Example 2, Example 3, Example 4, Comparative Example 1 and Comparative Example 2 were respectively subjected to high temperature molten chloride corrosion resistance tests, and the test method included:

[0070] In the glove box, a sample was placed in a quartz tube. An equal amount of mixed chloride salt (5 g) was added to each quartz tube through a long-necked funnel to completely cover the entire sample. The mixed chloride salt was a mixture of NaCl, MgCl2, and KCl, in which the amount of NaCl accounted for 30.2%, the amount of MgCl2 accounted for 47.1%, and the amount of KCl accounted for 22.7%. The weight / sample surface area ratio of the mixed chloride salt was approximately 5×10 4 g / m -2 . The quartz tube was stored in a glove box as a backup. The quartz tube was sealed in a vacuum containing the sample and mixed chloride salt, with a vacuum degree greater than 0.1 Pa, and the sealing was tested with ethanol. The quartz tube was placed in a muffle furnace for immersion experiments. Considering that the operating temperature of the next-generation CSP plant is 600℃-800℃, the static immersion temperature is set to 700℃. The immersion times are 200h, 400h, 600h, and 800h, respectively. After the sample was naturally cooled in the furnace, the sample was removed from the quartz tube, and then washed with deionized water and alcohol for 15min to remove residual salt, and finally dried in air. Each sample was weighed five times with an analytical balance.

[0071] The cross-sectional morphology of the stainless steel sample of Example 1 after corrosion in the molten mixed chloride salt for 200h, 400h, 600h and 800h is as follows: Figure 1-Figure 4 As shown; Figure 1-Figure 4In the embodiment 1, the outermost layer of the stainless steel material sample is the FeNi layer, because the Cr in the stainless steel quickly dissolves into the chloride salt, leaving the Fe and Ni elements. Due to the outward diffusion of Cr, vacancies are left inside the matrix, which promotes the aggregation of Nb and Mo. The dark gray is the MgAl2O4 spinel layer, and the light gray is the Laves phase (Fe2(Nb,Mo)). The depth of the corrosion layer is mainly determined by the depth of Cr dissolution corrosion, and the corrosion tendency is along the grain boundary. As the corrosion time increases, the corrosion depth gradually increases. By measuring the corrosion depth of the sample cross-section SEM image and calculating the average value, the following conclusions are drawn: the stainless steel material sample in Example 1 is corroded at 700℃ high temperature for 200h, 400h, 600h, and 800h respectively, and its corresponding corrosion depth is 16.1μm, 26.5μm, 52.1μm, and 116.7μm.

[0072] Figure 5-Figure 8 They are EDS line scans of the stainless steel sample in Example 1 after being corroded in the molten mixed chloride salt for 200h, 400h, 600h and 800h respectively; Figure 5-Figure 8 It can be seen that the stainless steel material sample of Example 1 shows obvious Nb and Mo enrichment after corrosion for 200h, 400h and 600h, among which the enrichment at 600h is the most obvious. And by observing its EDS line scan, the intensity increase of Nb is the most obvious.

[0073] Figure 9-12 The microscopic morphology of the stainless steel sample in Example 1 after being corroded in the molten mixed chloride salt for 200h, 400h, 600h and 800h, respectively, combined with Figure 5-Figure 8 Analysis shows that obvious aggregation of Nb and Mo was observed in the stainless steel sample after 600h of corrosion, but this phenomenon disappeared after 800h, which led to a significant increase in the corrosion depth at 800h.

[0074] in, Figure 9-12 Finally, the element contents at each marked position are shown in the following table:

[0075]

[0076]

[0077] In the above table, (a):1, (a):2, and (a):3 are respectively Fig. 9 The marks 1, 2, and 3 in (b):1, (b):2, and (b):3 are Fig.10 The marks 1, 2, and 3 in (c):1, (c):2, and (c):3 are Fig.11 The marks 1, 2, 3, (d):1, (d):2 are Fig.12 Marks 1 and 2 in .

[0078] Figure 13-Figure 16 They are cross-sectional morphology diagrams of the stainless steel material sample in Example 2 corroded in 700°C molten mixed chloride salt (30.2% NaCl, 47.1% MgCl2, 22.7% KCl) for 200h, 400h, 600h, and 800h. The stainless steel material sample in Example 2 has a corresponding average corrosion depth of 33.1μm, 38.5μm, 54.2μm, and 71.8μm after being corroded for 200h, 400h, 600h, and 800h under the same corrosion conditions.

[0079] Figure 17-Figure 20 They are EDS line scans of the stainless steel sample in Example 2 after being corroded in the molten mixed chloride salt for 200h, 400h, 600h and 800h, respectively. Figure 17-Figure 20 It can be seen that the stainless steel sample in Example 2 showed obvious Nb and Mo enrichment after corrosion for 200h, 400h and 600h, among which the enrichment at 600h was the most obvious. And by observing its EDS line scan, the intensity increase of Nb was the most obvious.

[0080] Figure 21-24 They are the microscopic morphology of the stainless steel sample in Example 2 after being corroded in the molten mixed chloride salt for 200h, 400h, 600h and 800h, respectively. Figure 17-Figure 20 Analysis shows that obvious Nb and Mo aggregation was found at 800h, and the bright white phase is the second phase containing Nb and Mo - Laves phase. Therefore, its 800h corrosion depth is greatly reduced compared with AFA1 steel.

[0081] in, Figure 21-24 The element contents at each marked position are shown in the following table:

[0082]

[0083]

[0084] In the above table, (a):1, (a):2, and (a):3 are respectively Fig.21 The marks 1, 2, and 3 in (b):1 and (b):2 are Fig. 22 The marks 1 and 2 in (c):1 and (c):2 are Fig.23 The marks 1, 2, (d):1, (d):2 are Fig.24 Marks 1 and 2 in .

[0085] comprehensive Figure 5-Figure 8 and Figure 17-Figure 20This indicates that the aggregation of Mo alone is not enough to resist chloride corrosion. Only the co-aggregation of Nb and Mo to form the second phase - Laves phase can effectively slow down molten chloride corrosion.

[0086] The corrosion depths of the stainless steel materials prepared in Examples 1 to 4, Comparative Examples 1 and 2 in 700° C. molten mixed chloride salt (NaCl content is 30.2%, MgCl2 content is 47.1%, and KCl content is 22.7%) for 200 h, 400 h, 600 h, and 800 h were measured respectively, and the following table was obtained:

[0087] 200h corrosion depth 400h corrosion depth 600h corrosion depth 800h corrosion depth Example 1 16.1 microns 26.5 microns 52.1 microns 116.7 microns Example 2 33.1 microns 38.5 microns 54.2 microns 71.8 microns Example 3 10.2 microns 17.3 microns 40.4 microns 62.2 microns Example 4 22.5 microns 21.6 microns 42.7 microns 55.4 microns Comparative Example 1 30.6 microns 35.8 microns 49.1 microns 68.8 microns Comparative Example 2 31.5 microns 36.1 microns 52.4 microns 69.4 microns

[0088] It can be seen from the above table that the stainless steel materials prepared in Example 1 and Example 2 have excellent resistance to molten chloride corrosion, and the corrosion depths of the stainless steel materials in Example 1 and Example 2 are both below 40 microns after 400 hours; among them, the corrosion depth of the stainless steel material in Example 1 can be as low as 16.1 microns after 200 hours, and the corrosion depth of the stainless steel material in Example 2 is 71.8 microns after 800 hours, indicating that it has the ability to resist long-term molten chloride corrosion.

[0089] The corrosion depth of the stainless steel material in Example 3 at 200 h is as low as 10.2 μm, and the corrosion depths of Examples 3 and 4 at 200 h, 400 h, 600 h, and 800 h are significantly smaller than those of Examples 1-2 and Comparative Examples 1-2, indicating that after Si is added and a NiCrMoTi layer is laser clad on the surface of the stainless steel material, the stainless steel material's resistance to molten chloride salt corrosion is further improved.

[0090] At the same time, the corrosion depth of existing 304 stainless steel, In800h stainless steel, 310S stainless steel, 316L stainless steel, C276 stainless steel, C22 stainless steel, In625 stainless steel in 700℃ molten mixed chloride salt (NaCl accounts for 30.2%, MgCl2 accounts for 47.1% and KCl accounts for 22.7%) for 100h is shown in the following table:

[0091] Alloy Type Main components of alloy Corrosion depth (micrometer) 304 70Fe-18Cr-8Ni 230 In800h 39.5Fe-19Cr-30Ni 150 310S 53Fe-24Cr-19Ni 140 316L 68Fe-16Cr-10Ni-2Mo 130 C276 49Ni-17Mo-16.5Cr 110 C22 59Ni-20Cr-12.5Mo 50 In625 55Ni-23Cr-10Mo-4.15Nb 45

[0092] It can be seen from the above table that the corrosion depth of the above stainless steel materials exceeds 40 microns after 100 hours, indicating that the corrosion resistance of the above stainless steel materials to molten chloride salts is not as good as that of Examples 1 to 4.

[0093] The corrosion depth of existing Haynes 230 stainless steel in 700°C molten mixed chloride salt (NaCl accounts for 33%, MgCl2 accounts for 45.4% and KCl accounts for 21.6%) for 400 hours is shown in the following table:

[0094] Alloy Type Main components of alloy Corrosion depth (micrometer) Haynes230 61.06Ni-13.4W-21.6Cr-1.2Mo 100

[0095] The corrosion depth of Haynes 230 stainless steel in 700°C molten mixed chloride salt for 400 hours is much greater than that of Examples 1 to 4.

[0096] The corrosion depth of existing 625 stainless steel and 316SS stainless steel in 700℃ molten mixed chloride salt (NaCl accounts for 33%, MgCl2 accounts for 45.4% and KCl accounts for 21.6%) for 100h is shown in the following table:

[0097] Alloy Type Main components of alloy Corrosion depth (micrometer) 625 62Ni-21.5Cr-9Mo-3.6Nb-0.4Al 50 316SS 64.5Fe-17Cr-13Ni-2.6Mo 40

[0098] It can be seen from the above table that the corrosion depth of the above stainless steel materials has exceeded or reached 40 microns after 100 hours, indicating that the corrosion resistance of the above stainless steel materials to molten chloride salts is not as good as that of Examples 1 to 4.

[0099] The number of devices and processing scales described here are used to simplify the description of the present invention. Applications, modifications and variations of the present invention will be obvious to those skilled in the art.

[0100] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A stainless steel material resistant to high temperature molten chloride corrosion, characterized in that: include: Nb and Mo are added to AFA steel, and the Laves phase Fe2(Nb,Mo) is formed by the aggregation of Nb and Mo, and Al and O form an oxide layer, thereby obtaining resistance to high-temperature molten chloride salt corrosion.

2. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 1, characterized in that: The elements of the stainless steel material include: Fe, Cr, Ni, Al, Mo, Nb, and C.

3. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 2, characterized in that: The percentage of Fe is 52-59wt.%, the percentage of Cr is 14-16wt.%, the percentage of Ni is 18-27wt.%, the percentage of Al is 2-3wt.%, the percentage of Mo is 2-4wt.%, the percentage of Nb is 1-2wt.%, and the percentage of C is 0.08wt.%.

4. A method for preparing a stainless steel material resistant to high temperature molten chloride corrosion according to any one of claims 1 to 3, characterized in that: The following steps are involved: First, clean the crucible and weigh the raw materials in proportion: Fe, Cr, Ni, Mo, Al, Nb and C. Then, use a vacuum induction furnace to put the weighed raw materials into a water-cooled crucible in a non-consumable tungsten high vacuum arc furnace. The arc temperature is 1450-1600℃ and the cavity pressure is less than 10 -4 Pa; firstly, fully melt the raw materials into liquid to ensure uniform composition, then wait for 3 minutes to allow the sample to cool and solidify into a solid, flip the ingot and continue smelting; repeat this 3-4 times to form an ingot with uniform composition; then pass through a heating furnace, first heat to 800°C, heating rate 100°C / h, keep warm for 1-2h; then heat to 1200°C at a heating rate of 100°C / h, keep warm for 1 hour before starting forging; the steel ingot is forged at 1200°C at a forging ratio of 3:1, and then air-cooled to obtain a stainless steel material.

5. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 1, characterized in that: The stainless steel material corrosion performance testing method comprises: In a glove box, a stainless steel material sample is placed in a quartz tube, and mixed chloride salt is added into the quartz tube through a long-necked funnel so that the mixed chloride salt completely covers the stainless steel material sample; the quartz tube is sealed in a vacuum containing the stainless steel material sample and the mixed chloride salt; the quartz tube is placed in a muffle furnace for an immersion experiment, and after the stainless steel material sample is naturally cooled in the furnace, the stainless steel material sample is taken out of the quartz tube, and then washed with deionized water and alcohol to remove residual salt, and finally dried in air to obtain a stainless steel material sample corroded by high-temperature molten chloride salt.

6. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 5, characterized in that: The mixed chloride salt is a mixture of NaCl, MgCl2 and KCl, wherein the amount of NaCl accounts for 30.2%, the amount of MgCl2 accounts for 47.1%, and the amount of KCl accounts for 22.7%.

7. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 5, characterized in that: The ratio of the weight of the mixed chloride salt to the surface area of ​​the stainless steel material is 4×10 4 g / m -2 ~6×10 4 g / m -2 .

8. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 5, characterized in that: The vacuum degree of the quartz tube sealed in the vacuum containing the stainless steel material sample and the mixed chloride salt is greater than 0.1Pa.

9. The stainless steel material resistant to high temperature molten chloride corrosion according to claim 5, characterized in that: The static immersion temperature of the quartz tube in the muffle furnace is 600° C. to 700° C.; the immersion time of the quartz tube in the muffle furnace is 200 h to 800 h.

10. An application of the stainless steel material resistant to high temperature molten chloride corrosion as claimed in any one of claims 1 to 3, characterized in that: The stainless steel material is applied to the structural material of chloride molten salt in solar thermal power generation technology.