Stable colorless coating process and system for BC assembly
By degreasing, pickling and drying the BC components, combined with vapor deposition technology and heat treatment, the problems of insufficient substrate treatment and coating stability in the existing technology are solved, and a high-quality and stable colorless coating process is achieved, which improves the The pass rate and production efficiency of coating.
Patent Information
- Application Number
- CN202410816006.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-01
AI Technical Summary
The existing colorless coating process of BC components lacks the substrate treatment process, which causes oil stains and impurities to affect the coating quality. Bubbles are easily generated during the coating process, and the lack of post-treatment leads to warping or cracks, reducing the pass rate and increasing production costs.
By degreasing, pickling and drying the BC substrate, the surface oil and impurities are removed; the vapor deposition technology of magnesium raw materials and photosensitizers is used to coat the film in a vacuum environment, heat treatment and strong convection drying, and finally curing is carried out to Stable coating.
The quality and fit strength of the coating are improved, bubble generation is prevented, residual stress in the coating is eliminated, the pass rate of coating processing is improved, and the production cost is reduced.
Smart Images

Figure CN118880244A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of BC component coating, and in particular, relates to a stable colorless coating process and system for BC components. Background Art
[0002] In the photovoltaic industry, BC components specifically refer to a type of component that uses N-type monocrystalline silicon wafers. It has a high conversion efficiency and is mainly used in solar power stations, distributed photovoltaic power generation systems, electric vehicle charging piles and other fields. This component has been widely used in distributed photovoltaic power generation systems. As an important technical representative of the photovoltaic industry, BC components have played an important role in promoting the development of renewable energy with their high efficiency, stability and reliability. They are recognized for their high reliability, good stability and long durability. The colorless coating process used for BC components is an important technology. This process improves the performance and appearance of BC components by forming a colorless film on the surface of the BC components.
[0003] The existing colorless coating process for BC components can basically meet the daily use needs, but there are still some shortcomings;
[0004] First, the existing BC component colorless coating process lacks the substrate treatment process before coating. The residual oil and impurities on the substrate surface will affect the subsequent coating process, thereby affecting the coating quality.
[0005] Second, the existing BC component colorless coating process is limited by the parameters during coating. Bubbles are easily generated during the coating process, resulting in low bonding strength between the coating and the substrate, affecting the stability of the coating.
[0006] Third, the existing BC component colorless coating process lacks post-processing of the membrane structure after coating, which makes the coating prone to warping or cracking during the subsequent drying and curing process, thereby reducing the qualified rate of the coating process and increasing production costs.
[0007] Therefore, it is necessary to design a stable colorless coating process and system for BC components. Summary of the invention
[0008] In order to overcome the defects of the above-mentioned prior art, the present application provides a stable colorless coating process for BC components and its application.
[0009] The first object of the present application is to provide a stable colorless coating process for BC components, comprising:
[0010] Degreasing the BC substrate to obtain a degreased substrate;
[0011] performing pickling treatment on the degreased substrate to obtain a pickled substrate;
[0012] Drying the pickled substrate to obtain a water-free substrate;
[0013] Mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material;
[0014] Using vapor deposition raw materials to perform vapor deposition on an anhydrous substrate to obtain a colorless coating substrate;
[0015] heat-treating the colorless coating substrate to obtain a heat-treated coating material;
[0016] Performing strong convection drying on the heat-treated coating material to obtain a dry coating;
[0017] The dried coating is cured to obtain a stable colorless coating.
[0018] Furthermore, before degreasing, the BC components were mechanically scrubbed for 3 to 4 minutes and then rinsed with deionized water for 1 to 2 minutes;
[0019] Ethyl acetate is used as the degreasing agent for degreasing treatment, and the degreasing treatment temperature is 45-55°C and the time is 17-20 minutes;
[0020] After degreasing, the BC components are dried at a temperature of 180 to 200°C for 20 to 30 minutes.
[0021] Furthermore, before the pickling treatment, the degreased substrate is subjected to an alkaline washing treatment for 5 to 8 minutes using a sodium hydroxide solution having a concentration of 2% to 3%, and then rinsed with deionized water for 1 to 2 minutes;
[0022] The pickling treatment includes washing the degreased substrate with a sulfuric acid solution having a concentration of 10% to 20% for 30 to 35 minutes, and the content of ferrous sulfate in the sulfuric acid solution during the pickling treatment is 100 to 180 g / L;
[0023] After the pickling treatment, the degreased substrate is washed with water for 5 to 8 minutes.
[0024] Furthermore, the drying process is carried out at a temperature of 180 to 200° C. and for a time of 20 to 30 minutes.
[0025] Further, the mass ratio of the photosensitizer to the magnesium raw material is 0.15% to 0.18%;
[0026] The mixing temperature is 35-50°C, the stirring speed is 25-30 r / min, and the stirring time is 17-25 min.
[0027] Furthermore, the vacuum degree of the evaporation source during the vapor deposition process is 10 -3 ~10 -4Pa, the heating temperature of the evaporation source is 210~230℃.
[0028] Furthermore, the heat treatment includes keeping the colorless coated substrate at a constant temperature of 200 to 210° C. for 180 to 200 minutes, and then cooling it to 25 to 45° C. at room temperature.
[0029] Furthermore, the temperature of the strong convection drying treatment is 280-300° C., the time is 50-60 minutes, and the drying medium includes argon gas.
[0030] Furthermore, the curing treatment temperature is 180-183° C. and the time is 120-150 min.
[0031] The second object of the present application is to provide a stable colorless coating system for BC components, comprising:
[0032] A degreasing module, used for degreasing the BC substrate to obtain a degreased substrate;
[0033] A pickling module, used for pickling the degreased substrate to obtain a pickled substrate;
[0034] A drying module, used for drying the pickled substrate to obtain a water-free substrate;
[0035] A mixing module, used for mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material;
[0036] A vapor deposition module is used to perform vapor deposition on a water-free substrate using a vapor deposition raw material to obtain a colorless coating substrate;
[0037] A heat treatment module is used to heat treat the colorless coating substrate to obtain a heat-treated coating material;
[0038] A drying module is used to perform strong convection drying on the heat-treated coating material to obtain a dry coating;
[0039] The curing module is used to cure the dried coating to obtain a stable colorless coating.
[0040] Technical effects and advantages of this application:
[0041] 1. This application sequentially cleans, degreases and pickles the BC substrate to remove residual oil and impurities on the surface of the BC substrate, thereby ensuring the quality of the coating.
[0042] 2. In the present application, magnesium raw material with added photosensitizer mixed with fluorine gas is used as the raw material for vapor deposition, and coating is performed on the surface-treated BC substrate. During the coating process, the vacuum degree inside the equipment is increased and the negative pressure environment in the evaporation source is maintained so that the coating is closely attached to the surface of the substrate. This can reduce the gas dissolution process, inhibit gas diffusion, and prevent the generation of impurities and bubbles during the coating process, thereby ensuring the bonding strength after coating and making the coating effect more stable.
[0043] 3. The present application can eliminate the residual stress in the coating by heat-treating the colorless coated substrate and then sending it to the drying and curing process, thereby preventing the coating from deforming in the later stage and causing warping or cracking, thereby improving the qualified rate of the coating processing and reducing production costs.
[0044] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures indicated in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a flow chart of a stable colorless coating process for BC components of the present application. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0047] First, as Figure 1 As shown, the present application provides a stable colorless coating process for BC components, including: degreasing the BC substrate to obtain a degreased substrate; pickling the degreased substrate to obtain a pickled substrate; drying the pickled substrate to obtain an anhydrous substrate; mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material; using the vapor deposition raw material to perform vapor deposition on an anhydrous substrate to obtain a colorless coating substrate; heat-treating the colorless coating substrate to obtain a heat-treated coating material; performing strong convection drying on the heat-treated coating material to obtain a dry coating; and curing the dry coating to obtain a stable colorless coating.
[0048] In some embodiments of the present application, before degreasing, the BC substrate is first placed in a cleaning tank, and the BC component is mechanically scrubbed for 3 to 4 minutes using a brush, and then continuously rinsed with deionized water for 1 to 2 minutes; then the rinsed BC component is placed in a treatment tank, and ethyl acetate is selected as a degreasing agent to degrease the rinsed BC component. During the degreasing process, the temperature in the treatment tank is 45 to 55°C, and the degreasing time is 17 to 20 minutes; after the degreasing process, the BC component is placed in an oven for drying, and the drying temperature is 180 to 200°C, and the drying time is 20 to 30 minutes. By cleaning and degreasing the BC substrate, the residual oil and impurities on the surface of the BC substrate can be removed, and the oil and impurities can be prevented from affecting the subsequent coating process, thereby ensuring the quality of the coating.
[0049] In some embodiments of the present application, before the pickling treatment, the degreased substrate is subjected to alkaline washing treatment for 5 to 8 minutes using a sodium hydroxide solution with a concentration of 2% to 3%, and then rinsed with deionized water for 1 to 2 minutes; the pickling treatment includes washing the degreased substrate with a sulfuric acid solution with a concentration of 10% to 20% for 30 to 35 minutes, and the content of ferrous sulfate in the sulfuric acid solution is maintained at 100 to 180 g / L during the pickling treatment; after the pickling treatment, the degreased substrate is washed with water for 5 to 8 minutes. By pickling the degreased substrate, the oil and impurities remaining on the surface of the BC substrate can be further removed.
[0050] In some embodiments of the present application, when the pickled substrate is dried, the pickled substrate is placed in an oven, the temperature of the oven is adjusted to 180-200° C., and the drying time is 20-30 min.
[0051] In some embodiments of the present application, a magnesium raw material and a photosensitizer are placed in a blender for mixing to obtain a vapor deposition raw material, wherein the mass ratio of the photosensitizer to the magnesium raw material is 0.15% to 0.18%, the temperature in the blender during mixing is 35 to 50°C, the stirring speed of the blender is 25 to 30 r / min, and the stirring time is 17 to 25 min.
[0052] In some embodiments of the present application, an anhydrous substrate is used as a substrate of an evaporation source, a vapor deposition raw material is placed in the evaporation source, a vacuum system is turned on, and the vacuum degree of the evaporation source is controlled at 10 -3 ~10 -4Pa, then discharge the fluorine gas into the evaporation source, heat the evaporation source to 210-230°C, sublimate the vapor deposition raw material into steam, transport it to the substrate under negative pressure, and perform vapor deposition on the anhydrous substrate as the substrate to obtain a colorless coated substrate. The present application uses magnesium raw material with added photosensitizer mixed with fluorine gas as the raw material for vapor deposition, and performs coating on the surface-treated BC substrate. During the coating process, the vacuum degree inside the equipment is increased, and the negative pressure environment in the evaporation source is maintained to make the coating close to the surface of the substrate, which can reduce the gas dissolution process, inhibit the diffusion of the gas, and prevent the generation of impurities and bubbles during the coating process, thereby ensuring the bonding strength after coating and making the coating effect more stable.
[0053] In some embodiments of the present application, when the colorless coated substrate is heat-treated, the prepared colorless coated substrate is placed in a constant temperature chamber at 200-210°C and kept at a constant temperature for 180-200 minutes, and then the heated and heat-insulated colorless coated substrate is cooled to 25-45°C at room temperature. After the coating is completed, the colorless coated substrate is first heat-treated and then sent to the drying and curing process, which can eliminate the residual stress in the coating, stabilize the coating structure, and prevent the coating from deforming in the later stage, causing warping or cracking.
[0054] In some embodiments of the present application, the temperature of the strong convection drying treatment is 280-300° C., the time is 50-60 min, and the drying medium includes argon.
[0055] In some embodiments of the present application, when the dry coating is cured, the prepared dry coating is placed in a curing device, the curing temperature is set to 80-183°C, the curing time is set to 120-150 minutes, and the dry coating after curing is cooled to form a stable colorless coating on the BC component.
[0056] In a second aspect, the present application discloses a stable colorless coating system for BC components, comprising:
[0057] A degreasing module, used for degreasing the BC substrate to obtain a degreased substrate;
[0058] A pickling module, used for pickling the degreased substrate to obtain a pickled substrate;
[0059] A drying module, used for drying the pickled substrate to obtain a water-free substrate;
[0060] A mixing module, used for mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material;
[0061] A vapor deposition module is used to perform vapor deposition on a water-free substrate using a vapor deposition raw material to obtain a colorless coating substrate;
[0062] A heat treatment module is used to heat treat the colorless coating substrate to obtain a heat-treated coating material;
[0063] A drying module is used to perform strong convection drying on the heat-treated coating material to obtain a dry coating;
[0064] The curing module is used to cure the dried coating to obtain a stable colorless coating.
[0065] In summary, the present application sequentially cleans, degreases and pickles the BC substrate before coating to remove residual oil and impurities on the surface of the BC substrate, thereby preventing the oil and impurities from affecting the subsequent coating process, thereby ensuring the quality of the coating; during the coating process, by increasing the vacuum degree inside the equipment, the gas dissolution process is reduced, the gas diffusion is inhibited, and the generation of impurities and bubbles during the coating process is prevented, which can ensure the bonding strength after coating and make the coating effect more stable; after coating, the colorless coated substrate is heat-treated and then sent to the drying and curing process to eliminate residual stress in the coating, prevent the subsequent coating deformation from causing warping or cracking, thereby improving the pass rate of the coating process and reducing production costs.
[0066] Finally, it should be noted that the above is only a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A stable colorless coating process for BC components, It is characterized in that include: Degreasing the BC substrate to obtain a degreased substrate; Performing pickling treatment on the degreased substrate to obtain a pickled substrate; Drying the acid-washed substrate to obtain an anhydrous substrate; Mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material; Using the vapor deposition raw material to perform vapor deposition on the anhydrous substrate to obtain a colorless film-coated substrate; Heat-treating the colorless film-coated substrate to obtain a heat-treated film-coated material; Performing a strong convection drying treatment on the heat-treated coating material to obtain a dry coating; The dried plated film is cured to obtain a stable colorless plated film.
2. A stable colorless coating process for BC components according to claim 1, It is characterized in that Before the degreasing treatment, the BC component is mechanically scrubbed for 3 to 4 minutes and then rinsed with deionized water for 1 to 2 minutes; The degreasing treatment uses ethyl acetate as a degreasing agent, the degreasing treatment temperature is 45-55°C, and the time is 17-20 minutes; After the degreasing treatment, the BC assembly is dried at a temperature of 180 to 200° C. for 20 to 30 minutes.
3. A stable colorless coating process for BC components according to claim 1, It is characterized in that Before the pickling treatment, the degreased substrate is subjected to an alkali washing treatment for 5 to 8 minutes using a sodium hydroxide solution having a concentration of 2% to 3%, and then rinsed with deionized water for 1 to 2 minutes; The pickling treatment includes washing the degreased substrate with a sulfuric acid solution having a concentration of 10% to 20% for 30 to 35 minutes, wherein the content of ferrous sulfate in the sulfuric acid solution during the pickling treatment is 100 to 180 g / L; After the pickling treatment, the degreased substrate is washed with water for 5 to 8 minutes.
4. A stable colorless coating process for BC components according to claim 1, It is characterized in that The drying process is carried out at a temperature of 180 to 200° C. and for a time of 20 to 30 minutes.
5. A stable colorless coating process for BC components according to claim 1, It is characterized in that The mass ratio of the photosensitizer to the magnesium raw material is 0.15% to 0.18%; The mixing temperature is 35-50° C., the stirring speed is 25-30 r / min, and the stirring time is 17-25 min.
6. A stable colorless coating process for BC components according to claim 1, It is characterized in that The vacuum degree of the evaporation source during the vapor deposition process is 10 -3 ~10 -4 Pa, the heating temperature of the evaporation source is 210~230℃.
7. A stable colorless coating process for BC components according to claim 1, It is characterized in that The heat treatment comprises placing the colorless coated substrate at a constant temperature of 200 to 210° C. for 180 to 200 minutes, and then cooling it to 25 to 45° C. at room temperature.
8. A stable colorless coating process for BC components according to claim 1, It is characterized in that The temperature of the strong convection drying treatment is 280-300° C., the time is 50-60 minutes, and the drying medium includes argon gas.
9. A stable colorless coating process for BC components according to claim 1, It is characterized in that The curing treatment is performed at a temperature of 180 to 183° C. and for a time of 120 to 150 minutes.
10. A stable colorless coating system for BC components, It is characterized in that include: A degreasing module, used for degreasing the BC substrate to obtain a degreased substrate; A pickling module, used for pickling the degreased substrate to obtain a pickled substrate; A drying module, used for drying the acid-washed substrate to obtain a water-free substrate; A mixing module, used for mixing a magnesium raw material and a photosensitizer to obtain a vapor deposition raw material; A vapor deposition module, used for performing vapor deposition on the anhydrous substrate using the vapor deposition raw material to obtain a colorless coated substrate; A heat treatment module, used for heat treating the colorless film-coated substrate to obtain a heat-treated film-coated material; A drying module, used for performing a strong convection drying treatment on the heat-treated coating material to obtain a dry coating; The curing module is used to perform curing treatment on the dried coating to obtain a stable colorless coating.