Vacuum coating method
By independently using different target materials and gas deposited film layers in the vacuum coating process cavity, the problem of impurities entering is solved, the film layer purity and coating quality are improved, and the requirements of high-end mask plates are met.
Patent Information
- Application Number
- CN202411365320.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the vacuum coating process, when multiple film layers are deposited on the surface of the workpiece material, impurities are easily introduced, which affects the coating effect and cannot meet the application requirements.
The film layer is deposited independently using the first target material and the second target material in the same process cavity, and the coating operation is carried out through different process gases and sputtering areas to prevent impurities from entering each film layer.
It effectively improves the purity of the film layer and the quality of the coated workpieces, meeting the coating needs of high-end mask plates.
Smart Images

Figure CN118880255A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of vacuum coating, and in particular to a vacuum coating method. Background Art
[0002] Vacuum coating technology is widely used to improve the properties of workpiece materials and enrich their functions. It mainly uses magnetron sputtering and other technologies to sputter the target material under vacuum conditions to deposit a functional film layer on the surface of the workpiece material so that the coated workpiece meets the application requirements.
[0003] In the commonly used coating methods, coating is directly achieved by sputtering after the target material reacts in the atmosphere of process gas to form a film layer on the surface of the workpiece material. However, when depositing multiple film layers on the surface of the workpiece material, it is necessary to use multiple process gases to react with the target material separately. During the sputtering coating process, impurities are easily introduced into each film layer, affecting the coating effect, resulting in the obtained coated workpiece failing to meet the application requirements. Summary of the invention
[0004] In view of the problems in the prior art, the present application provides a vacuum coating method, which can ensure the purity of the deposited film layer, thereby effectively improving the performance of the coated workpiece.
[0005] The vacuum coating method provided in the present application performs coating operations in the same process chamber, wherein the process chamber is provided with a conveying assembly, a first target material and a second target material, and a first sputtering coating area and a second sputtering coating area respectively provided corresponding to the first target material and the second target material. The vacuum coating method comprises the following steps: A first process gas is introduced into the process chamber and the first target material is started. The workpiece to be plated is transported by the conveying assembly to the first sputtering coating area for the first sputtering coating. When the workpiece is moved out of the first sputtering coating area, the first film layer is deposited, and the ventilation and the operation of the first target material are stopped. A second process gas is introduced into the process chamber and the second target is started. The workpiece to be plated is transported by the conveying assembly to the second sputtering coating area for a second sputtering coating. When the workpiece is moved out of the second sputtering coating area, the second film layer is deposited, and the ventilation and the operation of the second target are stopped. During the process of introducing process gas into the process chamber, the process chamber is evacuated to maintain a stable internal pressure; The first process gas and the second process gas are different process gases.
[0006] Several optional methods are also provided below, but they are not intended to be additional limitations on the above-mentioned overall solution, but are merely further supplements or preferences. Under the premise that there are no technical or logical contradictions, each optional method can be combined with the above-mentioned overall solution separately, and multiple optional methods can also be combined.
[0007] Optionally, the first sputtering coating area and the second sputtering coating area are spaced apart in a conveying direction of the workpiece to be plated, and both the first process gas and the second process gas are introduced into the process chamber from the spaced area.
[0008] Optionally, the first process gas is blown toward the first target material or is blown perpendicularly to the traveling direction of the workpiece to be plated; The second process gas is blown toward the second target material or perpendicular to the moving direction of the workpiece to be plated.
[0009] Optionally, the first target material and the second target material are both selected from one of a chromium target material, a molybdenum target material, and a silicon target material.
[0010] Optionally, the first process gas is a mixture of nitrogen and argon, and the second process gas is a mixture of argon, nitrogen and carbon dioxide.
[0011] Optionally, the workpiece to be plated is preheated in a heating chamber and then sent into the process chamber for a first coating, and the heating chamber is arranged adjacent to the process chamber.
[0012] Optionally, the vacuum coating method comprises: The workpiece to be plated enters the heating chamber along a first moving direction to undergo the heating treatment; After completing the heating treatment, entering the process chamber along the second moving direction to perform the first sputtering coating; After completing the first sputtering coating, exit the process chamber, and then enter the process chamber along the first moving direction to perform the second coating; After completing the second sputtering coating, exit the process chamber; The first traveling direction and the second traveling direction are opposite.
[0013] Optionally, the workpiece to be plated passes through the vacuum transition chamber and the process chamber in sequence along a first direction and then enters the heating chamber, and the vacuum transition chamber and the heating chamber are respectively adjacent to two sides of the process chamber.
[0014] Optionally, after completing the first sputtering coating, the workpiece to be plated exits the process chamber and enters the vacuum transition chamber. After the second process gas and the second target material are ready, the workpiece to be plated returns to the process chamber along the first moving direction for a second sputtering coating. After completing the second sputtering coating, it exits from the process chamber along the second moving direction to the vacuum transition chamber.
[0015] Optionally, the vacuum coating method comprises: The workpiece to be plated enters the heating chamber along a first moving direction to undergo the heating treatment; After completing the heating treatment, entering the process chamber along the second moving direction to sequentially perform the first sputtering coating and the second sputtering coating, and exiting from the process chamber after completion; The first traveling direction and the second traveling direction are opposite.
[0016] Compared with the prior art, the present application uses the first target material to deposit the first film layer and the second target material to deposit the second film layer independently in the same process chamber at different coating stages, which can effectively avoid introducing impurities into each film layer, which is beneficial to improving the purity of each film layer, thereby ensuring the quality of the coated workpiece. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 A schematic diagram of a horizontal vacuum coating system in one embodiment of the present application; Figure 2 It is a schematic diagram of an existing horizontal vacuum coating system.
[0018] The reference numerals in the figures are described as follows: 100, horizontal vacuum coating system; 101, loading and unloading chamber; 102, low vacuum chamber; 103, high vacuum chamber; 104, process chamber; 105, heating chamber; 106, gas distribution pipe assembly; 107, transfer wheel; 108, first target; 109, second target; 110, first valve; 111, second valve; 112, third valve; 200. Existing horizontal vacuum coating system; 201. Loading and unloading chambers; 202. Low vacuum chamber; 203. First high vacuum chamber; 204. Process chamber; 205. Second high vacuum chamber; 206. Heating chamber; 207. First gas distribution pipe; 208. Second gas distribution pipe; 209. Conveying assembly; 210. First target material; 211. Second target material; 212. First valve; 213. Second valve; 214. Third valve; 300. Substrate. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0020] It should be noted that when a component is referred to as being "connected" to another component, it may be directly connected to the other component or there may be a central component. When a component is referred to as being "disposed on" another component, it may be directly disposed on the other component or there may be a central component at the same time.
[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0022] An embodiment of the present application provides a vacuum coating system, including a process chamber 104 for coating operation, wherein a transmission component, a first target material 108 and a second target material 109 are arranged in the process chamber 104, and a first sputtering coating area and a second sputtering coating area are arranged in the process chamber 104 corresponding to the first target material 108 and the second target material 109, respectively. Based on the vacuum coating system, the present application provides a vacuum coating method, which specifically includes the following steps: A first process gas is introduced into the process chamber 104 and the first target 108 is started. The workpiece to be plated is transported by the conveyor assembly into the first sputtering coating area for the first sputtering coating. When the workpiece is moved out of the first sputtering coating area, the first film layer is deposited. Then, the gas supply and the operation of the first target 108 are stopped. A second process gas is introduced into the process chamber 104 and the second target 109 is started. The workpiece to be plated is transported to the second sputtering coating area by the conveyor assembly for a second sputtering coating. When the workpiece is moved out of the second sputtering coating area, the second film layer is deposited. Then, the gas supply and the operation of the second target 109 are stopped. During the process of introducing the process gas into the process chamber 104 , the process chamber 104 is evacuated to maintain a stable internal pressure. In this embodiment, the first process gas and the second process gas are different process gases. In the same process chamber 104, at different coating stages, the first target material 108 is used to deposit the first film layer and the second target material 109 is used to deposit the second film layer. This can effectively avoid introducing impurities into each film layer, which is beneficial to improving the purity of each film layer, thereby effectively improving the performance of the coated workpiece.
[0023] In order to avoid mutual contamination of the targets due to sputtering, the first sputtering coating area and the second sputtering coating area are arranged at intervals in the conveying direction of the workpiece to be plated, and the first process gas and the second process gas are both introduced into the process chamber 104 from the interval area. Specifically, corresponding to the layout of each sputtering coating area, the first target 108 and the second target 109 are arranged at intervals in the conveying direction of the workpiece to be plated, and the interval distance is not less than 900 mm.
[0024] See also Figure 1In the illustrated embodiment, the process chamber 104 is equipped with a set of common gas distribution devices, which can introduce corresponding process gases into the process chamber 104 at different coating stages. To ensure the coating effect at each stage, the gas distribution device includes a gas distribution pipe assembly 106 with gas outlets, and the gas distribution pipe assembly 106 is arranged in the interval area between the first target material 108 and the second target material 109, so that the first process gas and the second process gas are both introduced into the process chamber 104 from the interval area between the first target material 108 and the second target material 109. The gas distribution pipe assembly 106 includes a main gas pipe and auxiliary gas pipes arranged on both sides of the main gas pipe, wherein the auxiliary gas pipe is a multi-stage structure arranged along the extension direction of the main gas pipe, for example, a three-stage structure.
[0025] Furthermore, the first process gas is blown toward the first target 108 or perpendicular to the moving direction of the workpiece to be plated, and the second process gas is blown toward the second target 109 or perpendicular to the moving direction of the workpiece to be plated. Preferably, in each coating stage, the first process gas and the second process gas are blown perpendicular to the moving direction of the workpiece to be plated, which is more conducive to reducing sputtering contamination between the two targets.
[0026] In addition, during the coating process, the gas is evacuated simultaneously, and the evacuation direction of the process chamber 104 is perpendicular to the moving direction of the workpiece to be plated. For example, when the first process gas is introduced into the process chamber 104, the gas is evacuated simultaneously until the first film layer is deposited, and before the second process gas is introduced into the process chamber 104, the process chamber 104 is evacuated to a certain vacuum degree before the second process gas is introduced, that is, the waste gas generated by the first sputtering coating is discharged before the second process gas is introduced.
[0027] The vacuum coating method of the present application can be applied to prepare a mask plate, which is a structure on which various functional patterns are made and precisely positioned on a substrate material for selective exposure of a photoresist coating, and can be used as a graphic master used in the photolithography process in microelectronics manufacturing.
[0028] In one embodiment, the substrate of the workpiece to be plated is quartz glass, and the light shielding layer is a composite film layer, including a first film layer and a second film layer sequentially arranged on the surface of the substrate, wherein the first film layer is a film layer with low light transmittance, such as a film layer formed by chromium nitride, molybdenum oxynitride or silicon oxynitride. Although the light transmittance of such film layers is ≤0.1%@450nm, which can play a good light shielding effect, the surface reflectivity is high. Therefore, the second film layer is a film layer with low reflectivity, such as a film layer formed by chromium oxynitride, molybdenum oxynitride or silicon oxynitride. The reflectivity of these film layers is ≤12%@436nm, which can effectively reduce surface reflection. The light shielding layer formed by the first film layer and the second film layer has a good light shielding effect. In the first film layer, the ratio of chromium (molybdenum or silicon) atoms to nitrogen atoms is 1~2:1; in the second film layer, the ratio of chromium (molybdenum or silicon) atoms, oxygen atoms and nitrogen atoms is 1~2:2~3:1~2.
[0029] Corresponding to each film layer, the first target 108 and the second target 109 are selected from one of a chromium (Cr) target, a molybdenum (Mo) target or a silicon (Si) target. For example, the first target 108 and the second target 109 are both chromium targets. Each target can be a planar target.
[0030] The process gases used in each coating stage are different. The first process gas is a mixture of nitrogen and argon, and the second process gas is a mixture of nitrogen, carbon dioxide and argon. When depositing the first film layer, the volume ratio of argon and nitrogen in the first process gas is (3-8):1, the pumping rate is 12000-18000L / s, the flow rate of argon is 100-500sccm, the flow rate of nitrogen is 30-200sccm, and the process pressure is 0.2-0.8Pa.
[0031] When depositing the second film layer, the volume ratio of argon, nitrogen and carbon dioxide in the second process gas is (1-4): (1-5): (0.1-0.5), the pumping rate in the process chamber 104 is 10000-14000 L / s, the flow rate of argon is 100-400 sccm, the flow rate of nitrogen is 100-500 sccm, the flow rate of carbon dioxide is 10-50 sccm, and the process pressure is 0.2-0.8 Pa.
[0032] Usually, the workpiece to be plated needs to be preheated before being sent into the process chamber 104 for the first coating. Accordingly, the vacuum coating system includes a heating chamber 105 arranged adjacent to the process chamber 104, and the workpiece to be plated is heated in the heating chamber 105.
[0033] In a specific embodiment, the vacuum coating method A comprises: The workpiece to be plated enters the heating chamber 105 along a first moving direction for heating treatment; After the heating treatment is completed, the first sputtering coating is performed by entering the process chamber 104 along the second moving direction; After the first sputtering coating is completed, the process chamber 104 is exited, and then the process chamber 104 is entered along the first moving direction for the second coating; After completing the second sputtering coating, exit the process chamber 104; The first traveling direction and the second traveling direction are opposite.
[0034] Furthermore, the workpiece to be plated passes through the vacuum transition chamber and the process chamber 104 in sequence along the first direction and then enters the heating chamber 105, and the vacuum transition chamber and the heating chamber 105 are respectively adjacent to the two sides of the process chamber 104. After the first sputtering coating is completed, the workpiece to be plated exits the process chamber 104 and enters the vacuum transition chamber, and after the second process gas and the second target material 109 are ready, the workpiece to be plated returns to the process chamber 104 along the first moving direction for the second sputtering coating; after the second sputtering coating is completed, the workpiece exits the vacuum transition chamber from the process chamber 104 along the second moving direction.
[0035] In another embodiment, the vacuum coating method B comprises: The workpiece to be plated enters the heating chamber 105 along a first moving direction for heating treatment; After the heating treatment is completed, the first moving direction and the second moving direction are entered into the process chamber 104 to perform the first sputtering coating and the second sputtering coating in sequence, and then the first moving direction and the second moving direction are exited from the process chamber 104 after completion. The first moving direction and the second moving direction are opposite.
[0036] Furthermore, the workpiece to be plated passes through the vacuum transition chamber and the process chamber 104 in sequence along the first direction and then enters the heating chamber 105, and the vacuum transition chamber and the heating chamber 105 are respectively adjacent to the two sides of the process chamber 104. After the workpiece to be plated is coated, it exits from the process chamber 104 to the vacuum transition chamber along the second direction.
[0037] See also Figure 1 In the illustrated embodiment, the vacuum coating system includes an upper and lower material chamber 101, a vacuum transition chamber, a process chamber 104, and a heating chamber 105, which are arranged in sequence, wherein the upper and lower material chamber 101 has an inlet and outlet for allowing the workpiece to be plated to enter and exit the entire system, and the vacuum transition chamber, the process chamber 104, and the heating chamber 105 are sealed and connected in sequence. In the entire process, the workpiece to be plated is input from the inlet and outlet, and then performs reciprocating linear motion (first direction of travel and second direction of travel) to complete the heating and coating operations, and after the coating is completed, it is output from the upper and lower material chamber 101.
[0038] Furthermore, the vacuum coating system includes two vacuum transition chambers connected in sequence, namely a low vacuum chamber 102 and a high vacuum chamber 103, wherein a first valve 110 is provided on the side where the loading and unloading chamber 101 is connected to the low vacuum chamber 102, a second valve 111 is provided on the side where the low vacuum chamber 102 is connected to the high vacuum chamber 103, and a third valve 112 is provided on the side where the high vacuum chamber 103 is connected to the process chamber 104. The process chamber 104 and the heating chamber 105 are not provided with valves and are always connected during the coating process. In this design, the heating chamber also serves as a buffer chamber for the coating process, thereby effectively reducing the length and manufacturing cost of the overall equipment. To avoid contamination, the heating chamber is basically made of aluminum material in one piece, and an anti-oxidation aluminum oxide layer can be formed on the surface during the coating process.
[0039] Accordingly, the vacuum coating method comprises the following steps: The first valve 110 is opened, and the workpiece to be plated enters the low vacuum chamber 102 from the loading and unloading chamber 101 along the first moving direction, and the first valve 110 is closed to evacuate the low vacuum chamber 102 until a first preset vacuum state is reached; The second valve 111 is opened, and the workpiece to be plated enters the high vacuum chamber 103 from the low vacuum chamber 102. The second valve 111 is closed, and the high vacuum chamber 103 is evacuated until a second preset vacuum state is reached; The third valve 112 is opened, and the workpieces to be plated sequentially enter the process chamber 104 and then reach the heating chamber 105 for heating treatment; After the heating treatment is completed, the workpiece to be plated enters the process chamber 104 along the second moving direction for the first sputtering coating; After the first sputtering coating is completed, the process chamber 104 is exited and the high vacuum chamber 103 is entered; After the second process gas and the second target material 109 of the process chamber 104 are ready, the workpiece to be plated enters the process chamber 104 along the first direction for a second sputtering coating; After the second sputtering coating is completed, the coated workpiece enters the high vacuum chamber 103 along the second moving direction, and the third valve 112 is closed; The second valve 111 is opened, the coating workpiece continues to move along the second moving direction and enters the low vacuum chamber 102, and the second valve 111 is closed; The low vacuum chamber 102 is vented until it reaches an atmospheric equilibrium point, the first valve 110 is opened, and the coated workpiece enters the upper and lower material chambers 101 for discharge.
[0040] In one embodiment, the vacuum coating system is a horizontal vacuum coating system 100, wherein the first target material 108, the second target material 109 and the air distribution pipe assembly 106 are located below the conveying assembly. The conveying assembly includes a conveying wheel 107 and a driving mechanism, the wheel surface of the conveying wheel 107 is a concave surface, the workpiece to be plated is loaded on the workpiece rack and sent into the upper and lower material chamber 101, and the bottom surface of the workpiece rack is provided with a guide rod that cooperates with the wheel surface of the conveying wheel 107. Furthermore, in order to effectively exhaust air, an exhaust port is opened at the bottom of the horizontal vacuum coating system, and the exhaust port is equipped with an exhaust pump, such as a molecular pump, and the exhaust airflow direction flows to the exhaust port of the molecular pump.
[0041] The following provides specific application examples in combination with specific parameters to further illustrate the present application.
[0042] Application Example 1 The substrate used is a quartz glass substrate, the vacuum coating system is a horizontal vacuum coating system 100, the first target material 108 and the second target material 109 in the process chamber 104 are chromium flat targets, and the purity of the target materials is not less than 99.99%. The vacuum coating method includes the following steps: (1) The cleaned substrate is transported by a robot and placed in the loading and unloading chamber 101, the first valve 110 is opened, the substrate is transferred from the loading and unloading chamber 101 to the low vacuum chamber 102, and the first valve 110 is closed; (2) The low vacuum chamber 102 is roughly pumped by the rough pumping group, and the atmospheric state of the low vacuum chamber 102 is pumped to the starting range of the molecular pump; (3) After the molecular pump starts to reach the range, the molecular pump dedicated plug valve of the low vacuum chamber 102 is opened, and the molecular pump can further increase the vacuum degree of the low vacuum chamber 102 to high vacuum; (4) The low vacuum chamber 102 reaches high vacuum (1.0×10 -3 After pa), the second valve 111 is opened, the substrate is transferred from the low vacuum chamber 102 to the high vacuum chamber 103, and the second valve 111 is closed; (5) Open the third valve 112, transfer the substrate from the high vacuum chamber 103 to the process chamber 104, and then stop at the heating chamber 105, bake the substrate, and set the baking time to 600 to 900 seconds. The baking time is determined according to the thickness of the substrate; (6) After the baking time is reached, Cr x N y The first process gas formula for film formation is introduced, and the cathode 1 sputtering power supply is turned on. The substrate is reversely driven through the first target 108 and exits the first sputtering zone to complete the Cr x N y Coating, turn off the first target 108 sputtering power, turn off Cr x N y The MFC formulation of the coating atmosphere, the substrate continues to move out of the second target 109 in the reverse direction and stops at the high vacuum chamber 103; (7) Cr x O y N z The second process gas formula for film formation is introduced, and the cathode 2 sputtering power supply is turned on. The substrate is forwardly driven through the second target material 109 and out of the second sputtering zone to complete the Cr x O y N z The coating is stopped, the sputtering power of the second target 109 is turned off, and the Cr x O y N z Coating atmosphere, according to the set Cr x O y N zThe film is stabilized for a film stabilization time (1.5 to 3 minutes). After the film stabilization time is reached, the substrate is reversely driven to the high vacuum chamber 103 to stop, and the third valve 112 is closed; (8) The second valve 111 is opened, the substrate is transferred from the high vacuum chamber 103 to the low vacuum chamber 102 and stops, and the second valve 111 is closed; (9) Stop exhausting the low vacuum chamber 102, and open the air-breaking valve to break the vacuum of the low vacuum chamber 102 to the atmospheric equilibrium point; (10) After the atmosphere confirmation meter confirms that the low vacuum chamber 102 has reached the atmospheric pressure, the first valve 110 is opened, and the substrate is transferred from the low vacuum chamber 102 to the loading and unloading chamber 101 and stops. The robot then carries and unloads the mask substrate that has been coated.
[0043] The first process gas formula is: the volume ratio of argon to nitrogen is 3:1, the pumping rate in the process chamber 104 is 15000 L / s, the flow rate of argon is 300 sccm, the flow rate of nitrogen is 100 sccm, the process pressure is 0.2 Pa, and the final Cr x N y The composition is controlled at x:y of 1:1.
[0044] The second process gas formula is: the volume ratio of argon, nitrogen and carbon dioxide is 3.5:1:0.3, the pumping rate in the process chamber 104 is 12000L / s, the flow rate of argon is 350sccm, the flow rate of nitrogen is 100sccm, the flow rate of carbon dioxide is 30sccm, the process pressure is 0.22Pa, and the final Cr x O y N z The composition is controlled at x:y:z of 1:3:1, with basically no other impurities. The entire film layer has good light-shielding properties, with a transmittance of ≤0.1%@450nm and a reflectivity of 10~11%@436nm.
[0045] Comparative Example 1 Figure 2 An existing horizontal vacuum coating system 200 is shown, comprising an upper and lower material chamber 101, a low vacuum chamber 202, a first high vacuum chamber 203, a process chamber 204, a second high vacuum chamber 205 and a heating chamber 206 connected in sequence, wherein a first valve 212 is provided between the upper and lower material chamber 101 and the low vacuum chamber 202, a second valve 213 is provided between the low vacuum chamber 202 and the first high vacuum chamber 203, and a third valve 214 is provided between the second high vacuum chamber 205 and the heating chamber 206. The substrate used for coating is a soda glass substrate, and the first target material 210 and the second target material 211 in the process chamber are chromium flat targets, and the purity of the target material is 99.95%. The coating method comprises the following steps: (1) The cleaned substrate is transported by a robot and placed in the loading and unloading chamber 101, the first valve 212 is opened, the substrate is transferred from the loading and unloading chamber 101 to the low vacuum chamber 202, and the first valve 212 is closed; (2) The low vacuum chamber 202 is roughly pumped by the rough pump group, and the atmospheric state of the low vacuum chamber 202 is pumped to the starting range of the molecular pump; (3) The second valve 213 is opened, the substrate is transferred from the low vacuum chamber 202 to the first high vacuum chamber 203, and the second valve 213 is closed; (4) The substrate is sequentially transferred from the first high vacuum chamber 203 to the process chamber 204, the second high vacuum chamber 205, and stops at the heating chamber 206. The substrate is baked and the baking time is set to 600 to 900 seconds. The baking time is determined according to the thickness of the substrate. (5) After the baking time is reached, Cr x O y The first process gas formula for film formation is introduced, and the sputtering power of the first target 210 and the second target 211 is turned on at the same time. The substrate is reversely driven to pass through the first target 210 and the second target 211 in turn and exit the sputtering area of the second target 211 to reach the first high vacuum chamber 203 and stop, completing the Cr x O y Coating, turn off the sputtering power of the first target 210 and the second target 211, turn off the Cr x O y MFC formulation of coating atmosphere; (6) Cr x N y The second process gas formula for film formation is introduced, and the sputtering power of the first target 210 and the second target 211 is turned on at the same time. The substrate is driven forward and passes through the second target 211 and the first target 210 in sequence, and then goes out of the sputtering area of the first target 210 to reach the second high vacuum chamber 205, completing the Cr x N y Coating, turn off the sputtering power of the first target 210 and the second target 211, turn off the Cr x N y MFC formulation of coating atmosphere; (7) Cr x O y N z The third process gas formula for film formation is introduced, and the sputtering power of the first target 210 and the second target 211 is turned on at the same time. The substrate is reversely driven to pass through the first target 210 and the second target 211 in turn, and then goes out of the sputtering area of the second target 211 to reach the first high vacuum chamber 203, completing the Cr x O y N z The coating is stopped, the sputtering power of the first target 210 and the second target 211 is turned off, and the Cr x Oy N z Coating atmosphere, according to the set Cr x O y N z Stabilize the film for 1.5 to 3 minutes; (8) After the film stabilization time is reached, the second valve 213 is opened, the substrate is reversely driven from the first high vacuum chamber 203 to the low vacuum chamber 202 and stops, and the second valve 213 is closed; (9) Stop exhausting the low vacuum chamber 202, and open the air-breaking valve to break the vacuum in the low vacuum chamber 202 to the atmospheric equilibrium point; (10) After the atmosphere confirmation meter confirms that the low vacuum chamber 202 has reached the atmospheric pressure, the first valve 212 is opened, and the substrate is transferred from the low vacuum chamber 202 to the loading and unloading chamber 101 and stops. The robot then carries and unloads the mask substrate that has been coated.
[0046] The existing process is a coating method using soda glass as the substrate, so a layer of Cr x O y film layer, thereby suppressing the Na + Penetrate into the light shielding layer. The first process gas formula is: the volume ratio of argon to oxygen is 5:1, the pumping rate in the process chamber is 12000L / s, the flow rate of argon is 300sccm, the flow rate of oxygen is 60sccm, the process pressure is 0.25Pa, and the final Cr x O y Its composition x:y is 2:3, and contains Cr x O y N z ingredients.
[0047] The second process gas formula is: the volume ratio of argon to nitrogen is 3:1.2, the pumping rate in the process chamber is 15000L / s, the flow rate of argon is 300sccm, the flow rate of nitrogen is 120sccm, the process pressure is 0.2Pa, and the final Cr x N y The composition of x:y is controlled at 1:1, and contains Cr x O y ingredients.
[0048] The third process gas formula is: the volume ratio of argon, nitrogen and carbon dioxide is 4:1.4:0.3, the pumping rate in the process chamber is 12000L / s, the flow rate of argon is 400sccm, the flow rate of nitrogen is 140sccm, the flow rate of carbon dioxide is 30sccm, the process pressure is 0.24Pa, and the final Cr x O y N z The composition is controlled at x:y:z of 1:3:1, and contains Crx N y The light transmittance of the whole film is 0.15%~0.2%@450nm, and the reflectivity is 12~13%@436nm.
[0049] Comparative Example 2 exist Figure 2 The conventional horizontal vacuum coating system 200 shown in the figure is used for coating, the substrate used for coating is a quartz glass substrate, the first target material 210 and the second target material 211 in the process chamber are chromium flat targets, and the purity of the target material is 99.95%. The coating method includes the following steps: (1) The cleaned substrate is transported by a robot and placed in the loading and unloading chamber 101, the first valve 212 is opened, the substrate is transferred from the loading and unloading chamber 101 to the low vacuum chamber 202, and the first valve 212 is closed; (2) The low vacuum chamber 202 is roughly pumped by the rough pump group, and the atmospheric state of the low vacuum chamber 202 is pumped to the starting range of the molecular pump; (3) The second valve 213 is opened, the substrate is transferred from the low vacuum chamber 202 to the first high vacuum chamber 203, and the second valve 213 is closed; (4) The substrate is sequentially transferred from the first high vacuum chamber 203 to the process chamber 204, the second high vacuum chamber 205, and stops at the heating chamber 206. The substrate is baked and the baking time is set to 600 to 900 seconds. The baking time is determined according to the thickness of the substrate. (5) After the baking time is reached, Cr x N y The first process gas formula for film formation is introduced, and the sputtering power of the first target 210 and the second target 211 is turned on at the same time. The substrate is reversely driven to pass through the first target 210 and the second target 211 in turn, and then goes out of the sputtering area of the second target 211 to reach the first high vacuum chamber 203, completing the Cr x N y Coating, turn off the sputtering power of the first target 210 and the second target 211, turn off the Cr x N y Process gas formulation for coating atmosphere; (6) Cr x O y N z The second process gas formula for film formation is introduced, and the sputtering power of the first target 210 and the second target 211 is turned on at the same time. The substrate is driven forward and passes through the second target 211 and the first target 210 in sequence, and then goes out of the sputtering area of the first target 210 to reach the second high vacuum chamber 205, completing the Cr x O y N z The coating is stopped, the sputtering power of the first target 210 and the second target 211 is turned off, and the Cr x O yN z Coating atmosphere, according to the set Cr x O y N z Stabilize the film for 1.5 to 3 minutes; (7) After the film stabilization time is reached, the second valve 213 is opened, the substrate is reversely driven from the second high vacuum chamber 205 to the low vacuum chamber 202 and stops, and the second valve 213 is closed; (8) Stop exhausting the low vacuum chamber 202, and open the air-breaking valve to break the vacuum in the low vacuum chamber 202 to the atmospheric equilibrium point; (9) After the atmosphere confirmation meter confirms that the low vacuum chamber 202 has reached the atmospheric pressure, the first valve 212 is opened, and the substrate is transferred from the low vacuum chamber 202 to the loading and unloading chamber 101 and stops. The robot then carries and unloads the mask substrate that has completed the coating.
[0050] The first-layer process gas formula is: the volume ratio of argon to nitrogen is 3:1, the pumping rate in the process chamber is 15000L / s, the flow rate of argon is 300sccm, the flow rate of nitrogen is 100sccm, the process pressure is 0.2Pa, and the final Cr x N y The composition x:y is shown to be 1:1.
[0051] The second process gas formula is: the volume ratio of argon, nitrogen and carbon dioxide is 3.5:1:0.3, the pumping rate in the process chamber is 12000L / s, the flow rate of argon is 350sccm, the flow rate of nitrogen is 100sccm, the flow rate of carbon dioxide is 30sccm, the process pressure is 0.24Pa, and the final Cr x O y N z The composition is controlled at x:y:z of 1:3:1, and contains Cr x N y The overall transmittance is 0.15% to 0.2% @ 450nm, and the reflectivity is 12 to 13% @ 436nm.
[0052] Results and analysis: The dust particle conditions during the coating process of Application Example 1, Comparative Example 1 and Comparative Example 2 and the coating quality of each film layer are shown in Table 1 and Table 2 respectively: Table 1 Particle situation
[0053] Table 2 Coating quality of the film
[0054] (1) The first layer of film Cr in Comparative Example 1 x Oy There is residual Cr x O y N z (After the previous substrate coating was completed, Cr remained on the target x O y N z )、The second film Cr x N y Residual Cr x O y 、The third layer of film Cr x O y N z There is residual Cr x N y This is mainly because the first target material 210 and the second target material 211 jointly participate in the deposition of each film layer. Therefore, when coating the next film layer, the components of the previous film layer will remain, which will eventually affect the purity of each film layer. In the coating method of the present application, a single cathode coating is specified for each single-layer film to avoid the problem of impure film layer purity.
[0055] (2) In comparative example 1, the first gas distribution pipe 207 and the second gas distribution pipe 208 are respectively arranged on both sides of the respective targets, which will cause the cathode gas distribution device to be overflow-plated and eventually the particles to rise.
[0056] (3) In comparative example 1, the horizontal vacuum coating system further includes a second high vacuum chamber 205, and the coating path appears to be longer and the particles are worse.
[0057] (4) The three-layer coating process is adopted in Comparative Example 1 mainly because the existing horizontal vacuum coating system is at the low-to-medium-end requirement level of the mask plate in terms of particle control. Therefore, considering the cost, the mask substrate generally adopts a soda glass substrate; while the coating equipment and vacuum coating method of the present application meet the requirements of high-end mask plates in terms of particle and coating quality control. Therefore, a quartz glass substrate is adopted, and the film layer process is changed from the original 3 layers to 2 layers, reducing the complexity of the process.
[0058] (5) In comparative example 2, the existing horizontal vacuum coating system is used to coat the quartz glass substrate, but the quality control of particles and coating cannot meet the requirements of high-end mask plates. However, the coating system and coating process of the present application can well control the quality of particles and coating, thereby producing high-quality mask plates.
[0059] To sum up, the present application uses the first target material to deposit the first film layer and the second target material to deposit the second film layer independently in the same process chamber at different coating stages, which can effectively avoid introducing impurities into each film layer, which is beneficial to improving the purity of each film layer, thereby ensuring the quality of the coated workpiece.
[0060] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the present application. It should be noted that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A vacuum coating method, characterized in that: The coating operation is performed in the same process chamber, wherein the process chamber is provided with a conveying component, a first target material and a second target material, and a first sputtering coating area and a second sputtering coating area respectively provided corresponding to the first target material and the second target material, and the vacuum coating method comprises the following steps: A first process gas is introduced into the process chamber and the first target material is started. The workpiece to be plated is transported by the conveying assembly to the first sputtering coating area for the first sputtering coating. When the workpiece is moved out of the first sputtering coating area, the first film layer is deposited, and the ventilation and the operation of the first target material are stopped. A second process gas is introduced into the process chamber and the second target is started. The workpiece to be plated is transported by the conveying assembly to the second sputtering coating area for a second sputtering coating. When the workpiece is moved out of the second sputtering coating area, the second film layer is deposited, and the ventilation and the operation of the second target are stopped. During the process of introducing process gas into the process chamber, the process chamber is evacuated to maintain a stable internal pressure; The first process gas and the second process gas are different process gases.
2. The vacuum coating method according to claim 1, characterized in that: The first sputtering coating area and the second sputtering coating area are spaced apart in the conveying direction of the workpiece to be plated, and the first process gas and the second process gas are both introduced into the process chamber from the spaced area.
3. The vacuum coating method according to claim 1, characterized in that: The first process gas is blown toward the first target material or perpendicular to the traveling direction of the workpiece to be plated; The second process gas is blown toward the second target material or perpendicular to the moving direction of the workpiece to be plated.
4. The vacuum coating method according to claim 1, characterized in that: The first target and the second target are both selected from one of a chromium target, a molybdenum target, and a silicon target.
5. The vacuum coating method according to claim 1, characterized in that: The first process gas is a mixed gas of nitrogen and argon, and the second process gas is a mixed gas of argon, nitrogen and carbon dioxide.
6. The vacuum coating method according to claim 1, characterized in that: The workpiece to be plated is preheated in the heating chamber and then sent into the process chamber for the first coating. The heating chamber is arranged adjacent to the process chamber.
7. The vacuum coating method according to claim 6, characterized in that: include: The workpiece to be plated enters the heating chamber along a first moving direction to undergo the heating treatment; After completing the heating treatment, entering the process chamber along the second moving direction to perform the first sputtering coating; After completing the first sputtering coating, exit the process chamber, and then enter the process chamber along the first moving direction to perform the second coating; After completing the second sputtering coating, exit the process chamber; The first traveling direction and the second traveling direction are opposite.
8. The vacuum coating method according to claim 7, characterized in that: The workpiece to be plated passes through the vacuum transition chamber and the process chamber in sequence along a first direction and then enters the heating chamber. The vacuum transition chamber and the heating chamber are adjacent to two sides of the process chamber respectively.
9. The vacuum coating method according to claim 8, characterized in that: After the first sputtering coating is completed, the workpiece to be plated exits the process chamber and enters the vacuum transition chamber, and after the second process gas and the second target material are ready, the workpiece to be plated returns to the process chamber along the first moving direction for the second sputtering coating; After the second sputtering coating is completed, the process chamber is withdrawn from the process chamber to the vacuum transition chamber along the second moving direction.
10. The vacuum coating method according to claim 6, characterized in that: include: The workpiece to be plated enters the heating chamber along a first moving direction to undergo the heating treatment; After completing the heating treatment, entering the process chamber along the second moving direction to sequentially perform the first sputtering coating and the second sputtering coating, and exiting from the process chamber after completion; The first traveling direction and the second traveling direction are opposite.
Citation Information
Patent Citations
Manufacturing method and equipment of mask substrate
CN113005410A
Ternary composite comprising rhodanine derivative and Organic photovoltaic device containing the same