Tray and preparation method and application thereof

By using vacuum trays in the ALD cavity to protect the non-coated surface, the problem that ALD coating technology cannot achieve selective coating is solved, and the single-sided or double-sided coating effect is achieved with simple operation and widely applicable, and the non-coated surface is protected without damage. Coated surface.

CN118880283APending Publication Date: 2024-11-01CHINA BUILDING MATERIALS ACADEMY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937356.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-01

Smart Images

  • Figure CN118880283A_ABST
    Figure CN118880283A_ABST
Patent Text Reader

Abstract

The invention relates to a tray and a preparation method and application thereof. The method comprises the following steps: (1) through holes are formed in the upper surface, the lower surface and the side edge of a hollow cylinder; 2) arranging a sealing ring on the outer edge of the hollow cylinder obtained in the step 1); (3) a groove is formed in a disc corresponding to the shape of the hollow cylinder, and then a product to be coated is placed in the groove; and (4) assembling the hollow cylinder obtained in the step (2) and the tray obtained in the step (3) into a tray, vacuumizing the tray through a through hole in the side edge of the hollow cylinder, and then placing the tray in an ALD cavity for coating. The technical problem to be solved is that a tray with a vacuum interior is adopted in an ALD furnace to protect a surface which does not need to be coated, so that single-surface coating is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor coating, and in particular relates to a tray for realizing single-sided coating or double-sided coating in an ALD chamber, and a preparation method and application thereof. Background Art

[0002] ALD atomic layer deposition technology began in the 1970s. It has good self-limiting surface reactions, uniform and controllable thickness, and can complete reactions on complex surfaces. It is more uniform and stable than chemical vapor deposition and physical vapor deposition. ALD coating can be used in many fields such as micro-nano structure processing, catalysis, photovoltaics, and batteries. It is commonly used for coating on silicon dioxide, but the ALD coating technology will coat all surfaces of the object in the cavity, and selective coating cannot be achieved, which has an adverse effect on the subsequent processing of the product. Therefore, in order to prevent it from coating all surfaces of the product, a common method is to stick high-temperature resistant tape on the surface that does not need to be coated, but the tape needs to be peeled off after it comes out of the oven, which makes the operation more cumbersome and complicated. Summary of the invention

[0003] In view of this, the main purpose of the present invention is to provide a tray for achieving single-sided or double-sided coating in an ALD chamber, and a preparation method and application thereof. The technical problem to be solved is to achieve single-sided coating by using an internal vacuum tray in the ALD chamber to protect the surface that does not need to be coated.

[0004] The purpose of the present invention and the technical problem to be solved are achieved by adopting the following technical solutions. A method for preparing a pallet according to the present invention comprises the following steps:

[0005] 1) Open holes on the upper and lower surfaces and sides of the hollow cylinder;

[0006] 2) setting a sealing ring on the outer edge of the hollow cylinder obtained in step 1);

[0007] 3) A groove is made on the disk corresponding to the shape of the hollow cylinder, and then the product to be coated is placed in the groove;

[0008] 4) Assembling the hollow cylinder obtained in step 2) and the disk obtained in step 3) into a tray, and evacuating the tray into a vacuum state through the through hole on the side of the hollow cylinder, and then placing the tray in an ALD chamber for coating.

[0009] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0010] Preferably, in the aforementioned method for preparing the tray, in step 1), the hollow cylinder is selected from one of a cylinder, an elliptical cylinder, a square cylinder, a hexagonal cylinder and an octagonal cylinder; the material of the hollow cylinder is selected from one of glass, quartz, stainless steel, aluminum alloy and magnesium alloy.

[0011] Preferably, in the aforementioned method for preparing a pallet, in step 1), the height of the hollow cylinder is 10 mm to 50 mm, and the diameter is 100 mm to 300 mm.

[0012] Preferably, in the aforementioned method for preparing a tray, in step 1), the diameter of the through holes on the upper and lower surfaces and the side of the hollow cylinder is 0.5 mm to 10 mm.

[0013] Preferably, in the aforementioned method for preparing a pallet, in step 1), after three height-adjustable hooks are welded at the outer edges of the upper and lower surfaces of the hollow cylinder, holes are opened in the upper and lower surfaces and sides of the hollow cylinder.

[0014] Preferably, in the aforementioned method for preparing a pallet, in step 1), the processing method of the return hook is one of precision carving and welding.

[0015] Preferably, in the aforementioned method for preparing a tray, in step 2), a groove with a depth of 5 mm is formed on the outer edge of the hollow cylinder obtained in step 1), and a sealing ring is disposed in the groove.

[0016] Preferably, in the aforementioned method for preparing a pallet, in step 2), the material of the sealing ring is selected from one of rubber, silicone and polyurethane.

[0017] Preferably, in the aforementioned method for preparing a tray, in step 3), the material of the tray is selected from one of glass, quartz, stainless steel, aluminum alloy and magnesium alloy.

[0018] Preferably, in the aforementioned method for preparing a tray, in step 3), the thickness of the tray is 2 mm to 50 mm, and the diameter is 95 mm to 295 mm.

[0019] Preferably, in the aforementioned method for preparing a tray, in step 3), the diameter of the groove on the tray is 14 mm to 245 mm, and the depth of the groove is 0.5 mm to 30 mm.

[0020] Preferably, in the aforementioned method for preparing a pallet, in step 3), the diameter or side length of the product to be coated is 15 mm to 250 mm, and the thickness is 0.5 mm to 30 mm.

[0021] Preferably, in the aforementioned method for preparing a tray, in step 3), the product to be coated is selected from one of a silicon wafer, a metal sheet, a wafer and a glass sheet.

[0022] Preferably, in the aforementioned method for preparing a tray, in step 3), the shape of the product to be coated is selected from one of circular, oval, square and diamond.

[0023] Preferably, in the aforementioned method for preparing a tray, in step 4), the hollow cylinder obtained in step 2) and the upper and lower trays obtained in step 3) are assembled and fixed by means of parent-child hooks.

[0024] Preferably, in the aforementioned method for preparing a tray, in step 4), the vacuum degree of the tray is 250Pa to 400MPa.

[0025] Preferably, in the aforementioned method for preparing a tray, in step 4), the film layer material of the coating is selected from one of SiO2, Al2O3, TiO2, Ta2O5 and HfO2.

[0026] Preferably, in the aforementioned method for preparing the tray, in step 4), the upper tray or the upper and lower trays of the tray are placed in an ALD chamber for coating.

[0027] The purpose of the present invention and the technical problems solved by the present invention are also achieved by the following technical solutions. According to a tray proposed by the present invention, it includes a hollow cylinder and two upper and lower plates connected to the hollow cylinder, a sealing ring is arranged on the outer edge of the hollow cylinder, and a groove is provided on the plate; through holes are provided on the upper and lower surfaces and the side of the hollow cylinder.

[0028] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0029] Preferably, in the aforementioned tray, a groove with a depth of 5 mm is formed on the outer edge of the hollow cylinder, and the sealing ring is arranged in the groove; and a return hook with adjustable height is provided on the outer edge of the hollow cylinder.

[0030] Preferably, in the aforementioned pallet, the height of the hollow cylinder is 10 mm to 50 mm, and the diameter is 100 mm to 300 mm.

[0031] Preferably, in the aforementioned tray, the diameter of the through holes on the upper and lower surfaces and the side of the hollow cylinder is 0.5 mm to 10 mm.

[0032] Preferably, in the aforementioned tray, the thickness of the plate is 2 mm to 50 mm, and the diameter is 95 mm to 295 mm.

[0033] Preferably, in the aforementioned tray, the hollow cylinder is assembled and fixed to the upper and lower trays by means of parent-child hooks.

[0034] The purpose of the present invention and the technical problem solved by the present invention are also achieved by adopting the following technical solutions. A method for single-sided coating in an ALD chamber proposed by the present invention comprises the following steps:

[0035] The product to be coated is placed in the groove of one of the trays, and the tray is evacuated into a vacuum state through the through holes on the side of the hollow cylinder of the tray, and then the tray is placed in the ALD chamber for coating.

[0036] The purpose of the present invention and the technical problem solved by the present invention are also achieved by adopting the following technical solutions. A method for double-sided coating in an ALD chamber proposed by the present invention comprises the following steps:

[0037] The product to be coated is placed in the groove of one of the trays, and then the tray is placed in the ALD chamber for coating.

[0038] By means of the above technical solution, a pallet and a preparation method and application thereof proposed by the present invention have at least the following advantages:

[0039] The tray of the present invention can realize single-sided or double-sided coating of the product; the method has uniform coating, simple operation, and is applicable to a wide range of products, and can improve the space utilization rate of the ALD chamber, and does not contact the non-coated surface, thereby protecting the non-coated surface to a great extent and not affecting the subsequent processing of the non-coated surface product;

[0040] The present invention can realize selective coating in the ALD furnace by using vacuum as a protective means, and does not contact the non-coated surface, can realize single-sided coating or double-sided coating, and does not damage the coated surface and the non-coated surface.

[0041] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 This is one of the schematic diagrams of the tray structure in the ALD chamber of the present invention that can achieve internal vacuum for single-sided coating;

[0043] Figure 2 The second schematic diagram of the tray structure capable of achieving internal vacuum for single-sided coating in the ALD chamber of the present invention;

[0044] Figure 3 This is the third schematic diagram of the tray structure in the ALD chamber of the present invention that can achieve internal vacuum for single-sided coating.

[0045] Among them, 1, upper plate; 1', lower plate; 2, hollow cylinder; 3, groove; 4, return hook mother part; 5, return hook part; 6, through hole; 7, sealing ring; 8, through hole. DETAILED DESCRIPTION

[0046] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose of the invention, the following is a detailed description of a pallet and its preparation method and application proposed according to the present invention, its specific implementation method, structure, characteristics and effects, in combination with the accompanying drawings and preferred embodiments.

[0047] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the usual meanings understood by ordinary technicians in the field to which the present invention belongs. If no specific experimental steps or conditions are specified below, the operations or conditions of the conventional experimental steps described in the literature in the field can be followed.

[0048] Some embodiments of the present invention provide a method for preparing a tray, comprising the following steps:

[0049] 1) Weld three height-adjustable hooks at the outer edges of the upper and lower surfaces of the hollow cylinder 2; then open holes 6 and 8 on the upper and lower surfaces and the side of the hollow cylinder 2; the processing method of the hooks is a kind of precision carving or welding; this setting is to ensure that the hollow cylinder and the disk are tightly combined before vacuuming;

[0050] 2) A groove with a depth of 5 mm is formed on the outer edge of the hollow cylinder 2 obtained in step 1), and a sealing ring 7 is arranged in the groove;

[0051] 3) A groove 3 is formed on a plate corresponding to the shape of the hollow cylinder 2, and then the product to be coated is placed in the groove 3;

[0052] 4) Assemble the hollow cylinder 2 obtained in step 2) and the plate obtained in step 3) into a tray through the parent-child hooks, as shown in FIG. Figure 1-Figure 3 As shown, the tray is evacuated into a vacuum state through the through hole on the side of the hollow cylinder 2, and then the tray is placed in the ALD chamber for coating; because the reaction pressure of the ALD chamber is between 90Pa and 110Pa, after repeatedly measuring the thickness of the film layer on the non-coated surface under different pressures in the tray, it is found that when the pressure in the tray is between 250Pa and 400Pa, the thickness of the film layer on the non-coated surface is zero. This proves that the tray plays a role in protecting the non-coated surface. Therefore, after the hollow cylinder and its corresponding disk are assembled into a tray, and the vacuum degree is evacuated to between 250Pa and 400Pa from the through hole 8 on the side of the cylinder, the tray can be placed in the ALD chamber for coating.

[0053] During specific implementation, in step 1), according to the shape and size of the desired coated product, the hollow cylinder can be selected from one of a cylinder, an elliptical cylinder, a square cylinder, a hexagonal cylinder and an octagonal cylinder.

[0054] Taking into account the sealing performance of the tray and the high temperature resistance and deformation resistance required in the ALD chamber, in the above technical solution, the hollow cylinder and the disk can be made of one of glass, quartz, stainless steel, aluminum alloy and magnesium alloy, with a processing accuracy of ±0.01mm.

[0055] Optionally, since the diameter of the ALD chamber space is 150mm to 400mm and the depth is 20mm to 60mm, the size of the tray should be slightly smaller than the chamber. Therefore, in step 1), the height of the hollow cylinder 2 can be designed to be 10mm to 50mm. If the height of the hollow cylinder 2 is lower than 10mm, it is not convenient to place the film to be plated and assemble the hollow cylinder. If the height of the hollow cylinder 2 is higher than 50mm, it is not convenient to take the tray out of the ALD chamber. The diameter of the hollow cylinder 2 can be designed to be 100mm~300mm. If the diameter of the hollow cylinder 2 is less than 100mm, the number of film sheets to be plated that can be placed is small, which is not convenient for batch coating. If the diameter of the hollow cylinder 2 is greater than 300nm, the distance between it and the ALD chamber is too small, which makes it easy for the film sheets to be plated at the outer diameter edge of the tray to be unevenly plated. The thickness of the product to be plated is approximately between 0.5mm and 30mm. The thickness of the tray should be greater than the thickness of the product to be plated to play a protective role. Therefore, the thickness of the tray can be designed to be 2mm~50mm. If the thickness of the tray is less than 2mm, the tray is prone to deformation during vacuum extraction. If the thickness of the tray is greater than 50mm, the height of the ALD chamber will exceed the height of the ALD chamber, and the chamber cannot be closed. Since the diameter of the hollow cylinder 2 is designed to be 100 mm-300 mm, and the width of the raised hook member 5 on the disk is 5 mm, in order to achieve the matching size of the disk and the hollow cylinder 2, the diameter of the disk should be designed to be 95 mm-295 mm.

[0056] Optionally, in step 1), since the diameter of the vacuum pipe of the vacuum system is 0.5-10 mm, in order to match the vacuum system, the aperture of the through hole 8 on the side of the hollow cylinder 2 is designed to be 0.5-10 mm. And the aperture of the through hole 6 on the upper and lower surfaces of the hollow cylinder 2 is designed to be 0.5-10 mm. If it is less than 0.5 mm, it is not convenient to process the through hole, and if it is greater than 10 mm, it is easy to leak during vacuuming.

[0057] Optionally, in step 2), in order to ensure the sealing of the tray, the vacuum degree of the hollow cylinder is measured and it is found that when the material of the sealing ring is one of rubber, silicone and polyurethane, it meets the required vacuum standard.

[0058] Optionally, in step 3), since the diameter of the product to be coated is generally between 15 mm and 250 mm, the aperture of the groove on the disk should be slightly smaller than the product to be coated, so that the outer edge of the product to be coated is in close contact with the disk after vacuuming. For a product to be coated with a diameter of 15 mm, if the aperture of the groove on the disk is less than 14 mm, the contact between the product to be coated and the disk is too large, which may easily cause defects such as scratches and contamination to its effective area. For a product to be coated with a diameter of 250 mm, if the aperture of the groove on the disk is greater than 245 mm, it is easy to be poorly sealed, causing air leakage, affecting the protective effect of the non-coated surface. Therefore, the aperture of the groove on the disk is designed to be 14 mm to 245 mm. Since the thickness of the product to be coated is between 0.5 mm and 30 mm, the depth of the groove on the disk is designed to be 0.5 mm to 30 mm.

[0059] Optionally, in step 3), the size of the product to be coated should be smaller than the diameter of the disc, so the diameter or side length of the product to be coated is 15 mm to 250 mm, and the thickness is 0.3 mm to 10 mm.

[0060] Optionally, in step 3), since the reaction pressure of the ALD chamber is between 90Pa and 110Pa, after repeatedly measuring the thickness of the non-coated surface film layer under different pressures in the tray, it is found that when the pressure in the tray is between 250Pa and 400Pa, the thickness of the film layer on the non-coated surface is zero. This shows that the hollow cylinder 2 plays a role in protecting the non-coated surface, so the vacuum degree of the hollow cylinder 2 can be designed to be 250Pa to 400Pa.

[0061] Optionally, in step 3), the material of the product to be coated can be silicon wafer, metal, wafer, glass sheet and other materials, but is not limited to these.

[0062] Optionally, in step 3), the shape of the product to be coated can be one of round, oval, square and diamond, but is not limited to these. However, most of the coated products of semiconductors are round and square.

[0063] Optionally, in step 4), the vacuum degree of the tray is 250Pa to 400MPa.

[0064] Optionally, in step 4), the film material needs to be individually designed according to the required refractive index, reflectivity, transmittance and other parameters, and the film material can be one of SiO2, Al2O3, TiO2, Ta2O5 and HfO2, but is not limited to these.

[0065] Optionally, in step 4), the upper plate or the upper and lower plates of the tray are placed in the ALD chamber for coating. Depending on the number of products to be coated, the tray can be assembled in a changeable manner. When there are fewer products to be coated, the coating tray may only have holes in the upper plate. When there are more products to be coated, the coating tray may also have holes in both the upper and lower plates.

[0066] like Figure 1-Figure 3 As shown, some embodiments of the present invention further provide a tray, which includes a hollow cylinder 2 and an upper plate 1 and a lower plate 1' connected to the hollow cylinder 2, a sealing ring 7 is provided on the outer edge of the hollow cylinder 2, and a groove 3 is provided on the upper plate 1 and the lower plate 1'; through holes 6 and 8 are respectively provided on the upper and lower surfaces and the side of the hollow cylinder 2.

[0067] Optionally, a groove with a depth of 5 mm is formed on the outer edge of the hollow cylinder 2, and the sealing ring 7 is arranged in the groove; a return hook with adjustable height is provided on the outer edge of the hollow cylinder 2. The return hook includes a return hook mother part 4 and a return hook sub-part 5 matched with the return hook mother part 4.

[0068] Optionally, the height of the hollow cylinder 2 is 10-50 mm, and the diameter is 100-300 mm.

[0069] Optionally, the diameters of the through holes 6 on the upper and lower surfaces of the hollow cylinder 2 and the through holes 8 on the side are 0.5 to 10 mm.

[0070] Optionally, the thickness of the disk is 2 to 50 mm, and the diameter is 95 to 295 mm. Since the thickness of the product to be coated is approximately between 0.5 mm and 30 mm, the thickness of the disk should be greater than the thickness of the product to be coated to play a protective role. Therefore, the thickness of the disk can be designed to be 2 mm to 50 mm. If the thickness of the tray is less than 2 mm, the tray is prone to deformation during vacuuming. If the thickness of the tray is greater than 50 mm, the height of the hollow cylinder 2 exceeds the height of the ALD chamber, and the chamber cannot be closed. Since the diameter of the hollow cylinder 2 is designed to be 100-300 mm, the width of the raised hook 5 on the disk is 5 mm, so in order to achieve the matching size of the disk and the hollow cylinder 2, the diameter of the disk should be designed to be 95 to 295 mm.

[0071] Optionally, the hollow cylinder 2 and the upper and lower plates are assembled and fixed by a return hook mother component 4 and a return hook son component 5. The return hook mother component 4 and the return hook son component 5 can constitute a return hook.

[0072] Some embodiments of the present invention further provide a method for single-sided coating in an ALD chamber, comprising the following steps:

[0073] The product to be coated is placed in the groove of one of the trays, and the tray is evacuated into a vacuum state through the through hole 8 on the side of the hollow cylinder 2 of the tray, and then the tray is placed in the ALD chamber for coating. The vacuum degree of the tray can be 250Pa to 400MPa.

[0074] Some embodiments of the present invention further provide a method for double-sided coating in an ALD chamber, characterized in that it comprises the following steps:

[0075] The product to be coated is placed in the groove of one of the trays, and then the tray is placed in the ALD chamber for coating.

[0076] The present invention is further described below in conjunction with more specific embodiments.

[0077] Example 1

[0078] This embodiment provides a method for preparing a tray, comprising the following steps:

[0079] S1, fix a 304 rectangular steel block with a length and width of 250 mm and a height of 22 mm with a three-jaw centering chuck, and process it into a cylinder with a diameter of 200 mm and a height of 20 mm by lathe, the lathe processing speed is 1200 r / min, and the processing tolerance is ±0.01 mm; weld three height-adjustable return hooks on the outer edges of the upper and lower surfaces of the cylinder;

[0080] S2, through holes with a diameter of 5 mm are processed on the upper and lower surfaces and the side of the cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 3 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the side through hole is half of the diameter; the center of the cylinder is the through hole;

[0081] S3, a groove with a depth of 5 mm is cut on the outer edge of the cylinder by a precision engraving machine, the diameter of the milling cutter is 3 mm, the rotation speed is 8000 r / min, the feed speed is 300 r / min, and a silicone sealing ring is placed in the groove;

[0082] S4, cut two discs made of 304 steel, with a diameter of 195 mm and a thickness of 3 mm using a lathe. The lathe processing speed is 1200 r / min and the processing tolerance is ±0.01 mm;

[0083] S5, 25 grooves with an inner diameter of 25mm, an outer diameter of 26mm and a depth of 0.5mm are cut on the upper and lower discs with a precision engraving machine. The diameter of the milling cutter is 10mm, the rotation speed is 15000r / min, the feed speed is 600r / min, the spiral cutter is lowered, the safety height is set to 3mm, the minimum slope length is 30% of the length of the tool (i.e., the precision engraving machine cutter head), and the slope angle is 15°;

[0084] S6, placing a silicon wafer to be coated on one side with a diameter of 26 mm in the groove with a hole on the disc, with the surface to be coated of the upper disc facing upward and the surface to be coated of the lower disc facing downward;

[0085] S7, assemble and fix the upper and lower disks and the cylinder through the mother-and-child hooks, pump the internal pressure of the two disks and the cylinder to 250Pa through the through holes on the side of the cylinder, and close the exhaust hole; put the tray into the ALD equipment chamber, and plan to plate the silicon wafer to be coated to 300nm; after the tray is taken out of the ALD equipment, it is found that the coated surface and the non-coated surface are not damaged. The thickness of the non-coated surface film layer is tested with an F50 thin film thickness gauge, and the thickness of the coated surface film layer is measured to be 302nm, and the thickness of the non-coated surface film layer is 0nm. This shows that the inside of the vacuum tray plays a role in protecting the non-coated surface, and its device is as follows Figure 1-Figure 3 shown.

[0086] Comparative Example 1

[0087] This embodiment provides a method for preparing a tray, comprising the following steps:

[0088] S1, fix a 304 steel block with a length and width of 250 mm and a height of 22 mm with a three-jaw centering chuck, and process it into a cylinder with a diameter of 200 mm and a height of 20 mm by lathe. The lathe processing speed is 1200 r / min, and the processing tolerance is ±0.01 mm; weld three height-adjustable return hooks on the outer edges of the upper and lower surfaces of the cylinder;

[0089] S2, small holes with a diameter of 5 mm are processed on the upper and lower surfaces and the side of the cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 3 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the small hole on the side is half of the diameter; the center of the cylinder is the through hole;

[0090] S3, use a precision engraving machine to carve a groove with a depth of 5 mm on the outer edge of the cylinder, the operating parameters are as above, and place a silicone sealing ring in the groove;

[0091] S4, cut two discs made of 304 steel using a lathe, with the operating parameters as above, with a diameter of 195 mm and a thickness of 3 mm;

[0092] S5, 25 grooves with an inner diameter of 25mm, an outer diameter of 26mm and a depth of 0.5mm are cut on the upper and lower discs with a precision engraving machine. The diameter of the milling cutter is 10mm, the rotation speed is 15000r / min, the feed speed is 600r / min, the spiral cutter is lowered, the safety height is set to 3mm, the minimum slope length is 30% of the tool (i.e., the precision engraving machine cutter head), and the slope angle is 15°;

[0093] S6, placing a silicon wafer to be coated on one side with a diameter of 26 mm in the groove with a hole on the disc, with the surface to be coated of the upper disc facing upward and the surface to be coated of the lower disc facing downward;

[0094] S7, assemble and fix the upper and lower disks and the cylinder through the mother-and-child hooks, pump the pressure inside the two disks and the cylinder to 100Pa through the through hole on the side of the cylinder, and close the exhaust hole; put the tray into the ALD equipment chamber, plate the silicon wafer to be coated to 300nm; after the tray is taken out of the ALD equipment, use the F50 film thickness meter to test the thickness of the non-coated surface film layer, and measure the film thickness of the coated surface to be 303nm, and the film thickness of the non-coated surface to be 245nm. This shows that when the pressure inside the tray is equivalent to the pressure of the ALD chamber, the vacuum tray is found inside the vacuum tray to play a role in protecting the non-coated surface.

[0095] Example 2

[0096] This embodiment provides a method for preparing a tray, comprising the following steps:

[0097] S1, a quartz cuboid with a length and width of 202 mm and a height of 30.5 mm is processed into a square column with a length and width of 200 mm and a height of 30 mm by precision carving, and the processing tolerance is ±0.01 mm; a height-adjustable hook is welded on each of the four sides of the upper and lower surfaces of the square column;

[0098] S2, a small hole with a diameter of 10 mm is processed on the upper and lower surfaces and the side of the square cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 5 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the small hole on the side is half of the diameter; the center of the square cylinder is a through hole;

[0099] S3, make a groove with a depth of 3mm on the outer edge of the cube, and place a silicone sealing ring in the groove;

[0100] S4, precision engraving two square pallets made of quartz, 300mm in length and width, 5mm in thickness, with a milling cutter diameter of 5mm, a rotation speed of 8000r / min, and a feed speed of 300r / min;

[0101] S5, 10 grooves with an inner diameter of 50mm, an outer diameter of 52mm and a depth of 1mm were opened on one of the pallets. The diameter of the milling cutter was 10mm, the rotation speed was 18000r / min, the feed speed was 500r / min, the cutting was spiral, the safety height was set to 2mm, the minimum slope length was 30% of the tool (i.e., the engraving machine cutter head), and the slope angle was 10°;

[0102] S6, placing a glass disc with a diameter of 52 mm and a thickness of 1.2 mm in the hole, with the surface to be coated on the upper tray facing upward, and the lower tray has no opening and does not place the disc to be coated;

[0103] S7, assemble and fix the upper and lower trays and the square cylinder through the mother-and-child hooks, and pump the pressure inside the two trays and the square cylinder to 350Pa through the through holes on the side of the cube, and close the exhaust hole; put the assembled square tray and square cylinder into the ALD equipment chamber, and plate the glass sheet to be coated to 500nm; after the tray is taken out of the ALD equipment, it is found that the coated surface and the non-coated surface are not damaged. The film thickness of the non-coated surface is tested with an F50 thin film thickness gauge, and the film thickness of the coated surface is measured to be 492nm, and the film thickness of the non-coated surface is 0nm. This shows that the inside of the vacuum tray plays a role in protecting the non-coated surface.

[0104] Comparative Example 2

[0105] This embodiment provides a method for preparing a tray, comprising the following steps:

[0106] S1, a quartz cuboid with a length and width of 202 mm and a height of 30.5 mm is processed into a square column with a length and width of 200 mm and a height of 30 mm by precision carving, and the processing tolerance is ±0.01 mm; a height-adjustable hook is welded on each of the four sides of the upper and lower surfaces of the square column;

[0107] S2, a small hole with a diameter of 10 mm is processed on the upper and lower surfaces and the side of the square cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 5 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the small hole on the side is half of the diameter; the center of the square cylinder is a through hole;

[0108] S3, precision engraving two square pallets made of quartz, 300mm in length and width, 5mm in thickness, with a milling cutter diameter of 5mm, a rotation speed of 8000r / min, and a feed speed of 300r / min;

[0109] S4, 10 grooves with an inner diameter of 50mm, an outer diameter of 52mm and a depth of 1mm were opened on one of the pallets. The diameter of the milling cutter was 10mm, the rotation speed was 18000r / min, the feed speed was 500r / min, the cutting was spiral, the safety height was set to 2mm, the minimum slope length was 30% of the tool (i.e., the engraving machine cutter head), and the slope angle was 10°;

[0110] S5, placing a glass disc with a diameter of 52 mm and a thickness of 1.2 mm in the hole, with the surface to be coated on the upper tray facing upward, and the lower tray has no opening and does not place the disc to be coated;

[0111] S6, the upper and lower trays and the square cylinder were assembled and fixed by the mother-and-child hooks. The tray was found to be leaking inside during vacuuming, and the required vacuum degree could not be achieved. It was planned to coat the surface of the glass sheet to be coated to 500nm; after the tray was taken out of the ALD equipment, the film thickness of the non-coated surface was tested with an F50 film thickness measuring instrument, and the film thickness of the coated surface was measured to be 505nm, and the film thickness of the non-coated surface was 453nm. This shows that when the tray leaked inside, the tray did not play a role in protecting the non-coated surface.

[0112] Example 3

[0113] This embodiment provides a method for preparing a tray, comprising the following steps:

[0114] S1, a cylinder made of aluminum alloy with a diameter of 300 mm and a height of 30 mm is processed by lathe at a lathe speed of 1200 r / min and a processing tolerance of ±0.01 mm; three height-adjustable hooks are welded on the outer edges of the upper and lower surfaces of the cylinder;

[0115] S2, small holes with a diameter of 10 mm are processed on the upper and lower surfaces and the side of the cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 5 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the small hole on the side is half of the diameter; the center of the cylinder is the through hole;

[0116] S3, make a groove with a depth of 2 mm on the outer edge of the cylinder, and place a polyurethane sealing ring in the groove;

[0117] S4, using a lathe to cut two aluminum alloy discs with a size of 295 mm and a thickness of 5 mm, with a milling cutter diameter of 5 mm, a rotation speed of 8000 r / min, and a feed speed of 300 r / min;

[0118] S5, a square groove with an inner width of 245 mm, an outer width of 250 mm, and a depth of 2 mm is opened on each of the two discs, and a square metal sheet with a width of 250 mm and a thickness of 3 mm is placed in the square groove, with the surface to be coated of the upper disc facing upward and the surface to be coated of the lower disc facing downward;

[0119] S6, assemble the disk and cylinder through the mother-and-child hooks, and pump the internal pressure of the disk and cylinder to 400Pa through the through hole on the side of the cylinder, and close the exhaust hole; put the assembled tray into the ALD equipment chamber, coat the metal sheet, and coat the glass sheet to be coated to 200nm. After the tray was taken out of the furnace, it was found that there was no damage on the coated surface and the non-coated surface; the film thickness of the non-coated surface was tested with an F50 film thickness gauge, and the film thickness of the coated surface was 196nm, and the film thickness of the non-coated surface was 0. This shows that the vacuum tray plays a role in protecting the non-coated surface.

[0120] Comparative Example 3

[0121] This embodiment provides a method for preparing a tray, comprising the following steps:

[0122] S1, a cylinder made of polytetrafluoroethylene with a diameter of 300 mm and a height of 30 mm is processed by lathe. The lathe processing speed is 800 r / min and the processing tolerance is ±0.01 mm;

[0123] S2, through holes with a diameter of 10 mm are processed on the upper and lower surfaces and the side of the cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 5 mm, the rotation speed is 2000 r / min, and the feed speed is 200 r / min; the depth of the small hole on the side is half of the diameter; the center of the cylinder is the through hole;

[0124] S3, make a groove with a depth of 2 mm on the outer edge of the cylinder, and place a polyurethane sealing ring in the groove;

[0125] S4, cut two discs made of polytetrafluoroethylene with a diameter of 295 mm and a thickness of 5 mm using a lathe, with a milling cutter diameter of 5 mm, a rotation speed of 2000 r / min, and a feed speed of 200 r / min;

[0126] S5, a square groove with an inner width of 245 mm, an outer width of 250 mm, and a depth of 2 mm is opened on each of the two discs, and a square metal sheet with a width of 250 mm and a thickness of 3 mm is placed in the square groove, with the surface to be coated of the upper disc facing upward and the surface to be coated of the lower disc facing downward;

[0127] S6, the disc and the cylinder were assembled by the mother-and-child hooks. When the vacuum was drawn, it was found that the tray made of polytetrafluoroethylene was bent and deformed, and the required pressure could not be reached. The surface of the metal sheet to be coated was plated to 200. After the tray was taken out of the ALD equipment, the film thickness of the non-coated surface was tested with an F50 film thickness measuring instrument. The film thickness of the coated surface was 210nm, and the film thickness of the non-coated surface was 191nm. This shows that when the tray material is too soft, the inside of the tray will leak, and the tray does not play a role in protecting the non-coated surface.

[0128] Example 4

[0129] This embodiment provides a method for preparing a tray, comprising the following steps:

[0130] S1, a glass cuboid with a length and width of 300 mm and a height of 40.5 mm is processed into a cylinder with a diameter of 260 mm and a height of 40 mm by precision carving, with a processing tolerance of ±0.01 mm; two height-adjustable hooks are welded on the upper and lower sides of the cylinder;

[0131] S2, small holes with a diameter of 10 mm are processed on the upper and lower surfaces and the side of the cylinder by a three-axis precision engraving machine; the diameter of the milling cutter is 5 mm, the rotation speed is 8000 r / min, and the feed speed is 300 r / min; the depth of the small hole on the side is half of the diameter; the center of the cylinder is the through hole;

[0132] S3, precision engraving two round trays made of glass with a diameter of 255mm and a thickness of 5mm. The milling cutter diameter is 5mm, the speed is 8000r / min, and the feed speed is 300r / min;

[0133] S4, a groove with an inner diameter of 245mm, an outer diameter of 250mm and a depth of 2mm is opened on one of the pallets. The diameter of the milling cutter is 10mm, the speed is 18000r / min, the feed speed is 500r / min, the spiral cutter is used, the safety height is set to 2mm, the minimum slope length is 30% of the tool (i.e., the engraving machine cutter head), and the slope angle is 10°;

[0134] S5, placing a glass disc with a diameter of 250 mm and a thickness of 3 mm in the hole, and coating both sides of the glass disc;

[0135] S6, the upper and lower trays and the square cylinder are assembled and fixed by the mother-and-child hook assembly and placed in the ALD equipment chamber for coating, and the planned coating thickness is 300nm; after the tray is taken out of the ALD equipment, it is found that the coated surface and the non-coated surface are not damaged. The film thickness of the glass disc is tested with an F50 film thickness measuring instrument, and the film thickness on one side is measured to be 303nm, and the film thickness on the other side is 299nm. This shows that the tray can also achieve simultaneous coating on both sides.

[0136] The technical features in the claims and / or the specification of the present invention may be combined, and the combination is not limited to the combination obtained by reference in the claims. The technical solution obtained by combining the technical features in the claims and / or the specification is also within the protection scope of the present invention.

[0137] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a pallet, characterized in that: The following steps are involved: 1) Open holes on the upper and lower surfaces and sides of the hollow cylinder; 2) setting a sealing ring on the outer edge of the hollow cylinder obtained in step 1); 3) A groove is made on the disk corresponding to the shape of the hollow cylinder, and then the product to be coated is placed in the groove; 4) Assembling the hollow cylinder obtained in step 2) and the disk obtained in step 3) into a tray, and evacuating the tray into a vacuum state through the through hole on the side of the hollow cylinder, and then placing the tray in an ALD chamber for coating.

2. The method for preparing a pallet according to claim 1, characterized in that: In step 1), the hollow cylinder is selected from one of a cylinder, an elliptical cylinder, a square cylinder, a hexagonal cylinder and an octagonal cylinder; the material of the hollow cylinder is selected from one of glass, quartz, stainless steel, aluminum alloy and magnesium alloy; the height of the hollow cylinder is 10 to 50 mm, and the diameter is 100 to 300 mm; through holes are opened on the upper and lower surfaces and the side of the hollow cylinder, and the hole diameter is 0.5 to 10 mm; after welding three height-adjustable hooks at the outer edges of the upper and lower surfaces of the hollow cylinder, through holes are opened on the upper and lower surfaces and the side of the hollow cylinder; the processing method of the hook is one of precision carving or welding.

3. The method for preparing a pallet according to claim 1, characterized in that: In step 2), a groove with a depth of 5 mm is formed on the outer edge of the hollow cylinder obtained in step 1), and the sealing ring is arranged in the groove; in step 2), the material of the sealing ring is selected from one of rubber, silicone and polyurethane.

4. The method for preparing a pallet according to claim 1, characterized in that: In step 3), the material of the disk is selected from one of glass, quartz, stainless steel, aluminum alloy and magnesium alloy; the thickness of the disk is 2mm~50mm, and the diameter is 95mm~295mm; the aperture on the disk is 16~260mm, and the depth of the groove is 0.5mm~30mm; the diameter or side length of the product to be coated is 15mm~250mm, and the thickness is 0.5mm~30mm; the product to be coated is selected from one of silicon wafers, metal sheets, wafers and glass sheets; the shape of the product to be coated is selected from one of round, square and diamond.

5. The method for preparing a pallet according to claim 1, characterized in that: In step 4), the hollow cylinder obtained in step 2) and the upper and lower plates obtained in step 3) are assembled and fixed by means of parent-child hooks; the vacuum degree of the tray is -0.9MPa to -0.04MPa; the film layer material of the coating is selected from one of SiO2, Al2O3, TiO2, Ta2O5 and HfO2.

6. A pallet, characterized in that: It comprises a hollow cylinder and upper and lower plates connected to the hollow cylinder. A sealing ring is arranged on the outer edge of the hollow cylinder, and a groove is opened on the plate. Through holes are opened on the upper and lower surfaces and the side of the hollow cylinder.

7. The tray according to claim 6, characterized in that The outer edge of the hollow cylinder is provided with a groove with a depth of 5 mm, and the sealing ring is arranged in the groove; the outer edge of the hollow cylinder is provided with a return hook with adjustable height; the height of the hollow cylinder is 10 mm to 50 mm, and the diameter is 100 mm to 300 mm; the aperture of the through holes on the upper and lower surfaces and the side of the hollow cylinder is 0.5 mm to 10 mm.

8. The tray according to claim 6, characterized in that The thickness of the disk is 2 mm to 50 mm, and the diameter is 95 mm to 295 mm; the hollow cylinder and the upper and lower disks are assembled and fixed by means of parent-child hooks.

9. A method for single-sided coating in an ALD chamber, characterized in that: The following steps are involved: The product to be coated is placed in the groove of one of the trays, and the tray is evacuated into a vacuum state through the through holes on the side of the hollow cylinder of the tray, and then the tray is placed in the ALD chamber for coating.

10. A method for double-sided coating in an ALD chamber, characterized in that: The following steps are involved: The product to be coated is placed in the groove of one of the trays, and then the tray is placed in the ALD chamber for coating.