Composite material with graphene surface plated with silver and copper and preparation method of composite material

By plating silver copper on the surface of graphene, and improving the activity and adsorption of graphene by ultrasonic stirring and electroless plating, the problem of insufficient conductivity and mechanical properties of graphene-based dual alloy composite materials is solved, and high-performance graphite is achieved Ethylene surface coated with silver-copper composite material.

CN118880302APending Publication Date: 2024-11-01JIANGXI JIATAO INORGANIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410941654.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing graphene-based bialloy composite materials have insufficient conductivity and mechanical properties in the fields of catalysis and sensing, making it difficult to meet the needs of high-performance electrochemical sensors.

Method used

The activity and adsorption of graphene are coated with silver copper on the surface of graphene by ultrasonic stirring and electroless plating. The activity and adsorption of graphene are improved by sodium hydroxide, chloroacetic acid, N,N-dimethylethylenediamine and glycine treatment, and chlorination is carried out through chlorination. Iridium promotes the density and conductivity of the plating layer.

Benefits of technology

The conductive and mechanical properties of the silver-copper composite material coated on the surface of graphene are significantly improved, the bonding force with the copper matrix is ​​enhanced, and the application range of the material is broadened.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite material with a graphene surface plated with silver and copper, which comprises the following steps: treating graphene oxide by sodium hydroxide, then treating by chloroacetic acid, partially carboxylating the graphene surface, and subsequently modifying by N, N-dimethylethylenediamine and glycine, so that the adsorbability of the graphene oxide is greatly improved; and finally, performing a plating process to form a silver-copper metal composite layer. The graphene surface silver-plated copper composite material prepared by the method disclosed by the invention is used as a filler, so that the mechanical property and the electrical conductivity of a copper base material can be remarkably improved, the strength of the copper base material is remarkably improved on the basis of keeping high electrical conductivity of copper, and the application range of a copper material is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene composite materials, and in particular to a composite material of graphene surface plated with silver and copper and a preparation method thereof. Background Art

[0002] Graphene is composed of sp2 hybridized carbon atoms, which form a two-dimensional single-layer sheet material with a hexagonal structure. All atoms are located in the same plane. The carbon atoms in the plane are connected by carbon-carbon σ bonds, while the large delocalized π bond system outside the plane makes graphene have good conductivity. At present, graphene has been widely used in the fields of chemistry, electronics, information, energy, materials and biomedicine. So far, graphene has been developed as a nanoscale matrix material for dispersing and stabilizing various metal and metal oxide nanoparticles. Among them, graphene-based dual alloy composites are widely used in the fields of catalysis and sensing. Due to the interaction between the two metal elements in the alloy, the alloy usually exhibits better performance than a single metal nanoparticle, such as higher catalytic activity, better catalytic selectivity and stronger resistance to deactivation, which is very beneficial for building electrochemical sensors with excellent performance.

[0003] Chemical plating, also known as electroless plating or autocatalytic plating, is a non-electroplating type of electroplating method. It is a non-electroplating process that reduces metal ions in the solution to metal elements to the plating surface without using external electrical energy. Summary of the invention

[0004] To this end, the present invention provides a method for preparing a composite material of graphene surface plated with silver and copper, the preparation steps comprising:

[0005] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, stirring for more than 2 hours under an ultrasonic environment, then separating the solid from the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove the residual alkali solution, then adding it to an aqueous solution of chloroacetic acid, stirring for more than 3 hours under an ultrasonic environment, separating the solid from the liquid after stirring, washing the solid phase with deionized water for more than 3 times, and then drying at 60° C. for more than 10 hours to obtain rough graphene;

[0006] (2) adding the roughened graphene to deionized water, stirring for more than 30 minutes under an ultrasonic environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring. After the addition is completed, the suspension is kept warm at 60±5° C. for more than 2 hours, condensing and refluxing during the insulation process, and separating the solid and liquid after the insulation is completed. The solid phase is dried at 60° C. for more than 15 hours to obtain pretreated graphene;

[0007] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; heating the composite aqueous solution of tin dichloride and hydrochloric acid to 55±3°C in a water bath to keep warm, then adding the pretreated graphene to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and after the addition is completed, ultrasonic stirring is performed at 55±3°C for more than 2h for sensitization treatment, and after sensitization, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at 60±3°C, ethylene glycol is added to the solution, and then ultrasonic stirring is performed at 60±3°C for more than 2h for activation treatment, and after activation, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and then added to an aqueous solution of sodium hypophosphite for ultrasonic stirring for more than 2h, and after the stirring is completed, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and dried at 60°C for more than 15h to obtain activated graphene;

[0008] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; mixing copper nitrate, silver nitrate, polyvinyl pyrrolidone, and deionized water to form a mixture, then dropping ammonia water and stirring, and continuously dropping ammonia water until the precipitate is completely dissolved to form a copper-silver ammonia solution; adding the activated graphene to the deionized water, and ultrasonically stirring for more than 30 minutes to obtain a dispersion; stirring the dispersion, and adding the copper-silver ammonia solution to the dispersion during the stirring process to obtain The mixed solution is heated in a water bath to 70±3° C. for insulation, and then the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and the aqueous solution of iridium chloride are added to the mixed solution under stirring, and after the addition is completed, the chemical plating is continued at 70±3° C. for more than 2 hours of constant temperature stirring, and condensation and reflux are performed during the constant temperature process; after the stirring is completed, the solid-liquid separation is performed, the solid phase is washed with deionized water for more than 3 times, and dried at 60° C. for more than 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

[0009] Furthermore, in the step (1), the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: aqueous solution of sodium hydroxide = 1:100.

[0010] Furthermore, in the step (1), the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 10-12 g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: chloroacetic acid aqueous solution = 1:100.

[0011] Furthermore, in the step (2), the mass ratio of the roughened graphene added to the deionized water is roughened graphene: deionized water = 1:200; the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.3-0.5:1-2:1.

[0012] Furthermore, in the step (3), in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is pretreated graphene: composite aqueous solution of tin dichloride and hydrochloric acid = 1:200; the washed solid phase and ethylene glycol are added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1 to 2:200; in the aqueous solution of sodium hypophosphite, the mass percentage of sodium hypophosphite is 2.5%, and the solvent is water; the mass ratio of the washed solid phase added to the aqueous solution of sodium hypophosphite is washed solid phase: aqueous solution of sodium hypophosphite = 1:500.

[0013] Furthermore, in the step (4), the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine is: 20-22 g / L disodium ethylenediaminetetraacetate, 1-2 g / L dimethylaminoborane, 12-18 g / L sodium hypophosphite, 5-6 g / L sodium borohydride, 8-9 g / L malic acid, 11-12 g / L succinic acid, 0.6-0.9 mg / L thiourea, 1-3 mg / L glycine, and the solvent is water; the mass ratio of the copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 3-4: 2.2-2.5: 0.2-0.3: 100; and the mass percentage of the solute in the ammonia water is 25%.

[0014] Furthermore, in the step (4), the activated graphene is added to deionized water in a mass ratio of activated graphene: deionized water = 1:100; the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine, and the aqueous solution of iridium chloride are added to the dispersion in a volume ratio of dispersion: copper-silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine: aqueous solution of iridium chloride = 50:40-50:100:4-6; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water.

[0015] The beneficial effect of the present invention is that the graphene surface coated with silver-copper composite material prepared by the method of the present invention can be used as a filler to significantly improve the mechanical properties and electrical conductivity of the copper matrix material, and on the basis of maintaining the high electrical conductivity of copper, the strength of the copper substrate is significantly improved, and the scope of use of the copper material is broadened. This is mainly because after the graphene surface is coated with silver-copper, the wettability and bonding force of the graphene and the copper matrix are improved. At the same time, silver itself has high electrical conductivity, and the coating layer doped with silver can further improve the electrical conductivity of the filler. The present invention first uses sodium hydroxide to treat graphene oxide. On the one hand, it can perform alkaline washing on the graphene oxide to remove the grease components on the graphene surface, and on the other hand, it can increase the number of active sites on the graphene surface, preparing for the subsequent silver-copper coating process; then, by treating with chloroacetic acid, the graphene surface is partially carboxylated, and then modified by N, N-dimethylethylenediamine and glycine, the adsorption of graphene oxide is greatly improved. In the plating process, more silver and copper complex ions are adsorbed on the surface of graphene oxide and then reduced to a silver-copper metal composite layer, which not only improves the plating efficiency of the silver-copper metal composite layer, but also makes the silver-copper metal composite layer and graphene more tightly combined, and is not easy to produce two-phase interface defects. The addition of iridium chloride in the plating process is mainly to promote plating nucleation and the silver content in the plating layer. After graphene adsorbs iridium ions, it can act as a non-uniform nucleation active point to promote the formation of crystal nuclei of the silver-copper plating layer on the graphene surface, improve the density of the plating layer, and improve the conductivity of the filler itself. Therefore, the added iridium chloride has a greater impact on the conductivity of the material. DETAILED DESCRIPTION

[0016] The present invention will be further described below in conjunction with the embodiments.

[0017] Example 1

[0018] A method for preparing a composite material of graphene surface plated with silver and copper, the preparation steps comprising:

[0019] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 10g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0020] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.3:1:1; after the addition is completed, continue to stir and incubate at 60±5° C. for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0021] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0022] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 20 g / L disodium ethylenediaminetetraacetate, 1 g / L dimethylaminoborane, 12 g / L sodium hypophosphite, 5 g / L sodium borohydride, 8 g / L malic acid, 11 g / L succinic acid, 0.6 mg / L thiourea, and 1 mg / L glycine, and the solvent is water; adding copper nitrate and silver nitrate; , polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 3:2.2:0.2:100; then ammonia water is added dropwise and stirred, and ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added into the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30min to obtain a dispersion; the mass ratio of the activated graphene added into the deionized water is activated Graphene: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during stirring to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the dispersion. The volume ratio of the aqueous solution of iridium chloride is dispersion liquid: copper silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine: aqueous solution of iridium chloride = 50:40:100:4; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C constant temperature and stirred for 2 hours, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water for 3 times, and dried at 60°C for 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

[0023] Example 2

[0024] A method for preparing a composite material of graphene surface plated with silver and copper, the preparation steps comprising:

[0025] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 11g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0026] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.4:1:1; after the addition is completed, continue to keep warm at 60±5° C. and stir for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0027] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0028] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 21 g / L disodium ethylenediaminetetraacetate, 1 g / L dimethylaminoborane, 14 g / L sodium hypophosphite, 5 g / L sodium borohydride, 8 g / L malic acid, 11 g / L succinic acid, 0.7 mg / L thiourea, and 2 mg / L glycine, and the solvent is water; adding copper nitrate and silver nitrate; , polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 3:2.3:0.2:100; then ammonia water is added dropwise and stirred, and ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added into the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30min to obtain a dispersion; the mass ratio of the activated graphene added into the deionized water is activated graphene: Graphene: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during stirring to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the dispersion. The volume ratio of the aqueous solution of iridium chloride is dispersion liquid: copper silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine: aqueous solution of iridium chloride = 50:40:100:5; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C constant temperature and stirred for 2 hours, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water for 3 times, and dried at 60°C for 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

[0029] Example 3

[0030] A method for preparing a composite material of graphene surface plated with silver and copper, the preparation steps comprising:

[0031] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 11g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0032] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.4:2:1; after the addition is completed, continue to stir and incubate at 60±5° C. for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0033] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:2:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0034] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 21 g / L disodium ethylenediaminetetraacetate, 2 g / L dimethylaminoborane, 16 g / L sodium hypophosphite, 6 g / L sodium borohydride, 9 g / L malic acid, 12 g / L succinic acid, 0.8 mg / L thiourea, and 2 mg / L glycine, and the solvent is water; adding copper nitrate and silver nitrate; , polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 4:2.4:0.3:100; then ammonia water is added dropwise and stirred, and ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added into the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30min to obtain a dispersion; the mass ratio of the activated graphene added into the deionized water is activated Graphene: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during stirring to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the dispersion. The volume ratio of the aqueous solution of iridium chloride is dispersion liquid: copper silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine: aqueous solution of iridium chloride = 50:50:100:5; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C constant temperature and stirred for 2 hours, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water for 3 times, and dried at 60°C for 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

[0035] Example 4

[0036] A method for preparing a composite material of graphene surface plated with silver and copper, the preparation steps comprising:

[0037] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 12g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0038] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.5:2:1; after the addition is completed, continue to keep stirring at 60±5° C. for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0039] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:2:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0040] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 22 g / L disodium ethylenediaminetetraacetate, 2 g / L dimethylaminoborane, 18 g / L sodium hypophosphite, 6 g / L sodium borohydride, 9 g / L malic acid, 12 g / L succinic acid, 0.9 mg / L thiourea, and 3 mg / L glycine, and the solvent is water; adding copper nitrate and silver nitrate; , polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 4:2.5:0.3:100; then ammonia water is added dropwise and stirred, and ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added into the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30min to obtain a dispersion; the mass ratio of the activated graphene added into the deionized water is activated Graphene: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during stirring to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and an aqueous solution of iridium chloride to the dispersion. The volume ratio of the aqueous solution of iridium chloride is dispersion liquid: copper silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine: aqueous solution of iridium chloride = 50:50:100:6; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C constant temperature and stirred for 2 hours, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water for 3 times, and dried at 60°C for 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

[0041] Comparative Example 1

[0042] A preparation method of a graphene surface-plated silver-copper composite material as a comparison, the preparation steps comprising:

[0043] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10% and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then drying for 10 hours under a 60°C environment to obtain the roughened graphene of this comparative example;

[0044] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.4:1:1; after the addition is completed, continue to keep warm at 60±5° C. and stir for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0045] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0046] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 21 g / L disodium ethylenediaminetetraacetate, 1 g / L dimethylaminoborane, 14 g / L sodium hypophosphite, 5 g / L sodium borohydride, 8 g / L malic acid, 11 g / L succinic acid, 0.7 mg / L thiourea, and 2 mg / L glycine, and the solvent is water; adding copper nitrate, silver nitrate, Polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate:silver nitrate:polyvinyl pyrrolidone:deionized water=3:2.3:0.2:100; then ammonia water is added dropwise and stirred, and the ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added to the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30 minutes to obtain a dispersion; the mass ratio of the activated graphene added to the deionized water is activated graphene: olefin: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during the stirring process to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and iridium chloride to the dispersion; The volume ratio of the aqueous solution is dispersion liquid: copper-silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine: aqueous solution of iridium chloride = 50:40:100:5; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C and stirred for 2h, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water 3 times, and dried at 60°C for 10h to obtain the graphene surface-copper-plated composite material described in this comparative example.

[0047] Comparative Example 2

[0048] A preparation method of a graphene surface-plated silver-copper composite material as a comparison, the preparation steps comprising:

[0049] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 11g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0050] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath and then adding N,N-dimethylethylenediamine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: roughened graphene = 0.4:1; continuing to stir and incubate at 60±5° C. for 2 h after the addition is completed, condensing and reflux during the insulation process, separating the solid and liquid after the insulation is completed, and drying the solid phase at 60° C. for 15 h to obtain the pretreated graphene of this comparative example;

[0051] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0052] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is: 21 g / L disodium ethylenediaminetetraacetate, 1 g / L dimethylaminoborane, 14 g / L sodium hypophosphite, 5 g / L sodium borohydride, 8 g / L malic acid, 11 g / L succinic acid, 0.7 mg / L thiourea, and 2 mg / L glycine, and the solvent is water; adding copper nitrate, silver nitrate, Polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate:silver nitrate:polyvinyl pyrrolidone:deionized water=3:2.3:0.2:100; then ammonia water is added dropwise and stirred, and the ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added to the deionized water, and ultrasonic (200W, 30kHz) is stirred for 30 minutes to obtain a dispersion; the mass ratio of the activated graphene added to the deionized water is activated graphene: olefin: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during the stirring process to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath, and then adding the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and iridium chloride to the mixed solution under stirring, adding the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and iridium chloride to the dispersion; The volume ratio of the aqueous solution is dispersion liquid: copper-silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine: aqueous solution of iridium chloride = 50:40:100:5; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water; after the addition is completed, the chemical plating is continued at 70±3°C and stirred for 2h, and condensation and reflux are carried out during the constant temperature process; after the stirring is completed, the solid-liquid separation is carried out, the solid phase is washed with deionized water 3 times, and dried at 60°C for 10h to obtain the graphene surface-copper-plated composite material described in this comparative example.

[0053] Comparative Example 3

[0054] A preparation method of a graphene surface-plated silver-copper composite material as a comparison, the preparation steps comprising:

[0055] (1) adding graphene oxide to an aqueous solution of sodium hydroxide, wherein the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: the aqueous solution of sodium hydroxide = 1:100; stirring for 2 hours under an ultrasonic (200W, 30kHz) environment, then separating the solid and the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove residual alkali solution, and then adding it to an aqueous solution of chloroacetic acid, wherein the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 11g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: the aqueous solution of chloroacetic acid = 1:100; stirring for 3 hours under an ultrasonic (200W, 30kHz) environment, separating the solid and the liquid after stirring, washing the solid phase with deionized water 3 times, and then drying at 60°C for 10 hours to obtain rough graphene;

[0056] (2) adding the roughened graphene to deionized water, wherein the mass ratio of the roughened graphene to the deionized water is roughened graphene: deionized water = 1:200; stirring for 30 min under an ultrasonic (200 W, 30 kHz) environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring, wherein the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine: glycine: roughened graphene = 0.4:1:1; after the addition is completed, continue to keep warm at 60±5° C. and stir for 2 h, condense and reflux during the insulation process, separate the solid and liquid after the insulation is completed, and dry the solid phase at 60° C. for 15 h to obtain pretreated graphene;

[0057] (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the composite aqueous solution of tin dichloride and hydrochloric acid is heated to 55±3° C. in a water bath and then added to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is 1:200; after the addition is completed, ultrasonic stirring (200 W, 30 kHz) is performed at 55±3° C. for 2 h for sensitization treatment, and solid-liquid separation is performed after sensitization, and the solid phase is washed with deionized water for 3 hours. times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at a constant temperature of 60±3°C, ethylene glycol was added to the solution, and the washed solid phase and ethylene glycol were added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1:200; then 60±3°C ultrasonic (200W, 30kHz) stirring for 2h for activation treatment, solid-liquid separation after activation, the solid phase was washed 3 times with deionized water, and then added to an aqueous solution of sodium hypophosphite with ultrasonic (200W, 30kHz) stirring for 2h, the mass percentage of sodium hypophosphite in the aqueous solution of sodium hypophosphite was 2.5%, and the solvent was water; the washed solid phase was added to the aqueous solution of sodium hypophosphite in a mass ratio of washed solid phase: aqueous solution of sodium hypophosphite = 1:500; after the stirring was completed, the solid-liquid separation was performed, the solid phase was washed 3 times with deionized water, and dried at 60°C for 15h to obtain activated graphene;

[0058] (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine is as follows: disodium ethylenediaminetetraacetate 21 g / L, dimethylaminoborane 1 g / L, sodium hypophosphite 14 g / L, sodium borohydride 5 g / L, malic acid 8 g / L, succinic acid 11 g / L, thiourea 0.7 mg / L, glycine 2 mg / L, The solvent is water; copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water are mixed and stirred to form a mixture, wherein the mass ratio of the copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 3:2.3:0.2:100; then ammonia water is added dropwise and stirred, and the ammonia water is continuously added dropwise until the precipitate is just completely dissolved to form a copper-silver ammonia solution; the mass percentage of the solute in the ammonia water is 25%; the activated graphene is added to the deionized water, and ultrasonic (200W, 30kHz) stirring is performed for 30 minutes to obtain dispersion; adding the activated graphene to deionized water in a mass ratio of activated graphene: deionized water = 1:100; stirring the dispersion, adding the copper-silver ammonia solution to the dispersion during stirring to obtain a mixed solution, heating the mixed solution to 70±3° C. in a water bath for insulation, then adding a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine to the mixed solution under stirring, and adding the copper-silver ammonia solution, the disodium ethylenediaminetetraacetate, dimethylaminoborane, The volume ratio of the composite aqueous solution of sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine is dispersion solution: copper silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetic acid, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine = 50:40:100; after the addition is completed, continue to stir at a constant temperature of 70±3°C for 2h for chemical plating, and condense and reflux during the constant temperature process; after stirring is completed, the solid and liquid are separated, the solid phase is washed with deionized water 3 times, and dried at 60°C for 10h to obtain the graphene surface-copper-plated composite material described in this comparative example.

[0059] Example 5

[0060] The composite materials prepared by the methods described in the above embodiments and comparative examples were used as fillers to prepare copper-based composite materials. The preparation method was as follows: the filler and copper powder were mixed in a mass ratio of filler: copper powder = 0.5:99.5, and the mixed materials were ball milled for 2 hours at a speed of 100 r / min to obtain a mixed powder; the mixed powder was sintered at 850°C for 10 minutes under a pressure of 50 MPa to obtain a copper-based composite material. The tensile strength of the copper-based composite materials obtained in each test group was tested, and the tensile speed was set to 0.5 mm / min; in addition, the conductivity of each copper-based composite material was tested using a digital eddy current metal conductivity meter, and each group of samples was measured 5 times to take the average value, and the results are shown in Table 1.

[0061] As shown in Table 1, the graphene surface coated with silver-copper composite material prepared by the method of the present invention as filler can significantly improve the mechanical properties and electrical conductivity of the copper matrix material, and on the basis of maintaining the high electrical conductivity of copper, significantly improve the strength of the copper substrate, and broaden the scope of use of the copper material. This is mainly because after the graphene surface is coated with silver-copper, the wettability and bonding force of the graphene and the copper matrix are improved. At the same time, silver itself has high electrical conductivity, and the coating layer doped with silver can further improve the electrical conductivity of the filler. The present invention first uses sodium hydroxide to treat graphene oxide. On the one hand, it can be alkali-washed to the graphene oxide to remove the grease components on the graphene surface. In addition, it can increase the number of active sites on the graphene surface, and prepare for the subsequent silver-copper coating process; then, it is treated with chloroacetic acid to partially carboxylate the graphene surface, and then modified by N, N-dimethylethylenediamine and glycine, which greatly improves the adsorption of graphene oxide. In the plating process, more silver and copper complex ions are adsorbed on the surface of graphene oxide and then reduced to a silver-copper metal composite layer, which not only improves the plating efficiency of the silver-copper metal composite layer, but also makes the silver-copper metal composite layer and graphene more tightly combined, and is not easy to produce two-phase interface defects. The addition of iridium chloride in the plating process is mainly to promote plating nucleation and the silver content in the plating layer. After graphene adsorbs iridium ions, it can act as a non-uniform nucleation active point to promote the formation of crystal nuclei of the silver-copper plating layer on the graphene surface, improve the density of the plating layer, and improve the conductivity of the filler itself. Therefore, the added iridium chloride has a greater impact on the conductivity of the material.

[0062] Table 1

[0063] Experimental Group Tensile strength(MPa) Electrical conductivity (%IACS) Example 1 116 92.3 Example 2 122 93.1 Example 3 120 92.9 Example 4 117 92.6 Comparative Example 1 108 79.8 Comparative Example 2 99 68.0 Comparative Example 3 111 73.4

[0064] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for preparing a composite material of graphene surface plated with silver and copper, It is characterized in that The preparation steps include: (1) adding graphene oxide to an aqueous solution of sodium hydroxide, stirring for more than 2 hours under an ultrasonic environment, then separating the solid from the liquid, washing the solid phase with deionized water until the washed liquid is neutral to remove the residual alkali solution, then adding it to an aqueous solution of chloroacetic acid, stirring for more than 3 hours under an ultrasonic environment, separating the solid from the liquid after stirring, washing the solid phase with deionized water for more than 3 times, and then drying at 60° C. for more than 10 hours to obtain rough graphene; (2) adding the roughened graphene to deionized water, stirring for more than 30 minutes under an ultrasonic environment to obtain a suspension, heating the suspension to 60±5° C. in a water bath, and then adding N,N-dimethylethylenediamine and glycine to the suspension under stirring. After the addition is completed, the suspension is kept warm at 60±5° C. for more than 2 hours, condensing and refluxing during the insulation process, and separating the solid and liquid after the insulation is completed. The solid phase is dried at 60° C. for more than 15 hours to obtain pretreated graphene; (3) preparing a composite aqueous solution of tin dichloride and hydrochloric acid, and preparing a composite aqueous solution of lead dichloride and hydrochloric acid; heating the composite aqueous solution of tin dichloride and hydrochloric acid to 55±3°C in a water bath to keep warm, then adding the pretreated graphene to the composite aqueous solution of tin dichloride and hydrochloric acid under stirring, and after the addition is completed, ultrasonic stirring is performed at 55±3°C for more than 2h for sensitization treatment, and after sensitization, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and then added to the composite aqueous solution of lead dichloride and hydrochloric acid in a water bath at 60±3°C, ethylene glycol is added to the solution, and then ultrasonic stirring is performed at 60±3°C for more than 2h for activation treatment, and after activation, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and then added to an aqueous solution of sodium hypophosphite for ultrasonic stirring for more than 2h, and after the stirring is completed, solid-liquid separation is performed, and the solid phase is washed with deionized water for more than 3 times, and dried at 60°C for more than 15h to obtain activated graphene; (4) preparing a composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine; mixing copper nitrate, silver nitrate, polyvinyl pyrrolidone, and deionized water to form a mixture, then dropping ammonia water and stirring, and continuously dropping ammonia water until the precipitate is completely dissolved to form a copper-silver ammonia solution; adding the activated graphene to the deionized water, and ultrasonically stirring for more than 30 minutes to obtain a dispersion; stirring the dispersion, and adding the copper-silver ammonia solution to the dispersion during the stirring process to obtain The mixed solution is heated in a water bath to 70±3° C. for insulation, and then the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, glycine and the aqueous solution of iridium chloride are added to the mixed solution under stirring, and after the addition is completed, the chemical plating is continued at 70±3° C. for more than 2 hours of constant temperature stirring, and condensation and reflux are performed during the constant temperature process; after the stirring is completed, the solid-liquid separation is performed, the solid phase is washed with deionized water for more than 3 times, and dried at 60° C. for more than 10 hours to obtain the composite material of the graphene surface plated with silver and copper.

2. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 1, It is characterized in that In the step (1), the mass percentage of sodium hydroxide in the aqueous solution of sodium hydroxide is 10%, and the solvent is water; the mass ratio of the graphene oxide added to the aqueous solution of sodium hydroxide is graphene oxide: aqueous solution of sodium hydroxide = 1:

100.

3. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 1, It is characterized in that In the step (1), the concentration of chloroacetic acid in the aqueous solution of chloroacetic acid is 10-12 g / L, and the solvent is water; the mass ratio of the material added to the aqueous solution of chloroacetic acid to the solution is material: chloroacetic acid aqueous solution = 1:

100.

4. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 1, It is characterized in that In the step (2), the mass ratio of the roughened graphene added to the deionized water is roughened graphene:deionized water=1:200; the mass ratio of N,N-dimethylethylenediamine and glycine added to the suspension to the mass ratio of the roughened graphene in the suspension is N,N-dimethylethylenediamine:glycine:roughened graphene=0.3-0.5:1-2:

1.

5. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 1, It is characterized in that In the step (3), in the composite aqueous solution of tin dichloride and hydrochloric acid, the concentration of tin dichloride is 2.8 g / L, the mass percentage of HCl is 1%, and the solvent is water; in the composite aqueous solution of lead dichloride and hydrochloric acid, the concentration of lead dichloride is 0.2 g / L, the mass percentage of HCl is 0.6%, and the solvent is water; the mass ratio of the pretreated graphene added to the composite aqueous solution of tin dichloride and hydrochloric acid is pretreated graphene: composite aqueous solution of tin dichloride and hydrochloric acid = 1:200; the washed solid phase and ethylene glycol are added to the composite aqueous solution of lead dichloride and hydrochloric acid in a mass ratio of washed solid phase: ethylene glycol: composite aqueous solution of lead dichloride and hydrochloric acid = 1:1 to 2:200; in the aqueous solution of sodium hypophosphite, the mass percentage of sodium hypophosphite is 2.5%, and the solvent is water; the mass ratio of the washed solid phase added to the aqueous solution of sodium hypophosphite is washed solid phase: aqueous solution of sodium hypophosphite = 1:

500.

6. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 1, It is characterized in that In the step (4), the concentration of each component in the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea and glycine is: 20-22 g / L of disodium ethylenediaminetetraacetate, 1-2 g / L of dimethylaminoborane, 12-18 g / L of sodium hypophosphite, 5-6 g / L of sodium borohydride, 8-9 g / L of malic acid, 11-12 g / L of succinic acid, 0.6-0.9 mg / L of thiourea, and 1-3 mg / L of glycine, and the solvent is water; the mass ratio of the copper nitrate, silver nitrate, polyvinyl pyrrolidone and deionized water is copper nitrate: silver nitrate: polyvinyl pyrrolidone: deionized water = 3-4: 2.2-2.5: 0.2-0.3: 100; and the mass percentage of the solute in the ammonia water is 25%.

7. A method for preparing a composite material of graphene surface plated with silver and copper according to claim 6, It is characterized in that In the step (4), the activated graphene is added to deionized water in a mass ratio of activated graphene: deionized water = 1:100; the copper-silver ammonia solution, the composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine, and the aqueous solution of iridium chloride are added to the dispersion in a volume ratio of dispersion: copper-silver ammonia solution: composite aqueous solution of disodium ethylenediaminetetraacetate, dimethylaminoborane, sodium hypophosphite, sodium borohydride, malic acid, succinic acid, thiourea, and glycine: aqueous solution of iridium chloride = 50:40-50:100:4-6; in the aqueous solution of iridium chloride, the concentration of iridium chloride is 400 mg / L, and the solvent is water.