Preparation of honeycomb porous carbon / ferronickel double hydroxide / foamed nickel photo-anode

Through the preparation of honeycomb porous carbon/nickel iron double hydroxide/foam nickel photoanode, the problem of insufficient catalytic activity of nickel iron layered double hydroxide photoelectrode in photoelectrochemical water decomposition is solved, and efficient water decomposition is achieved The reaction improves photocatalytic performance and stability.

CN118880368AActive Publication Date: 2024-11-01NORTHEASTERN UNIV CHINA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410799859.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-01
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The existing nickel-iron layered double hydroxide photoelectrodes have problems such as high photogenerated electron-hole recombination rate and narrow visible light absorption range in the photoelectrochemical water decomposition hydrogen production, resulting in insufficient catalytic activity and difficult to achieve efficient water decomposition reaction.

Method used

Honeycomb porous carbon/nickel iron double hydroxide/foam nickel photoanode is prepared by an autoclave and hydrothermal method, combined with high-temperature carbonization and hydrothermal calcination in nitrogen environment, forming photoelectric with large specific surface area and many reactive sites. The electrode can improve the separation and migration rate of photogenerated carriers and expand the visible light absorption range.

Benefits of technology

It has achieved improved photocatalytic activity, fast separation and migration rates of photogenerated carriers, low overlap rate of photogenerated carriers, high material stability, simple preparation process, low cost, high yield, good repeatability and environmental friendliness .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses a honeycomb porous carbon / ferronickel double hydroxide / foamed nickel photo-anode and a preparation method thereof. The ferro-nickel double hydroxide is prepared by calcining nickel nitrate, ferric nitrate, ammonium fluoride and urea as raw materials. The photoanode is prepared by mixing, stirring and calcining raw materials with different masses. The preparation method comprises the following steps: F1, grinding a certain mass of dried shaddock peel and pulp into powder, and carbonizing at high temperature to obtain honeycomb porous carbon; and F2, washing the product with ultrapure water and ethanol, drying, mixing, dissolving in water, putting into a high-pressure reaction kettle, putting foamed nickel into the reaction kettle, putting the high-pressure reaction kettle into a hydrothermal furnace, calcining at a certain temperature, and collecting the product, namely the honeycomb porous carbon / ferronickel double hydroxide / foamed nickel photo-anode. The prepared photo-anode has the advantages of being large in specific surface area, multiple in active site, high in photon-generated carrier separation and migration rate, high in photocatalytic activity and high in stability, and therefore improvement of the photoelectrocatalytic performance of the photo-anode is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nanomaterials and relates to a lamellar nickel-iron double hydroxide photocatalyst and a honeycomb porous carbon / nickel-iron double hydroxide / foam nickel photoanode and a preparation method thereof. Background Art

[0002] Energy shortage and environmental pollution caused by the continuous exploitation and burning of fossil fuels are becoming increasingly serious. Today, researchers are looking for renewable clean energy to replace non-renewable fossil fuels to meet the growing energy demand and solve related environmental problems. Hydrogen energy has many advantages such as cleanliness, efficiency, safety, storability and transportability, so it has been highly valued by various countries. Green hydrogen is expected to become a new generation of energy carrier, and hydrogen energy preparation technology is also a hot topic for scientists.

[0003] Photoelectrochemical (PEC) water splitting for hydrogen production can reasonably select the photoanode and photocathode, has high flexibility, can split water at room temperature, is simple to operate, and can directly separate and produce hydrogen. The overpotential required to produce the same amount of hydrogen is low. Photoelectrochemical water splitting is an attractive strategy for large-scale production of renewable hydrogen. The development of low-cost, highly active and stable semiconductor photoelectrodes is crucial to achieve efficient PEC water splitting. Although photoelectrocatalytic water splitting for hydrogen production is still in the theoretical research stage, this method has potential practical prospects. Perovskite oxides, as a large class of semiconductor metal oxides, are widely used for PEC water splitting for hydrogen production due to their abundant content, high (photo)electrochemical stability, composition and structural flexibility, high electrocatalytic activity, and strong sunlight absorption ability. Nickel-iron layered double hydroxide (NiFeLDH) has many advantages such as good visible light response properties, high thermochemical stability, easy to control structural morphology, non-toxic, easy to prepare, low cost, moderate bandgap width, large specific surface area, etc. However, it has the disadvantages of high photogenerated electron-hole recombination rate and narrow visible light absorption range. Therefore, the following methods are adopted to optimize it. First, it forms a heterojunction with other catalysts to improve the electron-hole mobility; second, it provides more reactive sites through morphology control (such as spheres, nanotubes, hollow spheres, nanosheets); third, it increases the specific surface area of ​​the material through structural design (loaded, core-shell, eggshell structure) to improve the thermal stability of the material. Nickel foam is used as an electrode of alkaline electrolyzer due to its rich and porous three-dimensional structure. In recent years, the HER (hydrogen evolution) of NiFeLDH has received widespread attention, and it has been shown that the doping of a small amount of honeycomb porous carbon can improve the catalytic activity. The in-situ grown synthesis of nickel foam photoanode has a fast reaction rate and can be completed in a short time, improving production efficiency.

[0004] From the perspective of green, clean and efficient, this patent intends to design and prepare a series of NiFe LDH complexes as new water splitting photoelectrodes, test the photoelectrochemical performance and analyze its reaction mechanism, and provide new ideas for further developing efficient and inexpensive hydrogen production materials and promoting the industrialization of water splitting hydrogen production technology. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In order to overcome the deficiencies in the prior art, the present invention provides a honeycomb porous carbon / nickel-iron double hydroxide / nickel foam photoanode with large specific surface area, multiple active sites, fast photogenerated carrier separation and migration rate, low photogenerated carrier coincidence rate, red-shifted visible light absorption range, high photocatalytic activity and high stability, and provides a preparation method with simple process, easy operation, relatively low production cost, high product yield and good repeatability.

[0007] (II) Technical solution (honeycomb porous carbon / nickel iron double hydroxide / nickel foam photoanode)

[0008] F1: Take a certain amount of grapefruit peel and cut it into small pieces, put it into a hot air drying oven and dry it for a period of time. After soaking the dried sample in potassium hydroxide solution, freeze-dry the obtained sample, and then grind the processed samples evenly to make powder;

[0009] F2: Put the powder into a nitrogen-filled tube furnace to carbonize the sample at high temperature in a nitrogen environment, grind the black solid into uniform powder and wash it with dilute nitric acid, centrifuge and dry it to obtain black powder;

[0010] F3: A certain amount of the above black powder, nickel nitrate, iron nitrate, ammonium fluoride and urea mixture are mixed in a certain proportion and put into a high-pressure reactor, and then the nickel foam is put into the solution, and the high-pressure reactor is placed in a hydrothermal furnace and calcined at a certain temperature to obtain black nickel foam. After the black nickel foam is dried, a photoelectrode is obtained.

[0011] In a preferred embodiment, in F1, 20 g of grapefruit peel and pulp are cut into small pieces, and the dried grapefruit peel and pulp are soaked in 100 mL of 1 mol·L -1 of KOH solution for 12h.

[0012] In a preferred embodiment, in F2, 5 g of the dried powder is placed in a crucible and placed in a tube furnace at 2 °C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1The temperature was raised to 800°C and maintained for 60 min, and then naturally cooled to room temperature to obtain a black solid.

[0013] In a preferred embodiment, in F3, the method for preparing the photoanode comprises the following steps:

[0014] (1) Weigh 0.9 g of honeycomb porous carbon powder, 0.52 g of nickel nitrate, 0.08 g of iron nitrate, 0.15 g of ammonium fluoride, and 0.6 g of urea, put the raw materials into a beaker in sequence, add 70 mL of ultrapure water, and stir for 3 h to fully mix;

[0015] (2) The sample and nickel foam are placed in a high-pressure reactor and calcined in a hydrothermal furnace at a certain temperature and time.

[0016] In a preferred embodiment, the step (2) comprises the following steps:

[0017] (1) The sample was placed in a hydrothermal furnace for calcination at 200 °C for 24 h and then naturally cooled to room temperature;

[0018] (2) The mass fraction of the honeycomb porous carbon in the nickel-iron double hydroxide doped with honeycomb porous carbon is in the range of 1% to 10%, with the preferred mass fraction being 2%. The nickel foam is a sample with a length of 4 cm and a width of 2 cm.

[0019] In a preferred embodiment, in F3, the black nickel foam obtained by naturally air-drying the nickel foam by clamping it with tweezers is the honeycomb porous carbon / nickel-iron double hydroxide / nickel foam photoanode.

[0020] (IV) Beneficial effects

[0021] The beneficial effects of the present invention are:

[0022] The present invention provides a honeycomb porous carbon / nickel-iron double hydroxide / nickel foam photoanode and a preparation method thereof. In the present invention, the material has the advantages of moderate band gap, excellent thermal stability and chemical stability, environmental friendliness, no toxic components and no secondary pollution, and is an ideal green catalyst. This material has a high specific surface area and abundant reaction active sites, and is a good charge transport material. The present invention proposes for the first time to use a NiFe LDH photocatalyst with a nickel-iron ratio of 9:1 and a 2% honeycomb porous carbon / nickel-iron double hydroxide / nickel foam photoanode to promote the separation and transmission of photogenerated carriers in the photocatalytic reaction. The use of such materials can improve the absorption rate of visible light, and increase the active sites of the water decomposition reaction by means of the large specific surface area of ​​the material, ultimately achieving the purpose of improving the overall photocatalytic performance of the photoanode.

[0023] The preparation process of the method of the present invention has the following advantages: simple process, easy operation, relatively low production cost, high product yield and good repeatability.

[0024] The photoanode prepared by the method of the present invention has the following advantages: large specific surface area, multiple active sites, fast separation and migration rate of photogenerated carriers, low coincidence rate of photogenerated carriers, red shift in visible light absorption range, high photocatalytic activity and high stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Flow chart for preparing nickel-iron double hydroxide photocatalyst and honeycomb porous carbon / nickel-iron double hydroxide / nickel foam photoanode for this patent;

[0026] Figure 2 0%-10% HLPC / Ni synthesized in Example 1 0.9 Fe 0.1 X-ray diffraction pattern of LDH;

[0027] Figure 3 is the Ni synthesized in Example 1 0.9 Fe 0.1 LDH and 2% HLPC / Ni 0.9 Fe 0.1 Scanning electron micrograph of LDH;

[0028] Figure 4 0%-10% HLPC / Ni synthesized in Example 1 0.9 Fe 0.1 Impedance diagram of LDH;

[0029] Figure 5 0%-10% HLPC / Ni synthesized in Example 1 0.9 Fe 0.1 Linear voltammetry (LSV) plot of LDH;

[0030] Figure 6 0%-10% HLPC / Ni synthesized in Example 1 0.9 Fe 0.1 Time-current graph of LDH.

[0031] Specific implementation scheme (Ni 0.9 Fe 0.1 LDH)

[0032] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation schemes.

[0033] This embodiment proposes a 2% honeycomb porous carbon / nickel iron double hydroxide / foam nickel photoanode and a preparation method thereof. The preparation method of the nanomaterial comprises the following steps:

[0034] F1: Take a certain amount of grapefruit peel and cut it into small pieces, put it into a hot air drying oven and dry it for a period of time. After soaking the dried sample in potassium hydroxide solution, freeze-dry the obtained sample, and then grind the processed samples evenly to make powder;

[0035] F2: The powder is placed in a nitrogen-filled tubular furnace to carbonize the sample at high temperature in a nitrogen environment. The black solid is ground into a uniform powder and washed with dilute nitric acid. After centrifugation, it is dried to obtain a black powder.

[0036] F3: A certain amount of the above black powder, nickel nitrate, iron nitrate, ammonium fluoride and urea mixture are mixed in a certain proportion and put into a high-pressure reactor, and then the nickel foam is put into the solution, and the high-pressure reactor is placed in a hydrothermal furnace and calcined at a certain temperature to obtain black nickel foam. After the black nickel foam is dried, a photoelectrode is obtained.

[0037] Specifically, F1 includes the following steps:

[0038] Take 20g of grapefruit peel and cut it into small pieces. Soak the dried grapefruit peel in 100mL of 1mol·L -1 of KOH solution for 12h.

[0039] Step F2 includes the following steps:

[0040] The dried powder was placed in a crucible and placed in a tube furnace at 2 °C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1 The temperature was raised to 800°C and maintained for 60 min, and then naturally cooled to room temperature to obtain a black solid.

[0041] Step F3 comprises the following steps:

[0042] F3.1: Weigh 0.9g of honeycomb porous carbon powder, 0.52g of nickel nitrate, 0.08g of iron nitrate, 0.15g of ammonium fluoride and 0.6g of urea, put the raw materials into a beaker in turn, add 70mL of ultrapure water and stir for 3h to fully mix them.

[0043] F3.2: Place the sample and nickel foam into a high-pressure reactor, calcine them at 200°C for 24 hours in a hydrothermal furnace, and then cool them naturally to room temperature.

[0044] F3.3: Remove the supernatant and collect the precipitate; place the precipitate in a drying oven at 60°C and dry it for 24 hours to obtain a honeycomb porous carbon / nickel iron double hydroxide photocatalyst. Use tweezers to pick up the nickel foam and let it air dry naturally to obtain the black nickel foam, which is the honeycomb porous carbon / nickel iron double hydroxide / nickel foam photoanode.

[0045] In step S3.2, the mass fraction of the honeycomb porous carbon in the honeycomb porous carbon-doped nickel-iron double hydroxide is in the range of 1% to 10%, preferably 2%, and the foamed nickel is a sample of 4 cm in length and 2 cm in width.

[0046] The present invention uses a hydrothermal method to prepare a honeycomb porous carbon / nickel iron double hydroxide / nickel foam photoanode, which has a large specific surface area, more active sites, faster separation and migration rate of photogenerated carriers, higher coincidence rate of photogenerated carriers, red shift in low visible light absorption range, high photocatalytic activity, and high stability, thereby improving the photocatalytic efficiency. The method of the present invention has simple and easy operation, relatively low production cost, high product yield, good repeatability, and has potential practical prospects.

[0047] The present invention is further illustrated by the following examples.

[0048] Example 1

[0049] Take 20g of grapefruit peel, cut it into small pieces, and put it into a hot air drying oven at 60℃ to dry for 24h. Then soak the dried sample in 100mL 1mol·L -1 After 12 hours in KOH solution, the obtained sample was freeze-dried for 48 hours, and then the treated samples were ground into powder and put into a crucible and placed in a tube furnace. Nitrogen was introduced into the tube furnace to carbonize the sample at high temperature in a nitrogen environment at a rate of 2 ° C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1 The temperature was raised to 800 °C and kept for 60 min. After cooling naturally to room temperature, the obtained black solid was ground into powder and 50 mL of 1 mol·L -1 The sample is washed once with HNO3 to remove KOH and other inorganic impurities in the sample, and the surface of the sample is oxidized. The sample is washed with ultrapure water to neutrality, centrifuged and dried, and the resulting black powder is the honeycomb porous carbon.

[0050] Prepare a beaker and a high-pressure reactor. Wash the beaker with water and alcohol and put it in a drying oven to dry. Soak the reactor in nitric acid for 10 minutes, then wash it with water and alcohol and put it in a drying oven to dry. Use an electronic balance to weigh 0.9 mg of honeycomb porous carbon powder, 0.52 g of nickel nitrate, 0.08 g of iron nitrate, 0.15 g of NH4F, 0.6 g of urea, and 70 mL of ultrapure water as a solvent. Put the raw materials into a 100 mL beaker in turn, add 70 mL of ultrapure water and stir for 3 hours to mix them thoroughly. Put the sample into a dried 100 mL high-pressure reactor, and then tilt the 4 cm long and 2 cm wide nickel foam into the solution and calcine it at 200 ° C in a hydrothermal furnace for 24 hours. The final black nickel foam is HLPC / Ni with a mass ratio of 1%. 0.9 Fe 0.1 LDH nickel foam photoelectrode.

[0051] Example 2

[0052] Take 25g of grapefruit peel and cut it into small pieces, put it into a hot air drying oven at 60℃ and dry it for 36h. Then soak the dried sample in 50mL 1mol·L -1 After 18 hours in KOH solution, the obtained sample was freeze-dried for 60 hours, and then the treated samples were ground into powder and put into a crucible and placed in a tube furnace. Nitrogen was introduced into the tube furnace to make the sample carbonized at high temperature in a nitrogen environment at a rate of 2 ° C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1 The temperature was raised to 800 °C and kept for 60 min. After cooling naturally to room temperature, the obtained black solid was ground into powder and 100 mL of 1 mol·L -1 The sample was washed twice with HNO3 to remove KOH and other inorganic impurities in the sample, and the surface of the sample was oxidized. The sample was washed with ultrapure water to neutrality, centrifuged and dried, and the obtained black powder was the honeycomb porous carbon.

[0053] Prepare a beaker and a high-pressure reactor. Wash the beaker with water and alcohol and put it in a drying oven to dry. Soak the reactor in nitric acid for 10 minutes, then wash it with water and alcohol and put it in a drying oven to dry. Use an electronic balance to weigh 1.8 mg of honeycomb porous carbon powder, 0.52 g of nickel nitrate, 0.08 g of iron nitrate, 0.15 g of NH4F, 0.6 g of urea, and 70 mL of ultrapure water as a solvent. Put the raw materials into a 100 mL beaker in turn, add 70 mL of ultrapure water and stir for 3 hours to mix them thoroughly. Put the sample into a dried 100 mL high-pressure reactor, and then tilt the 4 cm long and 2 cm wide nickel foam into the solution and calcine it at 200 ° C in a hydrothermal furnace for 24 hours. The final black nickel foam is HLPC / Ni with a mass ratio of 2%. 0.9 Fe 0.1 LDH nickel foam photoelectrode.

[0054] Example 3

[0055] Take 30g of grapefruit peel and cut it into small pieces, put it into a hot air drying oven at 60℃ and dry it for 48h. Then soak the dried sample in 150mL 1mol·L -1 After 24 hours in KOH solution, the obtained sample was freeze-dried for 72 hours, and then the treated samples were ground into powder and put into a crucible and placed in a tube furnace. Nitrogen was introduced into the tube furnace to make the sample carbonized at high temperature in a nitrogen environment at a rate of 2 ° C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1 The temperature was raised to 800 °C and kept for 60 min. After cooling naturally to room temperature, the obtained black solid was ground into powder and then heated to 150 mL 1 mol·L -1 The sample was washed three times with HNO3 to remove KOH and other inorganic impurities in the sample, and the surface of the obtained sample was oxidized. The sample was washed with ultrapure water to neutrality, centrifuged and dried, and the obtained black powder was the honeycomb porous carbon.

[0056] Prepare a beaker and a high-pressure reactor. Wash the beaker with water and alcohol and put it in a drying oven to dry. Soak the reactor in nitric acid for 10 minutes, then wash it with water and alcohol and put it in a drying oven to dry. Use an electronic balance to weigh 4.5 mg of honeycomb porous carbon powder, 0.52 g of nickel nitrate, 0.08 g of iron nitrate, 0.15 g of NH4F, 0.6 g of urea, and 70 mL of ultrapure water as a solvent. Put the raw materials into a 100 mL beaker in turn, add 70 mL of ultrapure water and stir for 3 hours to mix them thoroughly. Put the sample into a dried 100 mL high-pressure reactor, and then tilt the 4 cm long and 2 cm wide nickel foam into the solution and calcine it at 200 ° C in a hydrothermal furnace for 24 hours. The final black nickel foam is HLPC / Ni with a mass ratio of 5%. 0.9 Fe 0.1 LDH nickel foam photoelectrode.

Claims

1. Preparation of a honeycomb porous carbon / nickel iron double hydroxide / nickel foam photoanode, characterized in that: Includes steps: F1: Take a certain amount of grapefruit peel and cut it into small pieces, put it into a hot air drying oven and dry it for a period of time. After soaking the dried sample in potassium hydroxide solution, freeze-dry the obtained sample, and then grind the processed samples evenly to make powder; F2: The powder is placed in a nitrogen-filled tubular furnace to carbonize the sample at high temperature in a nitrogen environment. The black solid is ground into a uniform powder and washed with dilute nitric acid. After centrifugation, it is dried to obtain a black powder. F3: A certain amount of the above black powder, nickel nitrate, iron nitrate, ammonium fluoride and urea mixture are mixed in a certain proportion and put into a high-pressure reactor, and then the nickel foam is put into the solution, and the high-pressure reactor is placed in a hydrothermal furnace and calcined at a certain temperature to obtain black nickel foam. After the black nickel foam is dried, a photoelectrode is obtained.

2. The preparation method according to claim 1, characterized in that: In F1, 20 g of grapefruit peel was cut into small pieces. The dried grapefruit peel was soaked in 100 mL of 1 mol·L -1 of KOH solution for 12h.

3. The preparation method according to claim 1, characterized in that: In F2, the dried powder was placed in a crucible and placed in a tube furnace at 2 °C min -1 The heating rate was increased to 300 °C and kept at 300 °C for 60 min. -1 Raise to 600℃ and keep warm for 30min, and finally heat at 5℃·min -1 The temperature was raised to 800°C and maintained for 60 min, and then naturally cooled to room temperature to obtain a black solid.

4. The preparation method according to claim 1, characterized in that: In F3, the method for preparing the photoanode comprises the following steps: (1) Weigh 0.9 g of honeycomb porous carbon powder, 0.52 g of nickel nitrate, 0.08 g of iron nitrate, 0.15 g of ammonium fluoride, and 0.6 g of urea, put the raw materials into a beaker in sequence, add 70 mL of ultrapure water, and stir for 3 h to fully mix; (2) The sample and nickel foam were placed in a high-pressure reactor, calcined at 200°C for 24 h in a hydrothermal furnace, and then naturally cooled to room temperature. (3) The mass fraction of the honeycomb porous carbon in the nickel-iron double hydroxide doped with honeycomb porous carbon is in the range of 1% to 10%, with the preferred mass fraction being 2%. The nickel foam is a sample with a length of 4 cm and a width of 2 cm.

Citation Information

Patent Citations

  • Nickel-iron double hydroxide / foamed nickel catalyst based on ferric chloride / urea eutectic solvent, and preparation method and application thereof

    CN110201670A

  • P-N heterojunction composite material loaded on surface of foamed nickel and preparation method and application thereof

    CN111389442A

  • Photocatalytic degradation material of Cu-doped nitrogen-deficient g-C3N4 / ZnCo2O4 heterojunction

    CN111604084A

  • Preparation method of carbon material loaded tubular carbon nitride photocatalyst

    CN113578370A

  • Phosphorus-doped porous flaky NiCo2O4 difunctional electrocatalyst as well as preparation and application thereof

    CN114438537A