Method for growing sub-nano protection layer in upper limit domain of perovskite metal oxide and performance prediction method
By growing subnano-level protective layer and metal particles in the limit domain of the perovskite surface, the problem of poor stability of perovskite catalysts in harsh atmospheres is solved, and the efficient catalytic performance and stability improvement in water is achieved, which is suitable for large-scale production .
Patent Information
- Application Number
- CN202410275120.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-01
AI Technical Summary
Perovskite-based catalysts have poor stability in harsh atmospheres, which limits their application in heterogeneous catalysis.
By growing a sub-nano-scale metal oxide protective layer in the confined domain of the perovskite surface and diffusing the B-position element outward under a reducing atmosphere, the FeOx protective layer and FeNi alloy metal particles are formed, and the stability and activity of the catalyst are improved.
The stability and catalytic performance of perovskite catalysts are improved under harsh conditions, the surface metal active sites are enhanced, and the catalytic reactions are efficient in water, and suitable for large-scale production.
Smart Images

Figure CN118880376A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for growing a sub-nanometer protective layer in a perovskite metal oxide upper limit domain and a performance prediction method, belonging to the technical field of catalysts. Background Art
[0002] As a non-precious metal oxide with an easily regulated structure, perovskite (general formula ABO3) is expected to become an effective substitute for traditional high-efficiency precious metal catalysts. Its crystal structure, elemental composition, defects and valence state can be adjusted to make the perovskite material exhibit different physical and chemical properties, thereby optimizing the performance in the expected direction. At present, perovskite materials have shown excellent catalytic performance in many fields. During the reaction process, the catalyst material inevitably comes into contact with reactants and products, including reducing (such as carbon monoxide) and corrosive gases (such as water vapor). Such a harsh atmosphere environment places extremely high demands on the stability of the catalyst. For perovskite, its A-position or B-position elements are easily affected by the external environment and segregate or react, thereby destroying the original crystal structure and inactivating the catalyst, which seriously restricts the long-term application and development of perovskite materials in the field of catalysis. Summary of the invention
[0003] The first technical problem to be solved by the present invention is that the stability of perovskite-based catalysts in harsh atmospheres such as water or CO2 is poor, which limits their application in heterogeneous catalysis. The present invention uses perovskite as a substrate, utilizes its unique crystal structure, and uses a simple reduction precipitation method to design A-site defects to provide a reduction driving force, so that the B-site elements within a limited depth on the perovskite surface diffuse outward and are reduced, and a sub-nanometer protective layer is confined to grow on the perovskite surface, without losing the original activity, and then regulates to obtain a catalyst material with excellent performance and stability under harsh conditions.
[0004] The first aspect of the present invention:
[0005] A perovskite oxide catalytic material, comprising: a base oxide, a protective layer, and metal particles on the protective layer;
[0006] The base oxide is a perovskite metal oxide having the general formula of ABO3, and the A-site element is a defect amount;
[0007] The protective layer is a metal oxide layer with a thickness of 0.1-3nm;
[0008] The metal particles are composed of one or more of the B-site elements.
[0009] In the photos of the perovskite oxide catalytic material obtained at a magnification of 50,000-100,000, the number of surface metal particles ranges from 20 to 200; the particle size ranges from 30 to 200 nm.
[0010] The A-site element of the perovskite metal oxide is selected from rare earth or alkali metal elements, such as Be, Mg, Ca, Sr, Ba, La, Ce, Cd, Pb or Bi; the B-site element of the perovskite metal oxide is selected from transition metal elements, such as Fe, Ni, Ti, Ta, Nb, Co, Mn, Al, Mo, Cu, Sc or Cr.
[0011] The chemical formula of the perovskite metal oxide in step 1 is Sr 0.9 Fe 0.81 Ta 0.09 Ni 0.1 O 3-δ .
[0012] The material of the protective layer is FeO x , the material of the metal particles is FeNi alloy.
[0013] A method for growing a sub-nanometer protective layer on a perovskite metal oxide upper domain comprises the following steps:
[0014] Step 1, based on the general formula of ABO3 perovskite metal oxides, metal oxide raw materials are mixed according to the stoichiometric ratio of A-site defects, and solid phase sintering is performed to form a phase;
[0015] Step 2, treating the oxide obtained in step 1 under a reducing atmosphere to diffuse the transition metal element at the B position to the surface, thereby obtaining a protective layer with a metal anchored on the surface.
[0016] The metal oxide raw materials are selected from SrCO3, Fe2O3, Ta2O5 and NiO; during the solid phase sintering process, the sintering parameters are 1000-1400°C for 1-20h.
[0017] In step 2, the atmosphere in the reduction step is pure hydrogen or an inert gas containing 1-99% hydrogen; the temperature of the reduction process is 500-1000° C. and the time is 1-5 hours.
[0018] The perovskite oxide material with a metal protective layer directly obtained by the above method.
[0019] Application of the above-mentioned perovskite oxide material in hydrogen evolution reaction (HER) in water electrolysis.
[0020] The above application also includes a method for predicting the catalytic performance of perovskite oxide materials, the steps comprising:
[0021] Step a, obtaining a perovskite oxide material with a metal protective layer obtained under different preparation conditions, and obtaining a surface SEM photograph;
[0022] Step b, based on the integrity of the material surface on the SEM photo, the preparation conditions corresponding to the surface protection layer with the best flatness are used as the preparation conditions for the material with the best HER catalytic performance.
[0023] The flatness is determined by cracks and / or holes on the base oxide and the protective layer; when there are the least cracks and / or holes, it is determined to have the best flatness.
[0024] The crack width is 10-100nm, and the hole diameter ranges from 200-2000nm.
[0025] The different preparation conditions refer to different reduction reaction times.
[0026] Beneficial Effects
[0027] 1. By confining the growth of a protective layer on the surface of perovskite and utilizing the superior stability of metal oxides in water compared to perovskite, the overall stability of the perovskite-based catalyst is improved. 2. In the process of confined growth, metal nanoparticles anchored on the surface of the protective layer can be obtained simultaneously, the number of exposed metal active sites can be increased, and a more active catalyst can be obtained by direct reduction. 3. The whole process is easy to operate, the conditions are easy to control, and it is suitable for large-scale production. The present invention has the advantages of novel structure, simple process conditions, low cost, and is more suitable for large-scale production. Its large-scale market launch will surely produce positive social benefits and significant economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 XRD diffraction spectra of SFTN perovskite-based samples obtained at different reduction times in Examples 1-6
[0029] Figure 2 SEM images of SFTN perovskite-based materials obtained at different reduction times in Examples 1-6, Figures (a)-(f) correspond to SEM images of reduction for 0-5h, respectively
[0030] Figure 3 Particle size distribution diagrams of metal nanoparticles grown on the surface of SFTN perovskite-based samples obtained at different reduction times in Examples 1-5. Figures (a)-(e) correspond to the particle size distribution diagrams of metal nanoparticles grown on the surface of the samples reduced for 1-5 h, respectively.
[0031] Figure 4 Atomic-level spherical aberration-corrected TEM image and EELS analysis of the cross section of the sample reduced for 2 h in Example 1
[0032] Figure 5 LSV curves of SFTN perovskite-based materials obtained at different reduction times in Examples 1-6 and the corresponding calculated 10 mA cm -1 Overpotential at and (b) Tafel slope volcano plot
[0033] Figure 6 Calculation of double-layer capacitance of SFTN perovskite-based materials obtained at different reduction times in Examples 1-6
[0034] Figure 7 Electrochemical impedance spectroscopy of SFTN perovskite-based materials obtained at different reduction times in Examples 1-6
[0035] Figure 8 HER stability performance test of electrolyzed water of Examples 1 and 6
[0036] Fig. 9 TEM high-resolution images of Examples 1 and 6 after the electrolytic water HER stability performance test DETAILED DESCRIPTION
[0037] Due to the difference in interfacial ion concentration, the A-site metal elements of perovskite oxides will experience severe ion leaching in water. This phenomenon is the direct cause of catalyst dissolution and deactivation. By constructing an ultra-thin protective film on the perovskite surface through the confined growth method, the perovskite surface can be protected and the stability problem when in contact with water can be effectively solved. This composite structure can reconstruct the surface electronic structure and inhibit the ion leaching of perovskite oxides in water. At the same time, the metal nanoparticles precipitated synchronously on the surface and the protective layer can further improve the catalytic activity of the material, achieving a simultaneous improvement in stability and catalytic performance.
[0038] In some specific implementations, the technical solution of this patent may be:
[0039] A method for confined growth of a protective layer on a perovskite surface. The method comprises:
[0040] Step 1: According to the designed stoichiometric ratio, the metal oxide raw material and the ball milling medium are fully mixed by ball milling, and after drying and sieving, they are placed in a muffle furnace for sintering to obtain the A-site defect perovskite powder;
[0041] The second step: Place the sintered perovskite powder material into a corundum crucible, and then into a sealed large glass sleeve, and perform reduction treatment under high temperature and hydrogen atmosphere to drive the B-site transition metal in the perovskite to change valence and diffuse outward, thus preparing a perovskite-based composite material with a metal / metal oxide protective layer grown on the surface.
[0042] Wherein: the ball milling medium is anhydrous ethanol.
[0043] The first step is performed under different parameter conditions to obtain a perovskite material, and a diffraction pattern of the perovskite material is obtained by an XRD method; in the XRD patterns of the samples prepared under different preparation conditions, the lowest temperature in the parameter conditions corresponding to the pattern having a good perovskite crystal phase and no impurity peaks is taken as the optimal value;
[0044] The different parameter conditions mentioned refer to the sintering temperature.
[0045] In the reduction treatment step, the reducing atmosphere is 5% H2+Ar, the heating and cooling rate is 5°C / min, and N2 is used as the protective gas during the heating and cooling process.
[0046] A perovskite-based composite material with a metal / metal oxide protective layer grown on the surface. The composite material is prepared by a confined growth method.
[0047] The perovskite-based composite material is an inorganic composite material in which a metal oxide protective layer is grown and wrapped on the surface of the perovskite, and metal nanoparticles are anchored on the protective layer.
[0048] The electrochemical test method process in the following examples is as follows:
[0049] Step a: Prepare the electrochemical test ink sample of the catalyst. Weigh 20 mg of catalyst and 20 mg of Super P.Li (conductive carbon black) powder into a special small glass bottle; add 1.8 mL of anhydrous ethanol and 0.2 mL of Nafion membrane solution (binder), pre-shake for 10 seconds, and ultrasonicate for 0.5 hours to evenly disperse the powder in the solution; use ice bags to control the temperature of the ultrasonic environment during the ultrasonic process, and finally obtain the test ink sample.
[0050] Step b: The ink samples were tested for HER catalytic performance. The experiment was a three-electrode system, the reference electrode was a RE-61AP / 1M KOH mercury-containing electrode, the counter electrode was a glassy carbon electrode, and the 1M KOH solution was purged with Ar to saturation.
[0051] (1) Use a pipette to take 5 μL of sample and drop it onto the electrode surface, then let it stand to dry.
[0052] (2) Set the electrode rotation speed to 1600 rpm, and slowly immerse the catalyst-coated portion of the electrode into the electrolyte. If there are small bubbles on the electrode, lift the electrode and immerse it again in the electrolyte until the small bubbles are completely eliminated, and then turn off the speed switch.
[0053] (3) Cyclic voltammetry (CV) test: the test voltage was -1.0 to -1.6 V, the potential scanning rate was -100 mv / s, and the measurement was repeated 3 times until the obtained curves overlapped.
[0054] (4) Linear cyclic voltammetry (LSV) test: the test voltage is -1.0 to 1.6 V, the potential scanning rate is -5 mv / s, and 3 sets of data are measured.
[0055] (5) Electrochemical impedance spectroscopy (EIS) test: The frequency range is 0.1 Hz to 100 kHz, the starting frequency is 100 kHz, the DC voltage is set to -1.2 V, and the AC voltage is set to 5 mV to test the electrochemical impedance performance of the catalyst at different frequencies.
[0056] (6) Electrochemical effective area test: The test voltage was -0.8 to -0.9 V, and the potential scanning rates were -10, -20, -30, -40, and -50 mv / s, from which the double layer capacitance was calculated.
[0057] Example 1
[0058] The method for confined growth of a metal / metal oxide protective layer on a perovskite surface is achieved by the following steps:
[0059] (1) Preparation of Sr with A-site defects by solid phase sintering process 0.9 Fe 0.81 Ta 0.09 Ni 0.1 O 3-δ Perovskite materials
[0060] SrCO3 (99.0%), Fe2O3 (99.0%), Ta2O5 (99.0%) and NiO (99.9%) were mixed in a stoichiometric ratio and then added with ethanol solvent. The mixture was ball-milled for 24 h. The obtained slurry was dried at 70 °C and the sieved powder was further calcined at 1250 °C for 5 h to form SrCO3 (99.0%). 0.9 Fe 0.81 Ta 0.09 Ni 0.1 O 3-δ The crushed sample was then subjected to high-energy ball milling in ethanol at 450 rpm for 2 h to reduce the particle size. After drying at 70 °C, the SFTN powder was ground and sieved (300 mesh) for subsequent reduction operations.
[0061] (2) Reduction process
[0062] In order to obtain the protective layer and metal nanoparticles with confined growth, 5% H2 (20 ml min -1 SFTN was treated with argon gas (balance). SFTN was reduced at 850 °C in a continuous mixed gas flow for 2 h, with a heating and cooling rate of 5 °C min -1After being taken out and sieved (300 mesh), a perovskite-based composite material with a surface confined growth metal / metal oxide protective layer was obtained, which was recorded as FeNi@SFTN-2h.
[0063] Example 2
[0064] The difference between this example and Example 1 is that the reduction time in step (2) is 1 h. The other steps and parameters are the same as those in Example 1, and are recorded as FeNi@SFTN-1h.
[0065] Example 3
[0066] The difference between this example and Example 1 is that the reduction time in step (2) is 3 h. The other steps and parameters are the same as those in Example 1, and are recorded as FeNi@SFTN-3h.
[0067] Example 4
[0068] The difference between this example and Example 1 is that the reduction time in step (2) is 4 h. The other steps and parameters are the same as those in Example 1. , denoted as FeNi@SFTN-4h
[0069] Example 5
[0070] The difference between this example and Example 1 is that the reduction time in step (2) is 5 h. The other steps and parameters are the same as those in Example 1, and are recorded as FeNi@SFTN-5h.
[0071] Example 6
[0072] The difference between this example and Example 1 is that no reduction treatment is performed in step (2). The other steps and parameters are the same as those in Example 1, and are denoted as SFTN.
[0073] The above reduction process was used to regulate the catalytic activity and stability of the perovskite-based catalyst material. As the reduction time increased, the catalytic activity of the sample reached an optimal value, and the stability of the catalyst was significantly improved. The specific results are shown in the attached figure.
[0074] Figure 1 XRD spectra of SFTN perovskite-based materials under different reduction times obtained in Examples 1-6, with PDF cards of standard perovskite and FeNi alloy listed for comparison. All samples maintain a cubic perovskite crystal structure. As the reduction time increases, the XRD spectrum moves to a smaller diffraction angle, and the sample undergoes lattice expansion and increases oxygen vacancies after reduction. After reduction, the typical characteristic peaks of FeNi3 appear, which means that FeNi alloy exists on the surface of the sample after reduction. In the presence of A-site defects, when the oxygen vacancy concentration reaches a sufficiently high value, stoichiometric reorganization will occur on the perovskite surface, causing the B-site metal to spontaneously diffuse outward. Limited by the accuracy of the instrument, the characteristic peaks of the sub-nanometer ultra-thin protective layer could not be detected.
[0075] Figure 2 The SEM images of SFTN perovskite-based materials prepared in Examples 1-6 at different reduction times. The surface of the unreduced SFTN is flat, and metal nanoparticles anchored on the surface are observed after reduction. As the reduction time increases, the metal particles partially aggregate, and eventually over-reduction causes holes to form on the substrate. More specifically, when the reduction is performed for 1-2 hours, more tiny metal particles appear on the surface, and a protective layer is formed between the metal particles and the substrate, and the protective layer is relatively flat, without large cracks and holes; and when the reduction treatment is continued, such as after 3-5 hours of reduction, the number of metal particles on the surface decreases, and larger cracks and holes gradually appear on the protective layer. The principle of this reaction process is that during the reduction process, the sample undergoes lattice expansion, accompanied by lattice oxygen overflow. These lattice oxygens will preferentially combine with the B-site metal element with a changed valence to form BO metal oxide, and then further reduced to metal nanoparticles that aggregate on the surface. In addition, due to long-term exposure to a reducing atmosphere, the average particle size of the metal particles (d m ) increased from 57.92 to 159.80nm( Figure 3 ). Excessive growth of particles will consume the metal oxide layer formed on the surface and even destroy the perovskite oxide substrate, forming holes and reducing the accessible specific surface area, which is not conducive to the catalytic reaction. The sample reduced for 2h has the best morphology.
[0076] Figure 4 Atomic-resolution images and EELS analysis of a cross-section of a 2h catalyst were taken using a spherical aberration-corrected transmission electron microscope. x The layer exists between the FeNi metal nanoparticles and the perovskite substrate, acting as a protective layer with a thickness of about 0.7nm. This protective layer limits the contact between the reactants and the products and catalysts during the reaction, effectively blocking the perovskite substrate from being affected by the harsh environment, which is beneficial to the stability of the perovskite-based materials during the catalytic process.
[0077] The present invention successfully confines and grows an ultra-thin (thickness <1nm) metal oxide protective layer on the surface of perovskite through reduction treatment, and metal nanoparticles are anchored on the surface of the protective layer. The surface morphology of the prepared perovskite-based composite material is observed by SEM, and the prepared sample is tested in conjunction with an electrochemical test method. The performance advantages and disadvantages shown by the obtained test curve can predict the optimal preparation process conditions. The perovskite-based composite material wrapped with a protective layer prepared under these conditions has good catalytic performance and stability, and the method successfully realizes stability experimental verification.
[0078] Specifically, the present invention preliminarily studies the surface morphology of the electron microscope photos of the oxide material prepared, and observes the flatness of the surface protective layer. Under some conditions, the surface of the material prepared is relatively flat and has no holes, which is inferred to have the best stability. Figure 2 In the verification experiment, the SFTN samples reduced for 0, 1, 2, 3, 4, and 5 hours were photographed by electron microscope respectively, and then at a magnification of 70000, it can be observed that under the reduction conditions of 1-2h, there are no cracks and holes on the surface; after 3h treatment, there are cracks with a width of 10-50nm on the surface, and the area of the cracks accounts for at least 80% of the total area; after 4h of reduction, there are still cracks with a width of 10-50nm on the surface, and they account for at least 80% of the total area; after 5h of reduction, there are holes and cracks on the surface at the same time, the hole diameter ranges from 600-1200nm, and the crack width is 10-50nm, both of which account for more than 80% of the total area. This is mainly because: before the reduction treatment, the perovskite oxide has a flat surface and distinct grain boundaries. After reduction, in the ABO3 structure of the perovskite, the B-site metal combines with the overflowing lattice oxygen to form a metal oxide layer, which serves as a protective layer. However, after a long period of reduction treatment, the metal oxide layer will be completely reduced to metal particles, and the B-site metal in the perovskite will be excessively missing, the ABO3 structure will collapse, and the surface will be reorganized, resulting in a morphology similar to corrosion, with cracks and holes.
[0079] Verify the above prediction process and verify the catalytic performance. Figure 5 The LSV curve of a shows that the HER catalytic performance of the sample shows a volcanic change trend with the increase of reduction time, first increasing and then decreasing. Pure carbon is selected as the blank control group to deduct the influence of background current. Under a certain current, the sample reduced for 2h has the lowest overpotential and the best performance. Figure 5 In the calculation of the Tafel slope of b, the Tafel slope of the sample reduced for 2h is the smallest, which has the fastest reaction kinetics. Figure 6 In the calculation of the double-layer capacitance, the slope of the curve obtained by the sample reduced for 2h is the largest, and the number of exposed active sites is the largest. Figure 7 In the electrochemical impedance spectroscopy, the sample reduced for 2h has the smallest charge transfer resistance, indicating that the charge transfer rate between the catalyst and the redox species is the fastest. Figure 8This is the HER stability performance test of electrolyzed water of Examples 1 and 6. The performance of the untreated sample showed serious performance degradation within the first 30 minutes of the test, while the sample reduced for two hours could still maintain the initial catalytic activity after 800 hours of performance testing, indicating that the presence of the protective layer is very effective in improving the stability of the catalytic performance of the perovskite-based material. In the technical solution of the present invention, it is necessary to achieve the technical effect based on this ultra-thin protective layer to protect the perovskite base material. The protective layer cannot be too thick, otherwise it will lead to the loss of the catalytic performance of the perovskite base material. Fig. 9 It is the TEM high-resolution image of Examples 1 and 6 after the HER stability performance test of electrolyzed water. There are no clear lattice fringes near the surface of SFTN, and amorphous diffraction rings and diffraction points can be observed simultaneously in the selected area electron diffraction pattern, indicating that the amorphous phase and the crystalline phase coexist. In contrast, no obvious amorphous layer was observed in the sample reduced for 2h, and the base diffraction points were very clear, indicating that the surface crystallinity of the sample after reduction for 2h remained good after a long period of testing. There are many alloy particles, the protective layer gradually becomes thinner, and the performance is improved. However, if the reduction is excessive, the protective layer is destroyed and the performance will deteriorate. From the above results, we can see that the method of the present invention can effectively improve the ion leaching and deactivation problems of perovskite catalysts in water. The integrity of the surface protective layer observed in SEM can be used to predict the catalytic performance of the material, which confirms the reliability of the determination method. It is very meaningful to study the use of perovskite materials in complex and harsh atmospheres.
Claims
1. A perovskite oxide catalytic material, characterized in that: include: Base oxide, protective layer and metal particles on the protective layer; The base oxide is a perovskite metal oxide having the general formula of ABO3, and the A-site element is a defect amount; The protective layer is a metal oxide layer with a thickness of 0.1-3nm; The metal particles are composed of one or more of the B-site elements.
2. The perovskite oxide catalytic material according to claim 1, characterized in that: In the photos of the perovskite oxide catalytic material obtained at a magnification of 50,000-100,000, the number of surface metal particles ranges from 20 to 200; the particle size ranges from 30 to 200 nm.
3. The perovskite oxide catalytic material according to claim 1, characterized in that: The A-site element of the perovskite metal oxide is selected from rare earth or alkali metal elements, such as Be, Mg, Ca, Sr, Ba, La, Ce, Cd, Pb or Bi; the B-site element of the perovskite metal oxide is selected from transition metal elements, such as Fe, Ni, Ti, Ta, Nb, Co, Mn, Al, Mo, Cu, Sc or Cr.
4. The perovskite oxide catalytic material according to claim 1, characterized in that: The chemical formula of the perovskite metal oxide in step 1 is Sr 0.9 Fe 0.81 Ta 0.09 Ni 0.1 O 3-δ ; The material of the protective layer is FeO x , the material of the metal particles is FeNi alloy.
5. The method for capping and growing a sub-nanometer protective layer on a perovskite oxide catalytic material according to claim 1 comprises the following steps: Step 1, based on the general formula of ABO3 perovskite metal oxides, metal oxide raw materials are mixed according to the stoichiometric ratio of A-site defects, and solid phase sintering is performed to form a phase; Step 2, treating the oxide obtained in step 1 under a reducing atmosphere, so that the transition metal element on the B position diffuses to the surface and is reduced, thereby obtaining a protective layer with a metal anchored on the surface.
6. The method according to claim 5, characterized in that The metal oxide raw materials are selected from SrCO3, Fe2O3, Ta2O5 and NiO; during the solid phase sintering process, the sintering parameters are 1000-1400°C for 1-20h.
7. The method according to claim 5, characterized in that In step 2, the atmosphere in the reduction step is pure hydrogen or an inert gas containing 1-99% hydrogen; the temperature of the reduction process is 500-1000° C. and the time is 1-5 hours.
8. Use of the perovskite oxide catalytic material according to claim 1 in hydrogen evolution reaction (HER) by water electrolysis.
9. The use according to claim 8, characterized in that: It also includes a method for predicting the catalytic performance of perovskite oxide materials, the steps comprising: step a, obtaining a perovskite oxide material with a metal protective layer obtained under different preparation conditions, and obtaining a surface SEM photograph; step b, based on the integrity of the material surface on the SEM photograph, taking the preparation conditions corresponding to the surface protective layer with the best flatness as the preparation conditions for the material with the best HER catalytic performance.
10. The use according to claim 9, characterized in that: The flatness is determined by the cracks and / or holes on the base oxide and the protective layer; when there is the least crack and / or hole area, it is determined to have the best flatness; the crack width is 10-100nm, and the hole diameter range is 200-2000nm; the different preparation conditions refer to different reduction reaction times.
Citation Information
Cited By
Perovskite type mixed conductor film with metal precipitated on surface, method for electrically driving in-situ precipitation of metal nanoparticles and application of perovskite type mixed conductor film
CN120082932A