Method for enlarging boron-doped monocrystalline silicon DZ clean area

By increasing the pulling speed and performing high-temperature heat treatment during the drawing process of boron-doped single crystal silicon, the problem of insufficient depth of DZ clean area in the prior art is solved, and a significant increase in the depth of DZ clean area and the maintenance of crystallization rate is achieved.

CN118880438APending Publication Date: 2024-11-01FERROTEC (NINGXIA) SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411039116.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to effectively increase the DZ clean zone depth of boron-doped single crystal silicon, and cannot meet the requirements of certain component processes for leakage and impurity adsorption.

Method used

By increasing the pulling speed after a predetermined distance in the equal diameter, pulling the crystal rod, increasing the temperature gradient, rolling and slicing, and then high-temperature heat treatment of the silicon wafer containing small-sized oxygen precipitation, diffusing oxygen and vacant positions, and dissolving small-sized oxygen Precipitate to form a DZ clean area with increased depth.

Benefits of technology

The depth of the DZ clean area is achieved by reaching more than 60μm, meeting the requirements of boron-doped single crystal silicon products, and improving the crystallization rate of the silicon wafer and the stability of the clean area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004971905680000011
    Figure HDA0004971905680000011
  • Figure HDA0004971905680000012
    Figure HDA0004971905680000012
  • Figure HDA0004971905680000021
    Figure HDA0004971905680000021
Patent Text Reader

Abstract

The invention provides a method for enlarging a boron-doped monocrystalline silicon DZ clean area, and relates to the technical field of semiconductor monocrystalline silicon crystal pulling, after equal-diameter preset distance, the pulling speed is increased, so that a crystal bar is pulled at the preset pulling speed, the temperature gradient is increased, small-size oxygen precipitation point locations in the obtained crystal bar to be barreled are increased, and the crystal bar to be barreled is reduced. Barreling, segmenting and slicing the crystal bar to be barreled to obtain a silicon wafer; according to the method, the silicon wafer containing many small-size oxygen precipitates is subjected to heat treatment, oxygen and vacancies are diffused at a high temperature, the concentration of the oxygen and vacancies on the surface of a silicon crystal is lower than the saturation degree, and the small-size oxygen precipitates are dissolved at the high temperature, so that the depth of a DZ clean area of the silicon wafer after heat treatment is increased, and the depth of the DZ clean area reaches 60 microns or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor single crystal silicon pulling, and in particular relates to a method for increasing a DZ clean zone of boron-doped single crystal silicon. Background Art

[0002] In the component manufacturing process, oxygen precipitates can absorb some unnecessary metal impurities (for example: Ni, Fe, Na, Ag and other fast-diffusing metals), but oxygen precipitates can only appear in areas far away from the surface of the silicon wafer, because if it appears in the component area, leakage current will be generated. Therefore, in order to control the formation of oxygen precipitates, the supersaturated diffusion of oxygen at high temperature is generally used to make its concentration on the surface of the silicon wafer lower than the saturation concentration, so as to produce a DZ clean area without oxygen precipitates, so as to play the role of isolating leakage and adsorbing impurities.

[0003] In the prior art, for example, the Chinese invention with application number 202211455602.7 discloses a method for adjusting the clean area of ​​a polished silicon wafer, specifically the first step: using Ar for furnace tube annealing to form BMD ablation and forming a uniform BMD core during the cooling process; the second step: using a rapid thermal treatment method, using H2 / Ar or O2 / Ar, and two-component or three-component gas in N2 for proportional adjustment, and undergoing rapid thermal treatment at 1100°C to 1300°C for 60s, with a cooling rate of 10 to 70°C / s, to form a vacancy and oxygen complex; the third step: using a polishing process to remove the rough surface or oxide layer caused by the rapid thermal treatment; the fourth step: sintering the polished silicon wafer through a BMD sintering process at a low temperature, and then measuring the BMD density using LST or corrosion method; the above-mentioned prior art realizes an annealed silicon wafer with a stable clean area width, and at the same time has the effect of eliminating COP, and the BMD density is E7 to E10ea / cm 3 , the DZ depth reaches 30-150 μm. The present invention provides a new method to increase the DZ clean area of ​​boron-doped single crystal silicon. Summary of the invention

[0004] In view of this, the present invention provides a method for increasing the DZ clean zone of boron-doped single crystal silicon.

[0005] The technical solution adopted by the present invention to solve its technical problem is: A method for increasing the DZ clean zone of boron-doped single crystal silicon comprises the following steps: S1: After the predetermined distance is equal to the diameter, the pulling speed is increased so that the crystal rod is pulled at the predetermined pulling speed to obtain the crystal rod to be rolled; S2: Rolling, segmenting and slicing the crystal rod to be rolled to obtain silicon wafers; S3: heat-treating the silicon wafer to obtain a heat-treated silicon wafer.

[0006] Preferably, in S1, the predetermined pulling speed is: 0.825 mm / min-1.075 mm / min.

[0007] Preferably, in S1, the equal diameter is predetermined to be 100 mm-200 mm.

[0008] Preferably, in S1, the furnace pressure is 5Kpa-5Kpa, and the inert gas flow rate is 40slm-80slm.

[0009] Preferably, in S1, the rotation speed of the crystal rod is 10 rpm-20 rpm, and the rotation speed of the crucible is 0.8 rpm-2.5 rpm.

[0010] Preferably, when S3 performs heat treatment on the silicon wafer, a predetermined temperature curve is used to treat the silicon wafer.

[0011] Preferably, the predetermined temperature ranges from 300°C to 1000°C.

[0012] Preferably, in S3, the gas used in the heat treatment is a mixture of nitrogen or hydrogen and dry oxygen.

[0013] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for increasing the DZ clean zone of boron-doped single crystal silicon. After a predetermined distance is reached, the pulling speed is increased so that the crystal rod is pulled at a predetermined pulling speed, and the temperature gradient is increased, so that the number of small-sized oxygen precipitation points in the obtained crystal rod to be rolled is increased, and the crystal rod to be rolled is rolled, segmented, and sliced ​​to obtain a silicon wafer; the silicon wafer containing many small-sized oxygen precipitations is heat-treated, oxygen and vacancies diffuse at high temperature, and their concentration on the surface of the silicon crystal is lower than saturation, and the small-sized oxygen precipitation is dissolved at high temperature, so that the depth of the DZ clean zone of the silicon wafer after the heat treatment is increased, and the depth of the DZ clean zone reaches more than 60μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A temperature profile is predetermined for heat treatment.

[0015] Figure 2 The following are the DZ depth detection result diagrams of Example 1, Comparative Example 1, and Comparative Example 2.

[0016] Figure 3 It is a result diagram of the crystallization rate of Example 1, Comparative Example 1, and Comparative Example 2.

[0017] In the figure: DryO2 refers to dry oxygen. DETAILED DESCRIPTION

[0018] The technical solutions and technical effects of the embodiments of the present invention are further described in detail below in conjunction with the accompanying drawings of the present invention.

[0019] A method for increasing the DZ clean zone of boron-doped single crystal silicon comprises the following steps: S1: After the predetermined distance is equal to the diameter, the pulling speed is increased so that the crystal rod is pulled at the predetermined pulling speed to obtain the crystal rod to be rolled; S2: Rolling, segmenting and slicing the crystal rod to be rolled to obtain silicon wafers; S3: heat-treating the silicon wafer to obtain a heat-treated silicon wafer.

[0020] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for increasing the DZ clean zone of boron-doped single crystal silicon. After a predetermined distance is reached, the pulling speed is increased so that the crystal rod is pulled at a predetermined pulling speed, and the temperature gradient is increased, so that the number of small-sized oxygen precipitation points in the obtained crystal rod to be rolled is increased, and the crystal rod to be rolled is rolled, segmented, and sliced ​​to obtain a silicon wafer; the silicon wafer containing many small-sized oxygen precipitations is heat-treated, oxygen and vacancies diffuse at high temperature, and their concentration on the surface of the silicon crystal is lower than saturation, and the small-sized oxygen precipitation is dissolved at high temperature, so that the depth of the DZ clean zone of the silicon wafer after the heat treatment is increased, and the depth of the DZ clean zone reaches more than 60μm.

[0021] Furthermore, in S1, the predetermined pulling speed is: 0.825mm / min-1.075mm / min. If the pulling speed is increased too high, it is easy to cause the crystal rod temperature to be too low and twist and deform, thereby affecting the crystallization rate of the crystal rod; if the pulling speed is set too low, the depth of the DZ clean zone cannot reach more than 60μm, which cannot meet the requirements of boron-doped single crystal silicon products.

[0022] Furthermore, in S1, the equal diameter is predetermined to be 100mm-200mm, and the pulling speed of the equal diameter head fluctuates greatly. The pulling speed is not easy to change randomly during the stabilization process, which affects the crystallization.

[0023] Furthermore, in S1, the furnace pressure is 5Kpa-5Kpa, and the inert gas flow rate is 40slm-80slm.

[0024] Furthermore, in S1, the rotation speed of the crystal rod is 10 rpm-20 rpm, and the rotation speed of the crucible is 0.8 rpm-2.5 rpm.

[0025] like Figure 1 As shown, further, when the silicon wafer is heat treated in S3, a predetermined temperature curve is used to treat the silicon wafer. In which: the silicon wafer is placed in a heat treatment furnace for heat treatment, and the temperature is raised and lowered according to the program segment, the time refers to the residence time, and the flow rate refers to the flow rate of the gas.

[0026] Furthermore, the predetermined temperature ranges from 300°C to 1000°C.

[0027] Furthermore, in S3, the gas used in the heat treatment is a mixture of nitrogen or hydrogen and dry oxygen.

[0028] The scheme of the present invention is introduced through the following embodiments and comparative examples. Embodiment 1:

[0029] S1: After the diameter is equal to 200 mm, the pulling speed is increased and the crystal rod is pulled at a pulling speed of 0.945 mm / min-1.045 mm / min, wherein: the furnace pressure is 5Kpa-5Kpa, the inert gas flow rate is 40slm-80slm, the crystal rod rotation speed is 10rpm-20rpm, and the crucible rotation speed is 0.8rpm-2.5rpm, to obtain the crystal rod to be rolled; S2: Rolling, segmenting and slicing the crystal rod to be rolled to obtain silicon wafers; S3: heat-treating the silicon wafer at a temperature such as Figure 1 As shown, a silicon wafer is obtained after heat treatment.

[0030] Comparative Example 1 In step S1, the pulling speed of the crystal rod is 0.4 mm / min-0.5 mm / min, and the other steps and parameters are the same as those in implementation 1.

[0031] Comparative Example 2 In step S1, the pulling speed of the crystal rod is 1.08 mm / min-1.1 mm / min, and the other steps and parameters are the same as those in implementation one.

[0032] The silicon wafers obtained in Example 1, Comparative Example 1 and Comparative Example 2 were tested for DZ clean area, and the results were as follows: Figure 2 As shown by Figure 2 It can be seen that compared with comparative example 1, after the pulling speed is increased in comparative example 2 and embodiment 1, the depth of the DZ cleaning zone of the silicon wafer is significantly improved, and the depth of the DZ cleaning zone at the center and 1 / 2R position of the silicon wafer in embodiment 1 is greater than the depth of the DZ cleaning zone at the edge of the silicon wafer.

[0033] Through the example 1, the comparative example 1 and the comparative example 2, the crystal rod is pulled, and the crystallization rate of the obtained crystal rod is as follows: Figure 3 As shown by Figure 3 It can be seen that the crystallization rate of Example 1 is not much different from that of Comparative Example 1. It can be seen that the crystallization rate of Example 1 is not affected after the pulling speed is increased. However, compared with Example 1, the crystallization rate of Comparative Example 2 is reduced. It can be seen that when the pulling speed is too high, the temperature of the crystal rod is too low and it twists and deforms, which reduces the crystallization rate of the crystal rod.

[0034] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.

Claims

1. A method for increasing the DZ clean zone of boron-doped single crystal silicon, characterized in that: The following steps are involved: S1: After the predetermined distance is equal to the diameter, the pulling speed is increased so that the crystal rod is pulled at the predetermined pulling speed to obtain the crystal rod to be rolled; S2: Rolling, segmenting and slicing the crystal rod to be rolled to obtain silicon wafers; S3: heat-treating the silicon wafer to obtain a heat-treated silicon wafer.

2. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 1, characterized in that: In S1, the predetermined pulling speed is: 0.825mm / min-1.075mm / min.

3. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 1 or 2, characterized in that: In S1, the equal diameter is predetermined to be 100 mm-200 mm.

4. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 1, characterized in that: In S1, the furnace pressure is 5Kpa-5Kpa, and the inert gas flow rate is 40slm-80slm.

5. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 1, characterized in that: In S1, the rotation speed of the crystal rod is 10 rpm-20 rpm, and the rotation speed of the crucible is 0.8 rpm-2.5 rpm.

6. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 1, characterized in that: When the S3 performs heat treatment on the silicon wafer, a predetermined temperature curve is used to treat the silicon wafer.

7. The method for increasing the DZ clean zone of boron-doped single crystal silicon according to claim 6, characterized in that: The predetermined temperature ranges from 300°C to 1000°C.