Two-dimensional transition metal disulfide material and preparation method thereof
Through the CVD method of induced domain-limited growth by multi-step CVD, the annealed Au foil and liquid phase precursor were used to solve the problem of difficulty in controlling the size and morphology in the preparation of two-dimensional transition metal dichalcogenide materials, and achieve high-quality The preparation of two-dimensional PtSe2 strips fully explored the application potential of materials.
Patent Information
- Application Number
- CN202410887554.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-01
AI Technical Summary
In the prior art, the two-dimensional transition metal dichalcogenide materials have problems such as small product size, difficult to control morphology and low crystal quality during the preparation process, especially the two-dimensional PtSe2 materials have not fully explored their application potential.
Using a multi-step chemical vapor deposition (CVD) method of induced confined domain growth, the annealed Au foil is used as the substrate to spin coating the liquid phase precursor and optimize the reactor size to achieve spatial confined domain and nucleation density. Control reduces the reactor size to avoid strong interlayer coupling and improves the crystal quality and morphological control of the product.
The controllable preparation of the ultra-thin 1T-PtSe2 strip with large size and high crystallization is achieved, solving the problems of small product domain size, difficult to control morphology and thickness, and low crystallization quality, and obtaining high-quality two-dimensional transition metal two Chronic acid material.
Smart Images

Figure CN118880451A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of two-dimensional material preparation, and in particular to a two-dimensional transition metal dichalcogenide material and a preparation method thereof. Background Art
[0002] Two-dimensional transition metal dichalcogenides are a new type of two-dimensional materials with wide applications in optics, electricity, magnetism and electrochemistry. At present, many two-dimensional transition metal dichalcogenides still have problems in controllable preparation. For example, two-dimensional PtSe 2 As a new material with great potential, most current studies have prepared it through mechanical exfoliation or heat-assisted conversion, which has problems such as small product domain size, difficult to control morphology and thickness, and low crystallization quality, and have failed to fully explore its application potential. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a two-dimensional transition metal dichalcogenide and a preparation method thereof.
[0004] In the first aspect, the preparation method of the two-dimensional transition metal dichalcogenide provided by the present invention includes: using the parallel arranged steps of the substrate to carry out directional induced growth in a narrow reaction space, specifically using annealed Au foil as the substrate, using a liquid precursor as the metal precursor, spin coating the liquid precursor onto the substrate, and using a multi-step induced confined growth CVD method to prepare a two-dimensional transition metal dichalcogenide material.
[0005] The multi-step induced confined growth CVD method proposed in the present invention can controllably prepare two-dimensional transition metal dichalcogenide materials, achieve spatial confinement by reducing the size of the reactor, and use liquid phase precursors to optimize the metal precursor concentration and nucleation density.
[0006] Preferably, the annealing time is not less than 25 h.
[0007] The present invention uses Au foil that has been annealed for a long time as a substrate to achieve large-scale, highly crystalline ultra-thin 1T-PtSe 2 Controllable preparation of strips.
[0008] Preferably, the annealing time is 25 to 30 h.
[0009] More preferably, the Au foil has a thickness of 40-60 μm, a length of 0.5-1.5 cm, and a width of 0.5-1.5 cm; and the annealing temperature is 1040-1070 °C.
[0010] In the present invention, by further optimizing the annealing conditions of the Au substrate, a large number of directional steps can be generated on the surface of the Au substrate, thereby better controlling the orientation of the product.
[0011] Preferably, the reaction container is a quartz tank, and the internal dimensions of the reaction container are 15-25 cm in length, 1-4 cm in width, and 1-4 cm in height; preferably, the internal dimensions are 20-22 cm in length and 2-2.2 cm in diameter.
[0012] In the present invention, by further optimizing the internal dimensions of the quartz tank required for the CVD reaction, spatial confinement can be achieved, thereby better controlling the growth rate of the product and making the nucleation sites evenly distributed.
[0013] Preferably, the concentration of the liquid precursor is 0.1-2 mg / mL, preferably 0.5-1 mg / mL.
[0014] More preferably, the liquid precursor is a soluble salt solution of a transition metal complex, preferably (NH 4 ) 2 PtCl 4 Aqueous solution; the amount of the liquid precursor is 10~30 μL, preferably 10~15 μL.
[0015] Preferably, the spin coating speed is 500-800 r / min.
[0016] More preferably, a solid powder comprising S, Se and Te is used as the non-metal precursor, and the mass of the non-metal precursor is not less than 800 mg, preferably 800-1500 mg.
[0017] In the present invention, the uniformity of the nucleation site distribution is further optimized by spin coating the liquid precursor.
[0018] Further preferably, the method for preparing the two-dimensional transition metal dichalcogenide comprises: 1) Substrate pretreatment: annealing the Au foil to obtain a substrate.
[0019] 2) Spin-coating a liquid precursor onto the substrate, placing a non-metallic precursor on the carrier gas inlet side of the reaction container, placing the substrate on the carrier gas outlet side, and preparing the substrate by a multi-step induced confined growth CVD method.
[0020] Preferably, the carrier gas is Ar / H 2 ; The carrier gas flow rate is 80~100 / 5~10 L / min, preferably 80 / 5 L / min; the heating temperature of the metal precursor is 200~450 ℃; the growth temperature is 700~850 ℃.
[0021] The present invention aims to prepare high-quality two-dimensional transition metal dichalcogenides. It adopts a multi-step induced confined growth CVD method, uses annealed Au foil as a substrate, and optimizes the precursor ratio, concentration and reactor size to achieve the controllable preparation of highly crystalline two-dimensional transition metal dichalcogenide strips.
[0022] In a second aspect, the present invention provides a two-dimensional transition metal dichalcogenide prepared by the method for preparing the two-dimensional transition metal dichalcogenide.
[0023] Preferably, the two-dimensional transition metal dichalcogenide material is MX 2 strip or film, wherein M is a transition metal element, X is S, Se and Te; preferably, the two-dimensional transition metal dichalcogenide material is PtSe 2 Strip; preferably, the thickness is 0.9~5 nm, the morphology is strip-shaped, and the domain size is 10×0.5~150×2 μm 2 , the crystallinity is single crystal.
[0024] The multi-step induced confined growth CVD method proposed in the present invention achieves spatial confinement by reducing the reactor size to avoid vertical stacking caused by strong interlayer coupling, and uses liquid precursors to optimize the metal precursor concentration and nucleation density. 2 The product is difficult to expand horizontally. Using Au foil that has been annealed for a long time as a substrate, large-scale, highly crystalline ultra-thin 1T-PtSe was achieved. 2 Controllable preparation of strips. Liquid metal precursor is used to reduce nucleation density and control the uniform distribution of nucleation sites. Se powder is used as a non-metallic precursor, and the product morphology is controlled by adjusting its dosage. Au foil is used as a substrate to achieve multi-step induced growth. Quartz tank is used as a reaction container to achieve spatial confinement. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 Schematic diagram of the preparation of two-dimensional transition metal dichalcogenides provided in an embodiment of the present invention; wherein (a) is a liquid precursor spin coating process, (b) is a quartz tank, and (c) is a CVD reaction. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] The multi-step induced confined growth CVD method provided in this embodiment ( Figure 1 ), including the following steps: (1) Substrate pretreatment to improve the irregular morphology of the product and utilize PtSe 2 The product is difficult to expand horizontally, so we cut 1×1 cm 2 Au foil (Alfa Aesar, 99.99%, 50 μm thick) was used as a substrate and annealed at 1060 °C for 25 h to obtain a flat and uniformly oriented Au substrate. The substrate used in the present invention is the key to synthesizing high-quality two-dimensional materials.
[0030] (2) Liquid precursor and spatial confinement. In order to accurately control the precursor concentration, reduce the nucleation density and reaction rate, 10 μL of low concentration (0.5 mg / mL) (NH 4 ) 2 PtCl 4 An aqueous solution of Alfa Aesar (99.9%) was used as a metal precursor and was spin-coated onto the Au substrate at a speed of 800 r / min to make it evenly distributed on the substrate surface. An excess of Se powder (Alfa Aesar, 99.5%, 800 mg) was selected as a non-metallic precursor and a quartz tank was used as a reaction container (size 20×5×1 cm 3 ), providing a narrow reaction space, strictly controlling the gas diffusion process and reaction rate, and achieving spatial confinement. 2 As carrier gas, the carrier gas flow rate was 80 / 5 L / min, and the reaction was carried out at 820 °C for 15 min to obtain a highly crystalline new two-dimensional 1T-PtSe 2 Strips.
[0031] Example 2
[0032] Same as Example 1, except that the concentration of the metal precursor was changed to 1 mg / mL.
[0033] Example 3
[0034] Same as Example 1, except that the size of the reaction vessel of the quartz tank is changed to 20×5×2 cm 3 .
[0035] Example 4
[0036] Same as Example 1, except that the amount of the non-metal precursor is changed to 500 mg.
[0037] Example 5
[0038] The same as Example 1, except that the substrate thickness is changed to 30 μm.
[0039] Example 6
[0040] Same as Example 1, except that the carrier gas flow rate is changed to 100 / 5 L / min.
[0041] Comparative Example 1
[0042] Preparation of two-dimensional PtSe by direct selenization 2 The Pt film can be selenized directly by evaporating Se in the solid phase and heating at 400 °C.
[0043] Comparative Example 2
[0044] Preparation of two-dimensional PtSe by mechanical exfoliation 2 . Adhesive tape was used to bond bulk PtSe 2 Peel off.
[0045] The two-dimensional transition metal dichalcogenides prepared in the above examples and comparative examples were tested.
[0046] Testing method: Optical microscopy, scanning electron microscopy, transmission electron microscopy and atomic force microscopy were used to characterize the prepared products.
[0047] Test results: Comparative Example 1 Direct selenization method can obtain large-area continuous PtSe 2 The film is polycrystalline, but the prepared film is polycrystalline with a domain size of about 40 nm. Comparative Example 2 The mechanical exfoliation method can prepare defect-free few-layer crystals, but the product morphology is random and difficult to control. The embodiments of the present invention can solve the above problems well. After analyzing the test results, the multi-step induced confined growth CVD method provided by each embodiment of the present invention can solve the problems of small product domain size, difficult to control morphology and thickness, and low crystal quality, and can control the preparation of high-quality two-dimensional transition metal dichalcogenide materials.
[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a two-dimensional transition metal dichalcogenide, characterized in that: include: Annealed Au foil is used as a substrate, a liquid precursor is used as a metal precursor, the liquid precursor is spin-coated onto the substrate, and a multi-step induced confined growth CVD method is used for preparation to obtain a two-dimensional transition metal dichalcogenide material.
2. The method for preparing a two-dimensional transition metal dichalcogenide according to claim 1, characterized in that: The annealing time is not less than 20 h; preferably, the annealing time is 25-30 h.
3. The method for preparing a two-dimensional transition metal dichalcogenide according to claim 2, characterized in that: The Au foil has a thickness of 40-60 μm, a length of 0.5-1.5 cm, and a width of 0.5-1.5 cm; and an annealing temperature of 1040-1070°C.
4. The method for preparing a two-dimensional transition metal dichalcogenide according to any one of claims 1 to 3, characterized in that: The reaction container is a quartz tank, and the internal dimensions of the reaction container are 15-25 cm in length, 1-4 cm in width, and 1-4 cm in height; preferably, the internal dimensions are 20-22 cm in length and 2-2.2 cm in diameter.
5. The method for preparing a two-dimensional transition metal dichalcogenide according to any one of claims 1 to 4, characterized in that: The concentration of the liquid precursor is 0.1-2 mg / mL.
6. The method for preparing a two-dimensional transition metal dichalcogenide according to claim 5, characterized in that: The liquid precursor is a soluble salt solution of a transition metal complex; the amount of the liquid precursor used is 10-30 μL.
7. The method for preparing a two-dimensional transition metal dichalcogenide according to claim 6, characterized in that: A solid powder comprising S, Se and Te is used as a non-metallic precursor, and the mass of the non-metallic precursor is not less than 800 mg, preferably 800-1500 mg.
8. The method for preparing a two-dimensional transition metal dichalcogenide according to any one of claims 1 to 7, characterized in that: include: 1) Substrate pretreatment: annealing the Au foil to obtain a substrate; 2) Spin-coating a liquid precursor onto the substrate, placing a non-metallic precursor on the carrier gas inlet side of the reaction container, placing the substrate on the carrier gas outlet side, and preparing the substrate by a multi-step induced confined growth CVD method; Preferably, the carrier gas is Ar / H2; the carrier gas flow rate is 80~100 / 5~10 L / min; the heating temperature of the non-metallic precursor is 200~450°C; and the growth temperature is 700~850°C.
9. The two-dimensional transition metal dichalcogenide prepared by the method for preparing the two-dimensional transition metal dichalcogenide according to any one of claims 1 to 8.
10. The two-dimensional transition metal dichalcogenide prepared by the method for preparing a two-dimensional transition metal dichalcogenide according to claim 9, characterized in that: The two-dimensional transition metal dichalcogenide material is a MX2 strip or film, wherein M is a transition metal element, and X is S, Se and Te.
Citation Information
Cited By
Preparation method of two-dimensional semiconductor phase platinum diselenide single crystal material
CN120099630A
A method for preparing a two-dimensional semiconductor phase platinum diselenide single crystal material
CN120099630B