High-transparency low-defect perovskite polycrystalline wafer, preparation method and direct X-ray detector
MAPbBr3 single crystals were prepared by solution growth method and high transparency, low defect perovskite polycrystalline wafers were prepared by low-temperature hot pressing method, which solved the problems of shape control and time-consuming in the existing technology, achieved high transparency and density, and improved The sensitivity and stability of the X-ray detector.
Patent Information
- Application Number
- CN202410909193.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
In the large-area application of the prior art, MAPbBr3 single crystal grown by solution method has problems such as difficult to control shape, time consumption and low raw material utilization. There are often residual pores in large-size perovskite wafers prepared by high-temperature hot pressing. and energy consumption and other defects.
The solution growth method is used to prepare MAPbBr3 single crystals, grind it into nano-scale powder, and then prepare high-transparent, low-defect perovskite polycrystalline wafers through low-temperature hot pressing method to control the hot pressing temperature, pressure and time to achieve orderly merging and assembly of grains , reduce grain boundaries and pores.
It improves the transparency and density of perovskite wafers, reduces the density of defect states, improves carrier mobility, and achieves high sensitivity, low detection limit and good stability in X-ray detectors.
Smart Images

Figure CN118880460A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-transparency, low-defect perovskite polycrystalline wafer, a preparation method and a direct X-ray detector, and belongs to the technical field of semiconductor photoelectric materials. Background Art
[0002] X-ray detectors are currently used in many fields, such as disease treatment and diagnosis in medicine, non-destructive testing of products in industry, as well as safety supervision, agricultural development, environmental protection and scientific research. Perovskite materials with excellent optoelectronic properties have shown great application potential in the field of X-ray detection. As the first single crystal perovskite material used in the light absorption layer of X-ray detectors, MAPbBr3 single crystals have advantages such as regular external shape and simple device structure, and the characteristics of high optical transmittance enable it to show better crystal quality and outstanding charge transfer performance. However, in terms of large-scale applications, MAPbBr3 single crystals grown by solution method have problems such as difficult shape control, time-consuming and low raw material utilization. At present, most of the large-size perovskite wafers prepared by hot pressing use high-temperature hot pressing of micron-sized perovskite powder, which will lead to defects such as residual pores and energy consumption in the wafer. Summary of the invention
[0003] In view of this, an object of the present invention is to provide a highly transparent and low-defect perovskite polycrystalline wafer, a preparation method and a direct X-ray detector.
[0004] To achieve the above objectives, the technical solution of the present invention is as follows.
[0005] A method for preparing a highly transparent and low-defect perovskite polycrystalline wafer, the method comprising the following steps:
[0006] (1) Preparation of MAPbBr3 single crystals by solution growth method;
[0007] (2) drying the MAPbBr3 single crystal and grinding it to obtain nanoscale MAPbBr3 powder;
[0008] (3) After the nanoscale MAPbBr3 powder is dried, it is placed in a hot pressing mold, the temperature is raised to 40-60°C at a heating rate of 2-5°C / min, and the temperature is maintained at 127-187 MPa for 3-5 hours to obtain a highly transparent and low-defect perovskite polycrystalline wafer.
[0009] Preferably, in step (1), methylammonium bromide (MABr) and lead bromide (PbBr2) powders are dissolved in N,N-dimethylformamide (DMF) to obtain a MAPbBr3 precursor solution, and the precursor solution is heated to 40-45°C and grown for 6-12 hours to obtain a MAPbBr3 single crystal.
[0010] Preferably, the molar ratio of MABr to PbBr2 is 1.25:1, and the concentration of the MAPbBr3 precursor solution is 1 to 1.2 mol / L.
[0011] Preferably, in step (2), the grinding time is 20 to 35 minutes.
[0012] Preferably, in step (2) and step (3), the drying temperature is 40 to 60° C. and the drying time is 4 to 10 hours.
[0013] Preferably, in step (3), the thickness of the polycrystalline wafer is 0.6 to 1 mm.
[0014] A highly transparent and low-defect perovskite polycrystalline wafer is prepared by the method.
[0015] A direct X-ray detector, wherein the perovskite layer of the detector adopts the high-transparency and low-defect perovskite polycrystalline wafer described in the present invention.
[0016] Preferably, the direct X-ray detector comprises a metal lower electrode, a hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer and a metal upper electrode which are arranged in sequence from bottom to top.
[0017] Preferably, the metal upper electrode and the metal lower electrode are Au, and the hole transport layer is molybdenum oxide (MoO x ), the electron transport layer is fullerene (C 60 ), the hole blocking layer is bathocuproin (BCP).
[0018] Beneficial Effects
[0019] The present invention provides a method for preparing a highly transparent and low-defect perovskite polycrystalline wafer. First, a solution growth method is adopted to prepare a MAPbBr3 single crystal. Then, the single crystal is ground to control the powder scale of the MAPbBr3 and reduce the powder size from the micron level to the nanometer level, thereby increasing the rate of evolution of the transparency of the perovskite wafer. Finally, the nanometer-level MAPbBr3 powder is hot-pressed and the temperature, pressure and time of the hot-pressing are controlled at the same time, thereby controlling the transition of the MAPbBr3 polycrystalline from opaque to transparent. The prepared wafer has a preferential crystal orientation, thereby realizing the orderly merging and assembly of grains. Driven by heat energy and pressure, the grain boundaries between the merged grains are fused to form larger grains, and the transparent MAPbBr3 wafer has a high degree of compactness.
[0020] The present invention provides a highly transparent and low-defect perovskite polycrystalline wafer. The structural phase purity of the prepared wafer can be ensured by grinding small-sized single crystals. Compared with the existing method of preparing wafers by hot pressing micron-sized perovskite powder at high temperature, the method of preparing wafers by hot pressing nano-sized perovskite powder at low temperature can quickly achieve the densification of the wafer, reduce the defect state density, and improve the quality of the wafer. The perovskite polycrystalline wafer prepared by this method has a carrier mobility equivalent to that of perovskite single crystal materials.
[0021] The present invention provides a direct X-ray detector, the sensitivity of which reaches 10 5 μC Gy air -1 cm -2 , the detection limit is low (149nGyair s -1 ), with a total dose of up to 5.9 Gyair under continuous X-ray irradiation, showing high uniformity and excellent stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Scanning electron microscope images of perovskite MAPbBr3 wafers prepared with different grinding times as described in Comparative Examples 1-2 and Example 1 of the present invention.
[0023] Figure 2 The scanning electron microscope images and grain size statistics of the perovskite MAPbBr3 polycrystalline wafers described in Comparative Examples 3-4 and Example 2 of the present invention.
[0024] Figure 3 This is a physical picture of the perovskite MAPbBr3 polycrystalline wafer described in Comparative Examples 3-4 and Example 2 of the present invention.
[0025] Figure 4 This is a sensitivity diagram of the perovskite MAPbBr3 polycrystalline chip X-ray detector described in Comparative Examples 3-4 and Example 2 of the present invention.
[0026] Figure 5 It is the light transmittance of the transparent perovskite MAPbBr3 polycrystalline wafer described in Example 2 of the present invention.
[0027] Figure 6 This is a performance diagram of the minimum detection limit of the transparent perovskite MAPbBr3 polycrystalline chip X-ray detector described in Example 2 of the present invention.
[0028] Figure 7 This is a performance diagram of the irradiation stability of the transparent perovskite MAPbBr3 polycrystalline chip X-ray detector described in Example 2 of the present invention.
[0029] Figure 8This is a sensitivity performance diagram of the perovskite MAPbBr3 polycrystalline chip X-ray detector according to Comparative Examples 5-6 and Example 2 of the present invention. DETAILED DESCRIPTION
[0030] The present invention will be further described in detail below in conjunction with specific embodiments.
[0031] Comparative Example 1
[0032] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0033] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0034] (3) Use tweezers to take out the MAPbBr3 single crystal and place it in an oven at 60°C for 6 hours.
[0035] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0036] (5) Weigh 1 g of the single crystal and put it into a grinding mortar. Grind it for 5 min to obtain MAPbBr3 powder.
[0037] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0038] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 4 h.
[0039] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm.
[0040] (9) The prepared wafers are tested for their surface morphology and particle size distribution, such as Figure 1 (a).
[0041] Comparative Example 2
[0042] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0043] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0044] (3) Use tweezers to take out the MAPbBr3 single crystal and place it in an oven at 60°C for 6 hours.
[0045] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0046] (5) Weigh 1 g of the single crystal and put it into a grinding mortar. Grind it for 15 min to obtain MAPbBr3 powder.
[0047] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0048] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 4 h.
[0049] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm.
[0050] (9) The prepared wafers are tested for their surface morphology and particle size distribution, such as Figure 1 (b).
[0051] Example 1
[0052] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0053] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0054] (3) Use tweezers to take out the MAPbBr3 single crystal and place it in an oven at 60°C for 6 hours.
[0055] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0056] (5) Weigh 1 g of the single crystal and put it into a grinding mortar. Grind it for 30 min to obtain nano-sized MAPbBr3 powder, as shown in the figure.
[0057] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0058] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 4 h.
[0059] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm.
[0060] (9) The prepared wafers are tested for their surface morphology and particle size distribution, such as Figure 1 (c).
[0061] Comparative Example 3
[0062] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0063] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0064] (3) Use tweezers to take out the MAPbBr3 single crystal, and place the taken out single crystal in an oven at 60°C for 6 hours.
[0065] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0066] (5) Weigh 1 g of the single crystal and put it into a grinding mortar and grind it for 30 min to obtain nano-sized MAPbBr3 powder.
[0067] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0068] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 5 min.
[0069] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm. The actual wafer is shown in the figure below. Figure 3 (a). Then, 20 nm of C was evaporated on the upper surface of the wafer. 60 As the electron transport layer, about 8 nm thick BCP as the blocking layer and 50 nm thick Au as the electrode.
[0070] (9) After completing step (8), the wafer is taken out and 10 nm thick MoO is sequentially evaporated on the lower surface of the wafer. x as the hole transport layer and 50 nm thick Au as the electrode.
[0071] (10) The surface morphology and grain distribution of the wafer were tested. Figure 2 (ab).
[0072] (10) The prepared device is tested for its X-ray sensitivity, such as Figure 4 (a).
[0073] Comparative Example 4
[0074] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0075] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0076] (3) Use tweezers to take out the MAPbBr3 single crystal, and place the taken out single crystal in an oven at 60°C for 6 hours.
[0077] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0078] (5) Weigh 1 g of the single crystal and put it into a grinding mortar and grind it for 30 min to obtain nano-sized MAPbBr3 powder.
[0079] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0080] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 1.5 h.
[0081] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm. The actual wafer is shown in the figure below. Figure 3 (b) Then, 20 nm of C was evaporated on the upper surface of the wafer. 60 As the electron transport layer, about 8 nm thick BCP as the blocking layer and 50 nm thick Au as the electrode.
[0082] (9) After completing step (8), the wafer is taken out and 10 nm thick MoO is sequentially evaporated on the lower surface of the wafer. x as the hole transport layer and 50 nm thick Au as the electrode.
[0083] (10) The surface morphology and grain distribution of the wafer were tested. Figure 2 (cd).
[0084] (11) The prepared device is tested for its X-ray sensitivity, such as Figure 4 (b).
[0085] Example 2
[0086] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0087] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0088] (3) Use tweezers to take out the MAPbBr3 single crystal, and place the taken out single crystal in an oven at 60°C for 6 hours.
[0089] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0090] (5) Weigh 1 g of the single crystal and put it into a grinding mortar and grind it for 30 min to obtain nano-sized MAPbBr3 powder.
[0091] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0092] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 50 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 50 °C, keep the temperature and press for 4 h.
[0093] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm. The actual wafer is shown in the figure below. Figure 3 (c) Then, 20 nm of C was evaporated on the upper surface of the wafer. 60 As the electron transport layer, about 8 nm thick BCP as the blocking layer and 50 nm thick Au as the electrode.
[0094] (9) After completing step (8), the wafer is taken out and 10 nm thick MoO is sequentially evaporated on the lower surface of the wafer. x as the hole transport layer and 50 nm thick Au as the electrode.
[0095] (10) The surface morphology and grain distribution of the wafer were tested. Figure 2 (ef), the light transmittance of the chip is Figure 5 .
[0096] (11) The prepared device was tested for its X-ray sensitivity, detection limit and irradiation stability, respectively. Figure 4 (c) Figure 6 and Figure 7 .
[0097] Comparative Example 5
[0098] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0099] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0100] (3) Use tweezers to take out the MAPbBr3 single crystal, and place the taken out single crystal in an oven at 60°C for 6 hours.
[0101] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0102] (5) Weigh 1 g of the single crystal and put it into a grinding mortar and grind it for 30 min to obtain nano-sized MAPbBr3 powder.
[0103] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0104] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 25 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 25 °C, keep the temperature and press for 4 h.
[0105] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm. Then, 20 nm of C 60 As the electron transport layer, about 8 nm thick BCP as the blocking layer and 50 nm thick Au as the electrode.
[0106] (9) After completing step (8), the wafer is taken out and 10 nm thick MoO is sequentially evaporated on the lower surface of the wafer. x as the hole transport layer and 50 nm thick Au as the electrode.
[0107] (10) The prepared device is tested for its X-ray detection sensitivity performance, such as Figure 8 (a).
[0108] Comparative Example 6
[0109] (1) First, weigh 2.0154 g of MABr and 5.2849 g of PbBr2 and dissolve them in 12 mL of DMF solvent, and stir and dissolve them at 900 rpm at room temperature to form a transparent perovskite MAPbBr3 precursor solution.
[0110] (2) Use a nylon filter with a diameter of 0.22 μm to filter out impurities from the perovskite MAPbBr3 precursor solution. Use a plastic wrap with small holes to seal the filtered solution, and place the glass bottle containing the solution in a 45°C oil bath for 12 hours.
[0111] (3) Use tweezers to take out the MAPbBr3 single crystal, and place the taken out single crystal in an oven at 60°C for 6 hours.
[0112] (4) Take the single crystal from step (3) out of the oven and cool it in an air environment for 20 minutes.
[0113] (5) Weigh 1 g of the single crystal and put it into a grinding mortar and grind it for 30 min to obtain nano-sized MAPbBr3 powder.
[0114] (6) Place the MAPbBr3 powder in a drying cabinet or hot plate and set the temperature to 60°C for 2 h.
[0115] (7) Place the dried MAPbBr3 powder in a hot pressing mold and flatten the powder in the mold. Then set the hot pressing pressure to 187 MPa, the hot pressing temperature to 100 °C, and the heating rate to 2 °C / min. After the temperature reaches the set temperature of 100 °C, keep the temperature and press for 4 h.
[0116] (8) After the wafer has cooled, use tweezers to remove the wafer with a diameter of 2 cm and a thickness of 1 mm. The actual wafer is shown in the figure below. Figure 3 (b) Then, 20 nm of C was evaporated on the upper surface of the wafer. 60 As the electron transport layer, about 8 nm thick BCP as the blocking layer and 50 nm thick Au as the electrode.
[0117] (9) After completing step (8), the wafer is taken out and 10 nm thick MoO is sequentially evaporated on the lower surface of the wafer. x as the hole transport layer and 50 nm thick Au as the electrode.
[0118] (10) The prepared device is tested for its X-ray detection sensitivity performance, such as Figure 8 (c).
[0119] See also Figure 1 The scanning electron microscope images of the perovskite MAPbBr3 wafers prepared in Comparative Examples 1-2 and Example 1 show that the powder obtained by extending the grinding time can produce denser wafers during the hot pressing process. Figure 2 , SEM images of perovskite MAPbBr3 wafers prepared at different hot pressing times in Comparative Examples 3-4 and Example 2. It can be seen from the figure that with the extension of hot pressing time, the average grain size of the prepared MAPbBr3 polycrystalline wafer gradually increases to a maximum of about 1μm, and the grain arrangement gradually becomes denser. Figure 3 These are the actual pictures of the perovskite MAPbBr3 wafer and the X-ray detector prepared in Comparative Examples 3-4 and Example 2. From Figures (ac), it can be found that as the hot pressing time increases, the transparent area of the wafer gradually expands, which is attributed to the growth of the grain size and the elimination of pores. Figure 4 The sensitivity of the X-ray detector of the perovskite MAPbBr3 polycrystalline wafer prepared based on different hot pressing times is shown in Comparative Examples 3-4 and Example 2. It can be seen from the figure that as the hot pressing time increases, the sensitivity of the perovskite MAPbBr3 polycrystalline wafer gradually increases, reaching 1.14×10 5 μC Gy air -1 cm-2 . See Figure 5 The light transmittance of the wafer in Example 2 is more than 60% in the wavelength range of 552-800nm. Figure 6 The lowest detection limit performance of the transparent perovskite MAPbBr3 wafer device in this embodiment 2 is 149nGy s at a signal-to-noise ratio of 3. -1 . See Figure 7 Example 2 shows the X-ray irradiation performance of the transparent perovskite MAPbBr3 chip device. After irradiation for about 12,500 seconds at an X-ray energy of 100 keV, the current of the device did not show obvious attenuation and the total cumulative dose was as high as 5.9 Gy, which is equivalent to 29,500 chest examinations. Figure 8 Comparative Examples 5-6 and Example 2 demonstrate the sensitivity of the perovskite MAPbBr3 polycrystalline chip X-ray detector prepared under different hot pressing temperature conditions. It can be seen from the figure that as the hot pressing temperature increases from room temperature to 50°C, the sensitivity of the perovskite MAPbBr3 polycrystalline chip gradually increases, but when the hot pressing temperature is further increased to 100°C, the sensitivity of the device begins to decrease.
[0120] In summary, the invention includes but is not limited to the above embodiments. Any equivalent substitution or partial improvement made under the spirit and principle of the invention shall be deemed to be within the protection scope of the invention.
Claims
1. A method for preparing a highly transparent and low-defect perovskite polycrystalline wafer, characterized in that: The method steps include: (1) Preparation of MAPbBr3 single crystals by solution growth method; (2) drying the MAPbBr3 single crystal and grinding it to obtain nanoscale MAPbBr3 powder; (3) After the nanoscale MAPbBr3 powder is dried, it is placed in a hot pressing mold, the temperature is raised to 40-60°C at a heating rate of 2-5°C / min, and the temperature is maintained at 127-187 MPa for 3-5 hours to obtain a highly transparent and low-defect perovskite polycrystalline wafer.
2. The method for preparing a highly transparent and low-defect perovskite polycrystalline wafer according to claim 1, characterized in that: In step (1), MABr and PbBr2 powders are dissolved in DMF to obtain a MAPbBr3 precursor solution, and the precursor solution is heated to 40-45° C. and grown for 6-12 hours to obtain a MAPbBr3 single crystal.
3. The method for preparing a highly transparent and low-defect perovskite polycrystalline wafer according to claim 2, characterized in that: The molar ratio of MABr to PbBr2 is 1.25:1, and the concentration of the MAPbBr3 precursor solution is 1-1.2 mol / L.
4. The method for preparing a highly transparent and low-defect perovskite polycrystalline wafer according to claim 1, characterized in that: In step (2), the grinding time is 20 to 35 minutes.
5. The method for preparing a highly transparent and low-defect perovskite polycrystalline wafer according to claim 1, characterized in that: In step (2) and step (3), the drying temperature is 40 to 60° C. and the drying time is 4 to 10 hours.
6. A method for preparing a highly transparent and low-defect perovskite polycrystalline wafer according to any one of claims 1 to 5, characterized in that: In step (3), the thickness of the polycrystalline wafer is 0.6 to 1 mm.
7. A highly transparent and low-defect perovskite polycrystalline wafer, characterized in that: It is prepared by the method according to any one of claims 1 to 6.
8. A direct X-ray detector, characterized in that: The perovskite layer of the detector adopts the high-transparency and low-defect perovskite polycrystalline wafer described in claim 7.
9. A direct X-ray detector as claimed in claim 8, characterized in that: The direct X-ray detector comprises a metal lower electrode, a hole transport layer, a perovskite layer, an electron transport layer, a hole blocking layer and a metal upper electrode which are arranged in sequence from bottom to top.
10. A direct X-ray detector as claimed in claim 8, characterized in that: The metal upper electrode and the metal lower electrode are Au, the hole transport layer is molybdenum oxide, the electron transport layer is fullerene, and the hole blocking layer is bathocuproin.
Citation Information
Cited By
Method for preparing complete mosaic-shaped barium strontium titanate solid solution ceramic sheet
CN118495943A
A method for preparing a complete mosaic-like barium strontium titanate solid solution ceramic sheet