Preparation method of high-purity low-oxygen gallium fluoride polycrystal
By reacting gallium oxide with ammonium hydrogen fluoride in a hydrothermal kettle and sublimating the treatment, the problems of high-purity gallium fluoride preparation and oxygen content control were solved, and high-purity low-oxygen gallium fluoride polycrystals were obtained, which improved the fluoride optical fiber. performance and preparation efficiency.
Patent Information
- Application Number
- CN202411113993.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult to prepare high-purity gallium fluoride crystals in the prior art, resulting in increased loss of fluoride fibers and less control of impurities anionic oxygen, which affects the quality and performance of the fibers.
In a hydrothermal kettle, gallium oxide reacts with excess ammonium hydrogen fluoride to prepare the crude product of gallium fluoride, and removes excess ammonia hydrogen fluoride by raising the temperature, and then reduces the oxygen content through sublimation operations to obtain high-purity low-oxygen gallium fluoride polycrystals.
The preparation of high-purity and low-oxygen gallium fluoride has been achieved, which has the characteristics of low pollution, high purity, few impurities and low oxygen content, and has improved the light transmittance and preparation efficiency of fluoride optical fibers.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of crystal preparation, and in particular relates to a method for preparing high-purity low-oxygen gallium fluoride polycrystal. Background Art
[0002] Fluoride optical fiber has extremely high light transmittance in the visible to mid-infrared band, and is the most promising ultra-low loss optical fiber material for long-distance base station-free communication. It has become a strategic key technology in the competition among major countries. Gallium fluoride is one of the important raw materials for fluoride optical fiber. Whether high-purity gallium fluoride crystals can be prepared is directly related to the loss of fluoride optical fiber.
[0003] However, the preparation of high-purity gallium fluoride is difficult. During the preparation process, problems such as incomplete fluorination and high impurity content in the product are prone to occur, making it impossible to obtain high-purity gallium fluoride, which further hinders the preparation of fluoride optical fibers and leads to increased losses in fluoride optical fibers. In order to solve this problem, researchers consciously began to control the content of impurity cations such as iron, copper, nickel, and cobalt during the preparation of gallium fluoride. However, few people paid attention to the control of impurity anions such as oxygen. However, in the preparation process of fluoride optical fibers, the control of impurity anions, especially oxygen, is particularly important. Excessive oxygen content will not only lead to low quality of the preform, but also cause the optical fiber to easily crystallize and increase losses.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a method for preparing high-purity low-oxygen gallium fluoride polycrystals, which has the advantages of being safe, convenient, efficient and easy to control.
[0006] The technical solution of the present invention is as follows: A method for preparing high-purity low-oxygen gallium fluoride polycrystal, comprising: Step 1, reacting gallium oxide and excess ammonium bifluoride in a hydrothermal kettle to obtain a crude gallium fluoride product, and then removing excess ammonium bifluoride in the crude gallium fluoride product by increasing the heating temperature of the hydrothermal kettle; Step 2: Subliming the gallium fluoride crude product after removing excess hydrogen fluoride and ammonia to obtain high-purity low-oxygen gallium fluoride polycrystals.
[0007] Optionally, the molar ratio of gallium oxide to ammonium bifluoride in step 1 is 1:(6-9).
[0008] Optionally, the reaction temperature in step 1 is 280-320° C., and the reaction time is 6-8 h.
[0009] Optionally, in step 1, the heating temperature of the hydrothermal reactor is increased to 680-750°C.
[0010] Optionally, the step 2 specifically includes: The gallium fluoride crude product after removing excess hydrogen fluoride and ammonia is placed in a crucible, the crucible is evacuated using a vacuum pump, and then filled with inert gas to a pressure of 10-120Kpa, followed by heat preservation at 900-1200°C for 12-24h, and finally cooled to obtain high-purity low-oxygen gallium fluoride polycrystals.
[0011] Optionally, the crucible is made of platinum.
[0012] Optionally, the pressure is 100 Kpa and the insulation temperature is 1200°C.
[0013] Optionally, the preparation method specifically comprises: Step 1, after gallium oxide and excess ammonium bifluoride are mixed uniformly in a molar ratio of 1:9, the mixture is placed in a hydrothermal kettle, the hydrothermal kettle is sealed, the hydrothermal kettle is heated to 300° C., reacted for 7 hours, and then naturally cooled to obtain a crude gallium fluoride product; then the excess ammonium bifluoride in the crude gallium fluoride product is removed by increasing the heating temperature of the hydrothermal kettle to 700° C. until no smoke is generated; Step 2: Put the crude gallium fluoride product after removing excess hydrogen fluoride and ammonia into a platinum crucible, use a vacuum pump to evacuate the platinum crucible, and then fill it with nitrogen to a pressure of 10Kpa, then heat it to 900°C at a rate of 20°C / min, keep it at 900°C for 12h, and finally turn off the heating device to cool to room temperature to obtain high-purity low-oxygen gallium fluoride polycrystals.
[0014] Compared with the prior art, the advantages of the present invention are: Gallium oxide and ammonium bifluoride react fully in the hydrothermal reactor, which can provide a high-pressure reaction environment for the fluorination reaction. Excess ammonium bifluoride can ensure that gallium oxide is more thoroughly fluorinated. Then, the excess ammonium bifluoride is removed by high temperature. Then, high-purity low-oxygen gallium fluoride polycrystals are obtained through sublimation operation.
[0015] The method of the invention prepares high-purity low-oxygen gallium fluoride polycrystals through a two-step process, and has the characteristics of low pollution, high purity, few impurities and low oxygen content. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0017] At present, it is difficult to prepare high-purity gallium fluoride. During the preparation process, problems such as incomplete fluorination and high impurity content in the product are prone to occur, making it impossible to obtain high-purity gallium fluoride, which further hinders the preparation of fluoride optical fibers and leads to increased loss of fluoride optical fibers. In order to solve this problem, researchers consciously began to control the content of impurity cations such as iron, copper, nickel, and cobalt during the preparation of gallium fluoride. However, few people paid attention to the control of impurity anions such as oxygen. However, in the preparation process of fluoride optical fibers, the control of impurity anions, especially oxygen, is particularly important. Excessive oxygen content will not only lead to low quality of the preform, but also cause the optical fiber to easily crystallize and increase loss.
[0018] Therefore, the present invention provides a method for preparing high-purity low-oxygen gallium fluoride crystals, wherein a crude gallium fluoride product is preliminarily synthesized by reacting gallium oxide and ammonium bifluoride in a hydrothermal reactor, and then high-purity gallium fluoride crystals are prepared by controlling the anion oxygen content through sublimation.
[0019] Specifically, an embodiment of the present invention provides a method for preparing high-purity low-oxygen gallium fluoride polycrystal, which comprises: Step 1, reacting gallium oxide and excess ammonium bifluoride in a hydrothermal reactor to obtain a crude gallium fluoride product; Step 2, removing excess hydrogen fluoride and ammonium in the gallium fluoride crude product by increasing the heating temperature of the hydrothermal reactor; Step 3: Subliming the gallium fluoride crude product after removing excess hydrogen fluoride and ammonia to obtain high-purity low-oxygen gallium fluoride polycrystals.
[0020] In the embodiment of the present invention, a gallium fluoride crude product is first prepared by reacting gallium oxide and excess ammonium bifluoride at low temperature, and then the excess ammonium bifluoride is removed at high temperature; and then the gallium fluoride crude product is sublimated by a sublimation device to reduce the impurity anion oxygen content in the gallium fluoride polycrystal. The preparation method of the embodiment of the present invention has the characteristics of low pollution, high purity, few impurities and low oxygen content.
[0021] In one embodiment, the molar ratio of gallium oxide to ammonium bifluoride in step 1 is 1:(6-9), such as 1:6, 1:7, 1:8, 1:9, etc. At this molar ratio, complete fluorination of gallium oxide can be ensured.
[0022] In one embodiment, the reaction temperature in step 1 is 280-320° C. (eg, 300° C.) and the reaction time is 6-8 hours (eg, 7 hours). Under this reaction condition ratio, it can be ensured that gallium oxide and ammonium bifluoride react fully.
[0023] In one embodiment, the hydrothermal reactor heating temperature in step 2 is increased to 680-750° C., such as 680° C., 690° C., 700° C., 710° C., 720° C., 730° C., 740° C., 750° C., etc. At this temperature, excess ammonium bifluoride can be effectively removed.
[0024] In one embodiment, the step 3 specifically includes: The gallium fluoride crude product after removing excess hydrogen fluoride and ammonia is placed in a crucible, and the crucible is evacuated using a vacuum pump, and then filled with inert gas to a pressure of 10-120Kpa (such as 10Kpa, 50Kpa, 100Kpa, 120Kpa, etc.), followed by heat preservation at 900-1200°C (such as 900°C, 1000°C, 1100°C, 1200°C, etc.) for 12-24h (such as 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc.), and finally cooled to obtain high-purity low-oxygen gallium fluoride polycrystals.
[0025] Through the above sublimation operation, the impurity anion oxygen content in the gallium fluoride polycrystal can be effectively reduced.
[0026] In one embodiment, the crucible is made of platinum. Using a platinum crucible instead of an ordinary alloy crucible can effectively avoid the introduction of excessive metal impurities. In addition, the growth characteristics of the crystal itself are conducive to eliminating other impurities, thereby obtaining a product with higher purity.
[0027] In one embodiment, the pressure is 100 KPa and the insulation temperature is 1200°C.
[0028] The present invention is described in detail below through specific embodiments.
[0029] Example 1 The method for preparing gallium fluoride polycrystal in this embodiment has the following specific steps: Raw material mixing: weigh 1 mol of gallium oxide and 9 mol of ammonium bifluoride, mix them evenly, put them into a hydrothermal kettle, cover it with a lid, and ensure that the system is sealed; Fluorination of gallium oxide: heat the hydrothermal autoclave to 300°C for 7 hours and then cool naturally to obtain a crude gallium fluoride product; Remove excess ammonium bifluoride: open the lid of the hydrothermal kettle, introduce high-purity nitrogen with a purity of 99.99%, and heat the hydrothermal kettle to 700°C until no smoke is produced; Sublimation crystallization: Place the crude gallium fluoride product after removing excess hydrogen fluoride and ammonia into a platinum crucible, evacuate it with a vacuum pump, and then fill it with high-purity nitrogen to normal pressure. Repeat this process twice, and finally fill it with high-purity nitrogen to a pressure of 10,000 Pa. Then heat it to 900°C at a rate of 20°C / min, keep it at 900°C for 12 hours, turn off the heating device, cool it to room temperature, and take out the gallium fluoride polycrystal from the platinum crucible.
[0030] Example 2-14 The preparation method of gallium fluoride polycrystals in Examples 2-14 is basically different from that in Example 1, except that the insulation temperature and pressure in the sublimation crystallization step are changed.
[0031] The oxygen content in the gallium fluoride polycrystals produced in Examples 1 to 14 was detected using a LECO ONH836 analyzer.
[0032] The parameters during sublimation crystallization of Example 1-14 and the oxygen content in the product gallium fluoride polycrystal are shown in Table 1 below: Table 1
[0033] It can be seen from Table 1 that low-oxygen gallium fluoride polycrystals are obtained through the preparation methods of Examples 1-14.
[0034] In summary, the present invention provides a method for preparing high-purity low-oxygen gallium fluoride polycrystals, which synthesizes a crude gallium fluoride product by a dry method, and then sublimates it in a high-temperature nitrogen atmosphere to obtain high-purity low-oxygen gallium fluoride polycrystals. Specifically, firstly, gallium oxide and excess ammonium bifluoride are used to synthesize a crude gallium fluoride product under low temperature conditions, and then the temperature is increased to remove excess ammonium bifluoride; then the crude gallium fluoride product is sublimated in a high-temperature nitrogen atmosphere to obtain high-purity low-oxygen gallium fluoride polycrystals. This method prepares high-purity low-oxygen gallium fluoride polycrystals by a two-step method, which has the characteristics of low pollution, high purity, few impurities, and low oxygen content.
[0035] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing high-purity low-oxygen gallium fluoride polycrystal, characterized in that: include: Step 1, reacting gallium oxide and excess ammonium bifluoride in a hydrothermal kettle to obtain a crude gallium fluoride product, and then removing excess ammonium bifluoride in the crude gallium fluoride product by increasing the heating temperature of the hydrothermal kettle; Step 2: Subliming the gallium fluoride crude product after removing excess hydrogen fluoride and ammonia to obtain high-purity low-oxygen gallium fluoride polycrystals.
2. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 1, characterized in that: The molar ratio of gallium oxide to ammonium bifluoride in step 1 is 1:(6-9).
3. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 1, characterized in that: The reaction temperature in step 1 is 280-320° C., and the reaction time is 6-8 hours.
4. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 1, characterized in that: In the step 1, the heating temperature of the hydrothermal reactor is increased to 680-750°C.
5. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 1, characterized in that: The step 2 specifically includes: The gallium fluoride crude product after removing excess hydrogen fluoride and ammonia is placed in a crucible, the crucible is evacuated using a vacuum pump, and then filled with inert gas to a pressure of 10-120Kpa, followed by heat preservation at 900-1200°C for 12-24h, and finally cooled to obtain high-purity low-oxygen gallium fluoride polycrystals.
6. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 5, characterized in that: The material of the crucible is platinum.
7. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 5, characterized in that: The pressure is 100 Kpa, and the insulation temperature is 1200°C.
8. The method for preparing high-purity low-oxygen gallium fluoride polycrystal according to claim 1, characterized in that: The preparation method specifically comprises: Step 1, after gallium oxide and excess ammonium bifluoride are mixed uniformly in a molar ratio of 1:9, the mixture is placed in a hydrothermal kettle, the hydrothermal kettle is sealed, the hydrothermal kettle is heated to 300° C., reacted for 7 hours, and then naturally cooled to obtain a crude gallium fluoride product; then the excess ammonium bifluoride in the crude gallium fluoride product is removed by increasing the heating temperature of the hydrothermal kettle to 700° C. until no smoke is generated; Step 2: Put the crude gallium fluoride product after removing excess hydrogen fluoride and ammonia into a platinum crucible, use a vacuum pump to evacuate the platinum crucible, and then fill it with nitrogen to a pressure of 10Kpa, then heat it to 900°C at a rate of 20°C / min, keep it at 900°C for 12h, and finally turn off the heating device to cool to room temperature to obtain high-purity low-oxygen gallium fluoride polycrystals.