Regenerated spandex fiber and preparation method thereof

By using crosslinking agents and reinforcement in the melt spinning process of regenerated spandex fibers, the problems of toxic solvent contamination and molecular chain breakage in the prior art are solved, and high-performance regenerated spandex fiber preparation is achieved, meeting global recycling standards and High temperature resistance and chemical resistance requirements.

CN118880488AActive Publication Date: 2024-11-01ZHEJIANG HUAFENG SPANDEX

Patent Information

Application Number
CN202411158409.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-01
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The dry spinning process used in the existing regenerated spandex process has the problem of toxic solvent contamination and molecular chain breakage during high-temperature melting, and it is difficult to meet global recycling standards and high-temperature and chemical resistance requirements.

Method used

Using melt spinning process, regenerated spandex fibers are prepared by recycling spandex reactions with crosslinking agents, mixed amines and reinforcers. The crosslinking agent is a polyurethane prepolymer, and the mixed amines are amine chain extenders and amine terminators, reinforcers. For silica, etc., it ensures that the spinning process is carried out under a weak alkaline environment and improves the high temperature and chemical resistance of the fibers.

Benefits of technology

100% raw material recycling has been achieved, no "three waste pollution" in the production process, and the fiber performance has reached the level of conventional non-recycled spandex, with good processing performance, high temperature and chemical resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a regenerated spandex fiber and a preparation method thereof, and the regenerated spandex fiber is prepared by the following steps: reacting recycled spandex, a cross-linking agent, mixed amine and a reinforcing agent to obtain a regenerated spinning material, and carrying out melt spinning on the regenerated spinning material to obtain the regenerated spandex fiber. The preparation method comprises the following steps: a polymerization step: carrying out crushing treatment and drying treatment on optional spandex components of spandex waste silk, spandex waste materials or waste fabrics to obtain recycled spandex; the drying treatment temperature is 90 to 200 DEG C; a spinning step: taking the regenerated spinning material as a raw material, and carrying out melt spinning, spinning and winding forming through a spinning assembly to obtain recycled spandex; the spinning temperature is 220 to 250 DEG C. The recycled spandex raw material is wide in source, the prepared regenerated spandex fiber is not only green, environment-friendly and pollution-free in raw material and good in process processing performance, but also high in product index and excellent in high temperature resistance and chemical resistance, and the performance level of a conventional melt spinning spandex fiber product can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of spandex recovery and reuse, and specifically relates to a regenerated spandex fiber and a preparation method thereof. Background Art

[0002] Green development of spandex is a general trend and is related to the core competitiveness of enterprises. All spandex production companies are actively expanding the field of recycled spandex. At present, there are a large number of patent technologies related to recycled spandex. For example:

[0003] Patent CN112538667A provides a method for regenerating spandex from spandex waste yarn, wherein the dried spandex waste yarn is mixed with a non-protonic polar solvent, and the mixture is heated and dissolved, and a spandex waste yarn solution is obtained after cooling, and the spandex waste yarn solution, prepolymer product and chain extender are used to prepare spandex spinning stock solution, and the solution is spun under nitrogen protection to obtain regenerated spandex. Patent CN110016730A mainly recycles aqueous spandex waste stock solution, which is suitable for producing spandex yarns with a denier of more than 140, and has high mechanical properties and resilience. Patent CN115182072A provides a method for regenerating spandex prepolymer waste liquid, wherein the spandex prepolymer waste liquid and mixed amine are subjected to chain extension reaction to obtain polyurethane urea stock solution A, and the polyurethane urea stock solution A is mixed with the normally produced polyurethane urea stock solution B, and the polyurethane urea elastic fiber is obtained by dry spinning after stirring and maturing.

[0004] The above-mentioned regenerated spandex process technologies are all based on dry spinning process, and the organic solvents used in the production process, such as DMAC, do not meet the requirements of the chemical part of the Global Recycling Standard (GRS). The regenerated spandex fiber prepared by the present invention adopts melt spinning, and its raw material recovery ratio can be as high as 100%, and no toxic solvents are used in the production process, and no "three wastes pollution" is generated, which fully meets the GRS certification requirements. In addition, the molecular chain breakage of the recycled spandex during the high-temperature melting process is easy to lead to poor subsequent spinning processing performance, insufficient product indicators, poor high temperature resistance and chemical resistance, etc. The present invention adds appropriate cross-linking agents and reinforcing agents in the melt spinning process, which well compensates for the defects of melt-spinning regenerated spandex. Summary of the invention

[0005] Technical problem: The purpose of the present invention is to solve the shortcomings of the current existing technology and provide a regenerated spandex fiber and a preparation method thereof, which uses recycled spandex as the main raw material, fully recycles and reuses waste spandex, and the regenerated spandex prepared by melt spinning has excellent performance, which is basically the same as the performance of conventional non-regenerated spandex and meets the use requirements.

[0006] Technical solution: A regenerated spandex fiber of the present invention comprises a regenerated spinning material obtained by reacting recycled spandex, a crosslinking agent, a mixed amine and a reinforcing agent, and the regenerated spinning material is melt-spun to obtain the regenerated spandex fiber.

[0007] The sources of the recycled spandex include one or more of spandex waste yarn, spandex waste material or spandex components of waste fabrics.

[0008] The crosslinking agent comprises a polyurethane prepolymer, which is an isocyanate-terminated polyurethane prepolymer obtained by reacting diisocyanate and polymer polyol; the crosslinking agent accounts for 1-10% of the total mass of the regenerated spandex fiber.

[0009] The NCO mass content of the terminal isocyanate polyurethane prepolymer is 2-6%.

[0010] The diisocyanate includes any one of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or dicyclohexylmethane diisocyanate, or a combination of at least two thereof, and diphenylmethane diisocyanate is more preferred.

[0011] The polymer polyol includes polyether polyol, and the polyether polyol includes any one of polytetramethylene ether glycol, polyethylene glycol or polypropylene glycol, or a combination of at least two of them.

[0012] The mixed amine includes an amine chain extender and an amine terminator; preferably, the molar ratio of the amine group in the mixed amine to the group reactive to the amine group in the cross-linking agent is 1.1:1 to 3:1, and the spinning process is in a weakly alkaline environment;

[0013] The amine chain extender includes a diamine having 2 to 30 carbon atoms, including one or more of ethylenediamine, propylenediamine, butylenediamine, pentylenediamine, methylpentylenediamine, methylpropylenediamine, hexylenediamine, phenylenediamine, phenylenediamine, diaminocyclohexane or hexamethylenediamine;

[0014] The amine terminator includes a monoamine with a carbon number of 2 to 20, including one or more of diethylamine, isopropylamine, n-butylamine, tert-butylamine, hexylamine, diethylamine, dimethylamine, di-n-butylamine, di-tert-butylamine, diisobutylamine, diisopropylamine, dipropylamine or cyclohexylamine or ethanolamine.

[0015] The molar ratio of the amine group of the amine chain extender to the amine group of the amine terminator is 10:1 to 30:1.

[0016] The reinforcing agent comprises one or more of silicon dioxide, hydrotalcite, silicon carbide, boron oxide or aluminum oxide; the reinforcing agent accounts for 0.5-3% of the total mass of the regenerated spandex fiber.

[0017] The preparation method of the regenerated spandex fiber of the present invention comprises the following steps:

[0018] Polymerization step: crushing and drying the spandex components of the optional spandex waste yarn, spandex waste material or waste fabric to obtain the recovered spandex; the drying temperature is 90-200°C;

[0019] The recycled spandex, crosslinking agent, mixed amine and reinforcing agent are uniformly mixed and fully reacted to obtain a regenerated spinning material; wherein the crosslinking agent accounts for 1 to 10% of the total mass of the regenerated spandex fiber; the reinforcing agent accounts for 0.5 to 3% of the total mass of the regenerated spandex fiber; the molar ratio of the amine group in the mixed amine to the group reactive to the amine group in the crosslinking agent is 1.1:1 to 3:1; the molar ratio of the amine group to the crosslinking agent makes the spinning process in a weakly alkaline state;

[0020] Spinning step: using the regenerated spinning material as raw material, performing melt spinning through a spinning assembly, spinning, winding and forming to obtain recycled spandex; the spinning temperature is 220-250°C.

[0021] Beneficial effects: The recycled spandex raw materials used in the present invention have a wide range of sources, including spandex waste yarn, spandex waste or spandex components of waste fabrics, which can be used as recycled spandex raw materials without complicated pretreatment. The regenerated spinning material obtained by compounding the recycled spandex with a specific crosslinking agent, a crosslinking agent, a mixed amine and a reinforcing agent can be directly melt-spun to prepare regenerated spandex fibers. The fibers are not only green and pollution-free raw materials, but also have good process performance, and the product indicators are strong, high temperature resistance and chemical resistance are excellent, which can reach the performance level of conventional melt-spun spandex fiber products. DETAILED DESCRIPTION

[0022] The regenerated spandex fiber comprises a regenerated spinning material obtained by reacting recycled spandex, a crosslinking agent, a mixed amine and a reinforcing agent, and is obtained by melt spinning the regenerated spinning material.

[0023] The sources of the recycled spandex include one or more of spandex waste yarn, spandex waste material or spandex components of waste fabrics;

[0024] The crosslinking agent includes a polyurethane prepolymer, and the polyurethane prepolymer is an isocyanate-terminated polyurethane prepolymer obtained by reacting a diisocyanate and a polymer polyol;

[0025] Preferably, the NCO mass content of the isocyanate-terminated polyurethane prepolymer is 2 to 6%;

[0026] Preferably, the diisocyanate includes any one of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or dicyclohexylmethane diisocyanate, or a combination of at least two thereof, and more preferably diphenylmethane diisocyanate;

[0027] Preferably, the polymer polyol includes a polyether polyol, and the polyether polyol includes any one or a combination of at least two of polytetramethylene ether glycol, polyethylene glycol or polypropylene glycol, and is more preferably polytetramethylene ether glycol;

[0028] In some embodiments of the present invention, the polyurethane prepolymer may also be directly recycled prepolymer, and the source of the recycled prepolymer includes waste terminal isocyanate polyurethane prepolymer generated in the preparation process of spandex;

[0029] The mixed amine includes an amine chain extender and an amine terminator;

[0030] The amine chain extender includes a diamine having 2 to 30 carbon atoms. Preferably, the diamine having 2 to 30 carbon atoms includes one or more of ethylenediamine, propylenediamine, butylenediamine, pentylenediamine, methylpentylenediamine, methylpropylenediamine, hexylenediamine, phenylenediamine, phenylenediamine, diaminocyclohexane or hexamethylenediamine.

[0031] The amine terminator includes a monoamine having 2 to 20 carbon atoms. Preferably, the monoamine having 2 to 20 carbon atoms includes one or more of diethylamine, isopropylamine, n-butylamine, tert-butylamine, hexylamine, diethylamine, dimethylamine, di-n-butylamine, di-tert-butylamine, diisobutylamine, diisopropylamine, dipropylamine, cyclohexylamine or ethanolamine;

[0032] In the present invention, the cross-linking agent and chain extender play a bridging role between the linear molecules of the original spandex during the reaction process, so that multiple linear molecules are bonded to each other to form a network structure to improve the comprehensive performance of the regenerated spandex.

[0033] The reinforcing agent includes one or more of silicon dioxide, hydrotalcite, silicon carbide, boron oxide or aluminum oxide;

[0034] In some examples of the present invention, the reinforcing agent has a nanometer particle size;

[0035] In the present invention, a proper amount of reinforcing agent is used to further improve the comprehensive performance of the regenerated spandex fiber.

[0036] The cross-linking agent accounts for 1 to 10% of the total mass of the regenerated spandex fiber;

[0037] The reinforcing agent accounts for 0.5-3% of the total mass of the regenerated spandex fiber;

[0038] The molar ratio of the amine group in the mixed amine to the group reactive to the amine group in the cross-linking agent is 1.1:1 to 3:1;

[0039] The molar ratio of the amine group of the amine chain extender to the amine group of the amine terminator is 10:1 to 30:1.

[0040] In the present invention, by controlling the slight excess of amine groups after the reaction, the spinning process is placed in a weakly alkaline environment, thereby inhibiting the precipitation and decomposition of impurities or additives in the recycled spandex at high temperature, such as the oil agent on the spandex waste yarn, thereby reducing the impact on the spinning system and improving the spinning stability.

[0041] The preparation method of recycled spandex comprises the following steps:

[0042] Polymerization step: uniformly mixing the recycled spandex, the cross-linking agent, the mixed amine and the reinforcing agent and fully reacting them to obtain the regenerated spinning material;

[0043] Wherein, the source of the recycled spandex includes one or more of spandex waste yarn, spandex waste material or spandex components of waste fabrics;

[0044] Preferably, the recovered spandex is pre-treated before the polymerization step;

[0045] The pre-treatment includes pulverizing and drying at least any one of the spandex waste yarn, spandex waste material or spandex component of waste fabric;

[0046] In some embodiments of the present invention, the pulverization process includes cutting the spandex waste yarn into spandex staple fibers of 5 to 10 mm, and cutting the spandex waste or spandex components of waste fabrics into particles of 5 to 10 mm;

[0047] The drying temperature is 90-200°C;

[0048] In some embodiments of the present invention, the polymerization step may use a screw extruder as a reactor. Specifically, the recycled spandex, crosslinking agent, mixed amine and reinforcing agent are added to the screw extruder for mixing reaction;

[0049] Wherein, the reaction temperature is 200-250°C.

[0050] Spinning step: using the regenerated spinning material as raw material, performing melt spinning through a spinneret assembly, and performing spinning and winding to obtain recycled spandex;

[0051] Wherein, the spinning temperature is 200-250°C.

[0052] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0053] Pretreatment of recycled spandex: crushing and drying at least one of the spandex waste yarn, spandex waste or spandex components of waste fabric;

[0054] The crushing process includes cutting the spandex waste yarn into spandex staple fibers of 5 to 10 mm, and cutting the spandex components of the spandex waste or waste fabric into particles of 5 to 10 mm;

[0055] The drying treatment includes drying the recycled spandex after the crushing treatment at 90-120° C. for 1-5 hours to obtain the pre-treated recycled spandex for standby use.

[0056] Example 1

[0057] 1200 kg of recycled spandex, 12.5 kg of cross-linking agent, 0.6 kg of mixed amine, and 6.5 kg of reinforcing agent are added to a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0058] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0059] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0060] The mixed amine is 0.5 kg of ethylenediamine and 0.1 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.24;

[0061] The reinforcing agent is silicon dioxide.

[0062] Example 2

[0063] 1100 kg of recycled spandex, 12 kg of cross-linking agent, 1.1 kg of mixed amine, and 6 kg of reinforcing agent were added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0064] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0065] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 4% obtained by reacting diphenylmethane diisocyanate with polytetramethylene ether glycol;

[0066] The mixed amine is 1 kg of ethylenediamine and 0.1 kg of diethylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.88;

[0067] The reinforcing agent is silicon dioxide.

[0068] Example 3

[0069] 1000 kg of recycled spandex, 15 kg of cross-linking agent, 1.1 kg of mixed amine, and 10 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0070] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0071] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3.5% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0072] The mixed amine is 1 kg of pentamethylenediamine and 0.1 kg of ethanolamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 2.75;

[0073] The reinforcing agent is silicon dioxide.

[0074] Example 4

[0075] 1000 kg of recycled spandex, 20 kg of cross-linking agent, 1.6 kg of mixed amine, and 30 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0076] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0077] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0078] The mixed amine is 1.5 kg of ethylenediamine and 0.1 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 2.19;

[0079] The reinforcing agent is hydrotalcite.

[0080] Example 5

[0081] 1200 kg of recycled spandex, 120 kg of cross-linking agent, 5.5 kg of mixed amine, and 7 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0082] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0083] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0084] The mixed amine is 5 kg of ethylenediamine and 0.5 kg of diethylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.26;

[0085] The reinforcing agent is silicon dioxide.

[0086] Example 6

[0087] 1000 kg of recycled spandex, 20 kg of cross-linking agent, 1.6 kg of mixed amine, and 35 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0088] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0089] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0090] The mixed amine is 1.5 kg of ethylenediamine and 0.1 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 2.19;

[0091] The reinforcing agent is hydrotalcite.

[0092] Example 7

[0093] 1200 kg of recycled spandex, 11 kg of cross-linking agent, 0.528 kg of mixed amine, and 6.5 kg of reinforcing agent were added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0094] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0095] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0096] The mixed amine is 0.44 kg of ethylenediamine and 0.088 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.24;

[0097] The reinforcing agent is silicon dioxide.

[0098] Example 8

[0099] 1200 kg of recycled spandex, 140 kg of cross-linking agent, 6.413 kg of mixed amine, and 7 kg of reinforcing agent were added to a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0100] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0101] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0102] The mixed amine is 5.83 kg of ethylenediamine and 0.583 kg of diethylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.26;

[0103] The reinforcing agent is silicon dioxide.

[0104] Example 9

[0105] 1200 kg of recycled spandex, 12.5 kg of cross-linking agent, 0.48 kg of mixed amine, and 6.5 kg of reinforcing agent were added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0106] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0107] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0108] The mixed amine is 0.4 kg of ethylenediamine and 0.08 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 0.99;

[0109] The reinforcing agent is silicon dioxide.

[0110] Example 10

[0111] 1200 kg of recycled spandex, 12.5 kg of cross-linking agent, 0.492 kg of mixed amine, and 6.5 kg of reinforcing agent were added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0112] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0113] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0114] The mixed amine is 0.41 kg of ethylenediamine and 0.082 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.02;

[0115] The reinforcing agent is silicon dioxide.

[0116] Embodiment 11

[0117] 1000 kg of recycled spandex, 15 kg of cross-linking agent, 1.32 kg of mixed amine, and 10 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0118] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0119] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3.5% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0120] The mixed amine is 1.2 kg of pentamethylenediamine and 0.12 kg of ethanolamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 3.30;

[0121] The reinforcing agent is silicon dioxide.

[0122] Comparative Example 1

[0123] 1200 kg of recycled spandex, 0.6 kg of mixed amine, and 6.5 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0124] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0125] The mixed amine is 0.5 kg of ethylenediamine and 0.1 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.24;

[0126] The reinforcing agent is silicon dioxide.

[0127] Comparative Example 2

[0128] 1200 kg of recycled spandex, 12.5 kg of cross-linking agent, and 6.5 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0129] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0130] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0131] The reinforcing agent is silicon dioxide.

[0132] Comparative Example 3

[0133] 1200 kg of recycled spandex and 6.5 kg of reinforcing agent are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0134] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0135] Wherein, the reinforcing agent is silicon dioxide.

[0136] Comparative Example 4

[0137] 1200 kg of recycled spandex, 12.5 kg of cross-linking agent, and 0.6 kg of mixed amine are added into a screw extruder through a mixing system for mixing and reaction to obtain a regenerated spinning material;

[0138] The material is melt-spun through a spinneret assembly, and the spinning and winding are performed to obtain recycled spandex;

[0139] The crosslinking agent is a polyurethane prepolymer having an NCO mass content of 3% obtained by reacting diphenylmethane diisocyanate and polytetramethylene ether glycol;

[0140] The mixed amine is 0.5 kg of ethylenediamine and 0.1 kg of cyclohexylamine, wherein the molar ratio of the amine group to the crosslinking agent NCO in the mixed amine is about 1.24.

[0141] The spandex fiber samples (40D) obtained in the above examples and comparative examples were subjected to the following performance tests, and the performance results are shown in Table 1 below:

[0142] Table 1:

[0143] performance SS300(gf) DS(gf) DE(%) Spinnability days / piece Example 1 10.5 46 48 15 Example 2 10.5 50 50 15 Example 3 10.8 55 54 12 Example 4 11.5 68 70 10 Example 5 10.5 46 48 2 Example 6 11.5 68 72 15 Example 7 10.2 44 46 20 Example 8 10 42 40 5 Example 9 10 44 40 25 Example 10 10.2 45 43 20 Embodiment 11 10.3 47 48 14 Comparative Example 1 10 40 40 45 Comparative Example 2 10.2 42 42 25 Comparative Example 3 9.8 38 40 50 Comparative Example 4 9 26 28 15 Conventional non-recycled melt-spun spandex 10.8 63 70 6

[0144] SS300: Indicates the stress when the product is stretched 300%.

[0145] High temperature resistance: The retention rate of tensile strength at break (DS) of the product after being subjected to 2.5 times stretching at 130°C for 40 minutes.

[0146] Alkali resistance: The retention rate of tensile strength at break (DS) of the product after being exposed to 25% alkalinity solution at 110℃ for 30 minutes.

[0147] SS300 and DS are tested in accordance with FZ / T 50006-2013 "Test Method for Tensile Properties of Spandex Yarn" using a microcomputer-controlled electronic universal testing machine.

[0148] Spinnability: Production line failures are summarized, and the average number of failures per 24 positions per day is calculated. If the number is less than or equal to 8, the spinnability is excellent; if the number is greater than 8 and less than 20, the spinnability is good; if the number is greater than 20 and less than 40, the spinnability is average; and if the number is greater than 40, the spinnability is poor.

Claims

1. A regenerated spandex fiber, characterized in that The method comprises the following steps: recovering spandex, a cross-linking agent, a mixed amine and a reinforcing agent to react to obtain a regenerated spinning material, and performing melt spinning on the regenerated spinning material to obtain regenerated spandex fibers.

2. The regenerated spandex fiber according to claim 1, characterized in that The sources of the recycled spandex include one or more of spandex waste yarn, spandex waste material or spandex components of waste fabrics.

3. The regenerated spandex fiber according to claim 1, characterized in that The crosslinking agent comprises a polyurethane prepolymer, which is an isocyanate-terminated polyurethane prepolymer obtained by reacting diisocyanate and polymer polyol; the crosslinking agent accounts for 1-10% of the total mass of the regenerated spandex fiber.

4. The regenerated spandex fiber according to claim 3, characterized in that The NCO mass content of the terminal isocyanate polyurethane prepolymer is 2-6%.

5. The regenerated spandex fiber according to claim 3, characterized in that: The diisocyanate includes any one of diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate or dicyclohexylmethane diisocyanate, or a combination of at least two thereof, and diphenylmethane diisocyanate is more preferred.

6. The regenerated spandex fiber according to claim 3, characterized in that: The polymer polyol includes polyether polyol, and the polyether polyol includes any one of polytetramethylene ether glycol, polyethylene glycol or polypropylene glycol, or a combination of at least two of them.

7. The regenerated spandex fiber according to claim 1, characterized in that: The mixed amine includes an amine chain extender and an amine terminator; the molar ratio of the amine group in the mixed amine to the group reactive to the amine group in the crosslinking agent is 1.1:1 to 3:1, and the spinning process is in a weakly alkaline environment; The amine chain extender includes a diamine having 2 to 30 carbon atoms, including one or more of ethylenediamine, propylenediamine, butylenediamine, pentylenediamine, methylpentylenediamine, methylpropylenediamine, hexylenediamine, phenylenediamine, phenylenediamine, diaminocyclohexane or hexamethylenediamine; The amine terminator includes a monoamine with a carbon number of 2 to 20, including one or more of diethylamine, isopropylamine, n-butylamine, tert-butylamine, hexylamine, diethylamine, dimethylamine, di-n-butylamine, di-tert-butylamine, diisobutylamine, diisopropylamine, dipropylamine or cyclohexylamine or ethanolamine.

8. The regenerated spandex fiber according to claim 7, characterized in that: The molar ratio of the amine group of the amine chain extender to the amine group of the amine terminator is 10:1 to 30:

1.

9. The regenerated spandex fiber according to claim 1, characterized in that: The reinforcing agent comprises one or more of silicon dioxide, hydrotalcite, silicon carbide, boron oxide or aluminum oxide; the reinforcing agent accounts for 0.5-3% of the total mass of the regenerated spandex fiber.

10. A method for preparing regenerated spandex fiber as claimed in claim 1, characterized in that: The method comprises the following steps: Polymerization step: crushing and drying the spandex components of the optional spandex waste yarn, spandex waste material or waste fabric to obtain the recovered spandex; the drying temperature is 90-200°C; The recycled spandex, crosslinking agent, mixed amine and reinforcing agent are uniformly mixed and fully reacted to obtain a regenerated spinning material; wherein the crosslinking agent accounts for 1 to 10% of the total mass of the regenerated spandex fiber; the reinforcing agent accounts for 0.5 to 3% of the total mass of the regenerated spandex fiber; the molar ratio of the amine group in the mixed amine to the group reactive to the amine group in the crosslinking agent is 1.1:1 to 3:1; the molar ratio of the amine group to the crosslinking agent makes the spinning process in a weakly alkaline state; Spinning step: using the regenerated spinning material as raw material, performing melt spinning through a spinning assembly, spinning, winding and forming to obtain recycled spandex; the spinning temperature is 220-250°C.

Citation Information

Patent Citations

  • Method for regenerating normalization spandex fibre from dry spinning spandex waste silk

    CN101096781A

  • Method for producing high resilience spandex fibers through waste spandex filaments

    CN102965758A

  • Preparation method of high-resilience low-draft differential melt-spun polyurethane filament

    CN104593883A

  • Method for regenerating spandex from spandex waste fibers

    CN112538667A

  • Method of making article from recoverable fabric

    CN116472152A

Cited By

  • Regenerated spandex fiber based on electron beam activation and intelligent crosslinking and preparation method thereof

    CN121826925A

  • Recyclable regenerated TPU spandex fiber and preparation method thereof

    CN121976319A