Composite fiber with skin-core structure and preparation method thereof

By modifying the skin core structure composite spinning of high-density polyethylene slices and PA6 slices, combined with hygroscopic thermal conductivity fillers, the problem of poor hygroscopicity of existing cool fibers is solved, and the excellent mechanical, flame retardant and thermal conductivity of the composite fibers are achieved. Simplified production process.

CN118880489APending Publication Date: 2024-11-01ANHUI YUANMENG BIO BASED MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410992624.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing cool fibers have poor hygroscopicity, resulting in complex production and high cost, making it difficult to achieve excellent thermal conductivity and flame retardant properties.

Method used

Modified high-density polyethylene slices are used as the cortical material, combined with PA6 slices as the core material, and composite spinning through the leather core structure, hygroscopic thermal filler is introduced to improve thermal conductivity and flame retardant properties, and through specific process steps and material ratios Optimized, enhances the mechanical properties of the fiber and moisture-absorbing and sweating.

Benefits of technology

The composite fibers have good mechanical properties, flame retardant properties and high contact coolness coefficients, while improving thermal conductivity and hygroscopic thermal conductivity, reducing production complexity and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959270720000111
    Figure BDA0004959270720000111
Patent Text Reader

Abstract

The invention discloses a skin-core structure composite fiber and a preparation method thereof, and belongs to the technical field of composite fibers.The preparation method comprises the following steps that modified high-density polyethylene slices serve as skin layer raw materials to prepare melt, then the melt is conveyed to a spinning manifold and then distributed into a skin-core composite assembly to serve as a skin layer component, and the skin-core composite fiber is obtained; preparing a melt by taking the dry PA6 slice as a core layer raw material, conveying the melt into a spinning manifold, and then distributing the melt into a skin-core composite component to serve as a core layer component; the skin layer component and the core layer component pass through a skin-core spinning composite assembly according to the mass ratio of-70: (30-40) and are uniformly extruded and formed, and the skin-core structure composite fiber is obtained through side air blowing cooling, oiling, heating drafting and winding and has good mechanical performance, the contact cool feeling coefficient is high, and the flame retardant property is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite fibers, and in particular relates to a composite fiber with a core-skin structure and a preparation method thereof. Background Art

[0002] In recent years, with the continuous development of society, people's living standards have gradually improved. People are no longer simply meeting the simple needs of food, clothing, housing and transportation, but are moving towards a more environmentally friendly, healthy and comfortable direction. Therefore, composite fibers such as conductive fibers, flame retardant fibers, antibacterial fibers, and cool fibers have been vigorously developed. Among them, cool fibers refer to fibers that can produce an instant cool feeling when in contact with the human body, and at the same time have additional functions such as absorbing sweat and quickly evaporating water. The resulting fabrics can effectively alleviate people's unbearable summer heat, thereby prompting people to increase the temperature of the air conditioner to achieve the purpose of reducing energy consumption and reducing emissions.

[0003] For example, China's patent authorization announcement number CN112481720B announced a preparation method and application of PE cool fiber, which uses high-density polyethylene slices as the skin material and low-melting-point polyester as the core material. The obtained fiber has a cool feeling due to the thermal conductivity and hydrophobicity of high-density polyethylene. However, due to poor hygroscopicity, it is necessary to co-spin with hydrophilic fibers to prepare cool fabrics. The co-spinning process is more complicated than the spinning process of a single fiber, and it is necessary to accurately control the ratio of the two fibers, the spinning speed, the tension and other parameters. The co-spinning process may involve more equipment and steps, which invisibly increases the production cost and the difficulty of operation. Therefore, providing a skin-core structure composite fiber with hygroscopic and thermal conductivity is a technical problem that needs to be solved at present. Summary of the invention

[0004] The object of the present invention is to provide a core-sheath structure composite fiber and a preparation method thereof, so as to solve the problem that the existing cool feeling fiber has poor performance.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a sheath-core structure composite fiber comprises the following steps:

[0007] S1, drying the PA6 slices at a temperature of 85-90°C and a vacuum degree of -0.1MPa for 12 hours to obtain dry PA6 slices;

[0008] S2, adding modified high-density polyethylene chips as the raw material for the skin layer into the first screw extruder, melting and extruding into a melt, and then conveying the melt to the spinning box body, the spinning box temperature is 265°C, passing through a pre-filter, and evenly distributed to the skin-core composite component as the skin layer component;

[0009] S3, adding the dried PA6 slices as the core layer raw material into the second screw extruder, melting and extruding into a melt, and then conveying the melt to the spinning box body, the spinning box temperature is 273 ° C, passing through the pre-filter, and evenly distributed to the skin-core composite component as the core layer component;

[0010] S4. The skin layer component and the core layer component are uniformly extruded through a skin-core type spinning composite assembly with a skin / core mass ratio of 70 / 30-60 / 40, and then subjected to side wind cooling, oiling, heating and stretching, and winding to obtain a skin-core structure composite fiber.

[0011] Furthermore, the temperature of the first screw extruder is 256-262° C., and the screw speed is 25 r / min.

[0012] Furthermore, the temperature of the second screw extruder is 265-272° C., and the screw speed is 48 r / min.

[0013] Furthermore, the preparation process of the modified high-density polyethylene slice is as follows:

[0014] The high-density polyethylene and the hygroscopic and thermally conductive filler are uniformly mixed in a mass ratio of 80-90:10-20 and then transferred to a twin-screw extruder for melt extrusion and granulation at a temperature of 120-170° C. to obtain modified high-density polyethylene chips.

[0015] Furthermore, the hygroscopic thermally conductive filler is a thermally conductive powder pretreated by grafting 11-mercaptoacylphosphorylcholine.

[0016] Furthermore, the pretreated thermally conductive powder is vinyltrimethoxysilane modified thermally conductive powder.

[0017] Further, the hygroscopic thermal conductive filler is prepared by the following steps:

[0018] The pretreated thermal conductive powder was added into tetrahydrofuran, and after ultrasonic dispersion for 1 hour, 11-mercaptoacylphosphorylcholine and benzoin dimethyl ether were added, and after stirring for 10-20 minutes, the powder was placed under ultraviolet light for reaction for 30-60 minutes. After the reaction was completed, the powder was filtered, and the filter cake was washed with anhydrous ethanol and dried to obtain a hygroscopic thermal conductive filler.

[0019] Furthermore, the dosage ratio of the pretreated thermally conductive powder, tetrahydrofuran, 11-mercaptoacylphosphorylcholine and benzoin dimethyl ether is 10g:100-200mL:2.5-5g:0.1g. Under the action of a photoinitiator, a thiol-ene click reaction is caused between the C=C bond on the surface of the pretreated thermally conductive powder and the -SH of 11-mercaptoacylphosphorylcholine, thereby introducing a phosphorylcholine structure carrying a long alkyl chain on the surface of the pretreated thermally conductive powder to obtain a hygroscopic thermally conductive filler.

[0020] Furthermore, the wavelength of the ultraviolet lamp is 250-450nm and the power is 15W.

[0021] Further, the pre-treated thermally conductive powder is prepared by the following steps:

[0022] Add thermal conductive powder and anhydrous ethanol into a flask, add formic acid to adjust the pH value to 3-6, ultrasonically disperse for 1 hour, stir at 65°C for 1 hour, then add vinyltrimethoxysilane ethanol solution, keep warm and stir to react for 3-5 hours. After the reaction is completed, filter, wash the filter cake with deionized water, and dry to obtain pretreated powder.

[0023] Furthermore, the amount of vinyltrimethoxysilane used is 1-2% of the mass of the thermally conductive powder.

[0024] Furthermore, the thermally conductive powder is a mixture of nano-scale mica powder and nano-scale aluminum nitride powder in a mass ratio of 2-3:1.

[0025] A composite fiber with a core-skin structure is made by the above-mentioned preparation method.

[0026] Beneficial effects of the present invention:

[0027] In order to improve the heat absorption and thermal conductivity of existing cool fibers, the present invention provides a sheath-core structured composite fiber, which uses modified high-density polyethylene chips as the sheath layer raw material and PA6 chips as the core layer raw material for sheath-core composite spinning. PA6 has excellent hygroscopic and mechanical properties, and the modified high-density polyethylene chips have good thermal conductivity, flame retardant properties, and moisture absorption and moisture conductivity. Ultimately, the obtained composite fiber not only has good mechanical properties, but also has a high contact coolness coefficient and good flame retardant properties.

[0028] The invention uses high-density polyethylene and hygroscopic thermally conductive filler as raw materials to prepare modified high-density polyethylene slices. The introduction of organic matter on the surface of the hygroscopic thermally conductive filler significantly improves its dispersibility in the high-density polyethylene, reduces the agglomeration between the thermally conductive powders, increases the compatibility of the thermally conductive powders with the high-density polyethylene, reduces interface defects, and enables the thermally conductive powders to form a thermally conductive path in the high-density polyethylene. In addition, by compounding two thermally conductive powders, the thermally conductive powders with small particle sizes are distributed between the powders with large particle sizes, which is beneficial to reducing the thermal resistance of the thermally conductive path, facilitating the conduction of heat, and improving the high The thermal conductivity of high-density polyethylene; in addition, the organic matter on the surface of the hygroscopic thermal conductive filler contains nitrogen, silicon, phosphorus, and sulfur flame retardant elements. The introduction of these flame retardant elements improves the flame retardant properties of the composite fiber; more importantly, the phosphorylcholine group on the surface of the hygroscopic thermal conductive filler carries both positive and negative charges due to the presence of quaternary ammonium and phosphate groups, and has a strong ability to bind water. Therefore, introducing it into high-density polyethylene is beneficial to improving the hydrophilicity of high-density polyethylene, thereby enhancing the hygroscopic and thermal conductive properties of the composite fiber, thereby enabling the composite fiber to play a good moisture absorption and perspiration function. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the following examples and comparative examples:

[0031] PA6 chips: spinning grade, melting point 220 °C, relative viscosity 2.75, white, purchased from Yongrong Holding Group (Jinjiang Technology);

[0032] High-density polyethylene: Fushun Petrochemical 2911, PetroChina Fushun Petrochemical Company;

[0033] Nano-grade mica powder: Lingshou County Dongxin Mineral Products Processing Plant;

[0034] Nano-grade aluminum nitride powder: Bangrui New Material Technology Co., Ltd.

[0035] Example 1

[0036] A hygroscopic thermally conductive filler is prepared by the following steps:

[0037] 10 g of the pretreated thermally conductive powder was added to 100 mL of tetrahydrofuran, and after ultrasonic dispersion for 1 h, 2.5 g of 11-mercaptoacylphosphorylcholine and 0.1 g of benzoin dimethyl ether were added. After stirring for 10 min, the mixture was placed under an ultraviolet lamp for reaction for 30 min. The wavelength of the ultraviolet lamp was 250 nm and the power was 15 W. The mixture was filtered, and the filter cake was washed with anhydrous ethanol and then dried to obtain a hygroscopic thermally conductive filler.

[0038] Pre-treated thermally conductive powder is made by the following steps:

[0039] 10 g of thermal conductive powder and 100 mL of anhydrous ethanol were added to a flask, formic acid was added to adjust the pH value to 3, ultrasonic dispersion was performed for 1 h, and stirring was performed at 65 °C for 1 h. Then, a solution consisting of 0.1 g of vinyltrimethoxysilane and 5 mL of anhydrous ethanol was added, and the mixture was stirred and reacted for 3 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed with deionized water and dried to obtain a pretreated powder. The thermal conductive powder was a mixture of nano-mica powder and nano-aluminum nitride powder in a mass ratio of 2:1.

[0040] Example 2

[0041] A hygroscopic thermal conductive filler is prepared by the following steps:

[0042] 10 g of the pretreated thermally conductive powder was added to 200 mL of tetrahydrofuran, and after ultrasonic dispersion for 1 h, 5 g of 11-mercaptoacylphosphorylcholine and 0.1 g of benzoin dimethyl ether were added. After stirring for 20 min, the mixture was placed under an ultraviolet lamp for reaction for 60 min. The wavelength of the ultraviolet lamp was 450 nm and the power was 15 W. The mixture was filtered, and the filter cake was washed with anhydrous ethanol and then dried to obtain a hygroscopic thermally conductive filler.

[0043] Pre-treated thermally conductive powder is made by the following steps:

[0044] 10 g of thermal conductive powder and 100 mL of anhydrous ethanol were added to a flask, formic acid was added to adjust the pH value to 6, ultrasonic dispersion was performed for 1 h, and stirring was performed at 65 °C for 1 h. Then, a solution consisting of 0.2 g of vinyltrimethoxysilane and 5 mL of anhydrous ethanol was added, and the mixture was stirred and reacted for 5 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed with deionized water and dried to obtain a pretreated powder. The thermal conductive powder was a mixture of nano-scale mica powder and nano-scale aluminum nitride powder in a mass ratio of 3:1.

[0045] Comparative Example 1

[0046] A pre-treated thermally conductive powder is prepared by the following steps:

[0047] 10 g of thermal conductive powder and 100 mL of anhydrous ethanol were added to a flask, formic acid was added to adjust the pH value to 3, ultrasonic dispersion was performed for 1 h, and stirring was performed at 65 °C for 1 h. Then, a solution consisting of 0.1 g of vinyltrimethoxysilane and 5 mL of anhydrous ethanol was added, and the mixture was stirred and reacted for 3 h. After the reaction was completed, the mixture was filtered, and the filter cake was washed with deionized water and dried to obtain a pretreated powder. The thermal conductive powder was a mixture of nano-mica powder and nano-aluminum nitride powder in a mass ratio of 2:1.

[0048] Comparative Example 2

[0049] A pretreated thermally conductive powder. Compared with the preparation method of comparative example 1, the thermally conductive powder is entirely nano-grade mica powder, and the remaining raw materials and preparation process are the same as those of comparative example 1.

[0050] Comparative Example 3

[0051] A pretreated thermally conductive powder. Compared with the preparation method of comparative example 1, the thermally conductive powder is entirely nano-grade aluminum nitride powder, and the remaining raw materials and preparation process are the same as those of comparative example 1.

[0052] Example 3

[0053] A method for preparing a sheath-core structure composite fiber comprises the following steps:

[0054] S1, drying the PA6 slices at a temperature of 85°C and a vacuum degree of -0.1MPa for 12 hours to obtain dried PA6 slices;

[0055] S2, adding modified high-density polyethylene chips as the raw material for the skin layer into the first screw extruder, and molten extruding into a melt, the temperature of the first screw extruder is: 250°C in the first zone, 260°C in the second zone, 262°C in the third zone, and 262°C in the fourth zone, and the screw speed is 25r / min. The melt is then transported to the spinning box body, and the spinning box temperature is 265°C. After passing through the pre-filter, it is evenly distributed to the skin-core composite component as the skin layer component;

[0056] S3, adding the dried PA6 slices as the core layer raw material into the second screw extruder, and molten extruding into a melt, the temperature of the second screw extruder is: 265°C in the first zone, 270°C in the second zone, 272°C in the third zone, and 272°C in the fourth zone, the screw speed is 48r / min, and then the melt is transported to the spinning box body, the spinning box temperature is 273°C, and passed through the pre-filter, and evenly distributed to the skin-core composite component as the core layer component;

[0057] S4. The skin layer component and the core layer component are passed through a sheath-core type spinning composite assembly and uniformly extruded into a sheath / core mass ratio of 70 / 30. After side wind cooling, oiling (using the 10wt% concentration of the liquid in Example 1 of the authorization publication number CN112481720B as the oiling liquid), heating and stretching, and winding, a sheath-core structure composite fiber is obtained.

[0058] The modified high-density polyethylene slice preparation process is as follows:

[0059] High-density polyethylene and the hygroscopic and thermally conductive filler of Example 1 were evenly transferred to a twin-screw extruder in a mass ratio of 90:10, and melt-extruded and granulated to obtain modified high-density polyethylene chips. The temperature of the twin-screw extruder was 120°C in zone 1, 150°C in zone 2, 160°C in zone 3, 160°C in zone 4, 160°C in zone 5, 160°C in zone 6, 160°C in zone 7, 160°C in zone 8, 160°C in zone 9, and 170°C in zone 10, and the screw speed was 50 rpm.

[0060] Crosswind conditions: wind speed 0.4m / s, wind temperature 20℃, relative humidity 70%; oil application rate: 2.0%.

[0061] Spinning speed: 4200m / min.

[0062] The heating and drawing process is performed by two hot roller drawing processes. The temperature of the first hot roller drawing process is 60°C and the speed is 800m / min; the temperature of the second hot roller drawing process is 90°C.

[0063] The winding speed is 2500m / min.

[0064] Example 4

[0065] A method for preparing a sheath-core structure composite fiber comprises the following steps:

[0066] S1, drying the PA6 slices at a temperature of 88°C and a vacuum degree of -0.1MPa for 12h to obtain dried PA6 slices;

[0067] S2, adding modified high-density polyethylene chips as the raw material for the skin layer into the first screw extruder, and molten extruding into a melt, the temperature of the first screw extruder is: 250°C in the first zone, 260°C in the second zone, 262°C in the third zone, and 262°C in the fourth zone, and the screw speed is 25r / min. The melt is then transported to the spinning box body, and the spinning box temperature is 265°C. After passing through the pre-filter, it is evenly distributed to the skin-core composite component as the skin layer component;

[0068] S3, adding the dried PA6 slices as the core layer raw material into the second screw extruder, and molten extruding into a melt, the temperature of the second screw extruder is: 265°C in the first zone, 270°C in the second zone, 272°C in the third zone, and 272°C in the fourth zone, the screw speed is 48r / min, and then the melt is transported to the spinning box body, the spinning box temperature is 273°C, and passed through the pre-filter, and evenly distributed to the skin-core composite component as the core layer component;

[0069] S4. The skin layer component and the core layer component are passed through a sheath-core type spinning composite assembly and uniformly extruded into a sheath / core mass ratio of 65 / 35. After side wind cooling, oiling (using the 10wt% concentration of the liquid in Example 1 of the authorization publication number CN112481720B as the oiling liquid), heating and stretching, and winding, a sheath-core structure composite fiber is obtained.

[0070] The modified high-density polyethylene slice preparation process is as follows:

[0071] The high-density polyethylene and the hygroscopic and thermally conductive filler of Example 2 were mixed evenly in a mass ratio of 85:15 and then transferred to a twin-screw extruder for melt-extrusion granulation to obtain modified high-density polyethylene chips. The temperatures of zone 1 of the twin-screw extruder were 120°C, zone 2 was 150°C, zone 3 was 160°C, zone 4 was 160°C, zone 5 was 160°C, zone 6 was 160°C, zone 7 was 160°C, zone 8 was 160°C, zone 9 was 160°C, zone 10 was 170°C, and the screw speed was 50rpm.

[0072] Crosswind conditions: wind speed 0.5m / s, wind temperature 23℃, relative humidity 75%; oiling rate: 2.4%.

[0073] Spinning speed: 4250m / min.

[0074] The heating and stretching process is performed by two hot roller stretchings. The temperature of the first hot roller stretching is 65°C and the speed is 1000m / min; the temperature of the second hot roller stretching is 100°C.

[0075] The winding speed is 3500m / min.

[0076] Example 5

[0077] A method for preparing a sheath-core structure composite fiber comprises the following steps:

[0078] S1, drying the PA6 slices at 90°C and vacuum degree -0.1MPa for 12h to obtain dried PA6 slices;

[0079] S2, adding modified high-density polyethylene chips as the raw material for the skin layer into the first screw extruder, and molten extruding into a melt, the temperature of the first screw extruder is: 250°C in the first zone, 260°C in the second zone, 262°C in the third zone, and 262°C in the fourth zone, and the screw speed is 25r / min. The melt is then transported to the spinning box body, and the spinning box temperature is 265°C. After passing through the pre-filter, it is evenly distributed to the skin-core composite component as the skin layer component;

[0080] S3, adding the dried PA6 slices as the core layer raw material into the second screw extruder, and molten extruding into a melt, the temperature of the second screw extruder is: 265°C in the first zone, 270°C in the second zone, 272°C in the third zone, and 272°C in the fourth zone, the screw speed is 48r / min, and then the melt is transported to the spinning box body, the spinning box temperature is 273°C, and passed through the pre-filter, and evenly distributed to the skin-core composite component as the core layer component;

[0081] S4. The skin layer component and the core layer component are passed through a sheath-core type spinning composite assembly and uniformly extruded into a sheath / core mass ratio of 60 / 40. After side wind cooling, oiling (using the 10wt% concentration of the liquid in Example 1 of Publication No. CN112481720B as the oiling liquid), heating and stretching, and winding, a sheath-core structure composite fiber is obtained.

[0082] The modified high-density polyethylene slice preparation process is as follows:

[0083] The high-density polyethylene and the hygroscopic and thermally conductive filler of Example 2 were mixed evenly in a mass ratio of 80:20 and transferred to a twin-screw extruder for melt-extrusion granulation to obtain modified high-density polyethylene chips. The temperatures of zone 1 of the twin-screw extruder were 120°C, zone 2 was 150°C, zone 3 was 160°C, zone 4 was 160°C, zone 5 was 160°C, zone 6 was 160°C, zone 7 was 160°C, zone 8 was 160°C, zone 9 was 160°C, zone 10 was 170°C, and the screw speed was 50rpm.

[0084] Crosswind conditions: wind speed 0.6m / s, wind temperature 25℃, relative humidity 80%; oiling rate: 2.6%.

[0085] Spinning speed: 4300m / min.

[0086] The heating and stretching process is performed by two hot roller stretchings. The temperature of the first hot roller stretching is 70°C and the speed is 1200 m / min; the temperature of the second hot roller stretching is 110°C.

[0087] The winding speed is 3900m / min.

[0088] Comparative Example 4

[0089] A method for preparing a composite fiber with a skin-core structure. Compared with Example 3, the hygroscopic and thermally conductive filler in Example 3 is replaced by the material in Comparative Example 1, and the remaining raw materials and preparation process are the same as in Example 3.

[0090] Comparative Example 5

[0091] A method for preparing a composite fiber with a skin-core structure. Compared with Example 3, the hygroscopic and thermally conductive filler in Example 3 is replaced by the material in Comparative Example 2, and the remaining raw materials and preparation process are the same as in Example 3.

[0092] Comparative Example 6

[0093] A method for preparing a composite fiber with a skin-core structure. Compared with Example 3, the hygroscopic and thermally conductive filler in Example 3 is replaced by the material in Comparative Example 3, and the remaining raw materials and preparation process are the same as Example 3.

[0094] The composite fibers prepared in Examples 3-5 and Comparative Examples 4-6 were subjected to the following steps: yarn guide - feeding roller - hot box - cooling plate - false twister - output roller - oiling to obtain the final finished product of sheath-core composite DTY yarn. Hot box temperature: 140°C; cooling temperature: 85°C; D / Y ratio: 1.2; drafting multiple: 1.25; oiling rate: 1.5%.

[0095] The performance tests were conducted on the sheath-core composite DTY yarns obtained in Examples 3-5 and Comparative Examples 4-6:

[0096] (1) According to GB / T14344-2008 "Test Method for Tensile Properties of Chemical Fiber Filaments", the mechanical properties test was carried out with a filament clamping distance of 500 mm, a tensile speed of 500 mm / min, and a pre-tension of 0.05±0.005 cN / detx. The elongation at break and the breaking strength of the test fiber were tested. Each sample was tested more than ten times and the average value was taken;

[0097] (2) Each group of sheath-core composite DTY yarns was humidified at 20°C and 60% humidity for 24 h, a certain mass of fiber was weighed and recorded as m0, and then placed in a vacuum oven at 90°C for 12 h, and the recorded mass was taken out and weighed as m1. The moisture regain R of the fiber was calculated according to the formula: R = (m0-m1) / m1×100%;

[0098] (3) The combustion behavior of the fiber was tested according to JI SL1091-1999. The fiber was made into a sample with a length of 15 cm, a width of 1.2 cm, and a thickness of 1 cm. The fire source was removed after 12 seconds of ignition, the combustion condition was observed, and the afterburning time was recorded;

[0099] (4) According to FZ / T 50048-2020 "Test method for instantaneous coolness of chemical fiber filaments on contact", the contact coolness coefficient of each group of sheath-core composite DTY yarns was tested.

[0100] The test results are shown in Table 1:

[0101] Table 1

[0102]

[0103] It can be seen from the data recorded in Table 1 that, compared with Comparative Examples 4-6, the core-skin structure composite fibers prepared in Examples 3-5 have better mechanical properties, flame retardant properties and coolness to touch.

[0104] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0105] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a core-skin structure composite fiber, characterized in that: The following steps are involved: S1, preparing a melt using modified high-density polyethylene chips as a raw material for the skin layer, conveying the melt to a spinning manifold, and then distributing the melt to a skin-core composite assembly as a skin layer component; S2, preparing a melt using dried PA6 slices as the core layer raw material, conveying the melt to a spinning manifold, and then distributing it to a skin-core composite assembly as a core layer component; S3, the skin layer component and the core layer component are uniformly extruded through a skin-core type spinning composite assembly according to a mass ratio of -70:30-40, and then subjected to side wind cooling, oiling, heating, drawing, and winding to obtain a skin-core structure composite fiber; The modified high-density polyethylene slices are obtained by melt extrusion granulation of high-density polyethylene and hygroscopic heat-conductive filler in a mass ratio of 80-90:10-20.

2. The method for preparing a core-skin structure composite fiber according to claim 1, characterized in that: The hygroscopic heat-conductive filler is a heat-conductive powder pretreated by grafting 11-mercaptoacylphosphorylcholine.

3. The method for preparing a core-skin structure composite fiber according to claim 1, characterized in that: The pretreated thermally conductive powder is vinyltrimethoxysilane modified thermally conductive powder.

4. The method for preparing a core-skin structure composite fiber according to claim 1, characterized in that: Hygroscopic thermally conductive fillers are made by the following steps: The pretreated thermally conductive powder is added to tetrahydrofuran, ultrasonically dispersed for 1 hour, and then 11-mercaptoacylphosphorylcholine and benzoin dimethyl ether are added. After stirring for 10-20 minutes, the powder is placed under an ultraviolet lamp for reaction for 30-60 minutes to obtain a hygroscopic thermally conductive filler.

5. The method for preparing a core-skin structure composite fiber according to claim 4, characterized in that: The dosage ratio of the pretreated thermal conductive powder, tetrahydrofuran, 11-mercaptoacylphosphorylcholine and benzoin dimethyl ether is 10g: 100-200mL: 2.5-5g: 0.1g.

6. The method for preparing a core-skin structure composite fiber according to claim 4, characterized in that: Pre-treated thermally conductive powder is made by the following steps: Add thermal conductive powder and anhydrous ethanol into a flask, add formic acid to adjust the pH value to 3-6, ultrasonically disperse for 1 hour, stir at 65°C for 1 hour, then add vinyltrimethoxysilane ethanol solution, keep warm and stir for 3-5 hours to obtain pretreated powder.

7. The method for preparing a core-skin structure composite fiber according to claim 6, characterized in that: The amount of vinyltrimethoxysilane used is 1-2% of the mass of the thermal conductive powder.

8. The method for preparing a core-skin structure composite fiber according to claim 6, characterized in that: The thermal conductive powder is a mixture of nano-scale mica powder and nano-scale aluminum nitride powder in a mass ratio of 2-3:

1.

9. A method for preparing a core-skin structure composite fiber, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8.