Degradation-controllable polypropylene film split filament
By using a combination of polypropylene waste and photoinitiator in the polypropylene film filament, controllable aging and intensity reduction under different light conditions are achieved, the problem of difficult aging of traditional polypropylene monofilaments is solved, and crop harvesting is improved Convenience and recycling efficiency.
Patent Information
- Application Number
- CN202411359648.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional polypropylene monofilament is not easy to age during crop growth, resulting in insufficient binding strength and needs to be cut manually during harvesting, which has low recycling efficiency and is prone to damage equipment, affecting mechanized operations.
The core structure of polypropylene film filament is adopted. The inner layer is polypropylene waste material, and the outer layer contains photoinitiator and polyethylene wax. Free radicals are formed under different light conditions through photoinitiator, resulting in aging and fracture of the polypropylene molecular chain. Achieve controllable strength reduction for easy harvesting and recycling.
The binding strength and aging speed of polypropylene film filaments are improved, the preparation cost is reduced, the recycling and utilization of polypropylene waste is increased, the harvesting process is simplified, the recycling efficiency is improved, and the equipment is protected.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention generally relates to the field of monofilament technology, and more particularly to a conductive monofilament and a preparation method thereof. Background Art
[0002] According to the characteristics of terrain, soil, climate, etc. in different regions, different types of greenhouses are built according to local conditions, such as Shandong greenhouse type, North China greenhouse type, plateau greenhouse type, Jiangnan greenhouse type, South China greenhouse type, etc. With the rapid development of technologies such as the Internet of Things, cloud computing, and big data, traditional greenhouses will gradually be replaced by smart greenhouses. Smart greenhouses use meteorological sensors to monitor data in real time and intelligently control the facilities and equipment in the greenhouse, greatly reducing labor costs. The growth cycle of greenhouse fruit and vegetables is generally 30-120 days. During the pruning period, some types of fruits and vegetables, such as tomatoes, peppers, and melons, still require manual operation by workers, using polypropylene wire as binding ropes, inserting racks to wrap around and fix seedlings, or using suspension to adjust the plants, which prevents the seedlings from falling over, and is conducive to the management of plants and the ventilation and light transmission of their growth environment, enhancing the resistance of plants, and avoiding the breeding of bacteria.
[0003] Photoconversion agricultural films have been used in many places. That is, photoconversion agents are added to the agricultural films to convert ultraviolet light and yellow-green light that are detrimental to the growth of crops into blue light or red-orange light. However, the effect of blue light or red-orange light on the aging and degradation of polypropylene is far less than that of ultraviolet light (polypropylene can only produce a series of photooxidation reactions under ultraviolet light and then cause the breakage of the molecular chain). Under this light, polypropylene monofilaments used as binding ropes are difficult to age; or, due to the short maturity period of crops, the strength of polypropylene monofilaments is still very high during the binding period of crops, and the aging effect is not obvious. When the fruits and vegetables are ripe and harvested, the binding ropes need to be cut manually one by one, which has low recycling efficiency and is time-consuming, which is not conducive to mechanized operations, and the higher-strength binding ropes are easy to damage the recycling equipment. Summary of the invention
[0004] In view of the above-mentioned defects or deficiencies in the prior art, it is desired to provide a polypropylene film with controllable degradation cracks.
[0005] In a first aspect, a degradation-controlled polypropylene film tear thread is provided, wherein the polypropylene film tear thread comprises an inner layer and an outer layer, wherein the outer layer wraps the inner layer, The inner layer material is polypropylene waste; The outer layer is composed of: polypropylene, photoinitiator, and polyethylene wax, wherein the mass percentage of the photoinitiator to the polypropylene is 0.2-6%, and the mass percentage of the polyethylene wax to the polypropylene is 3-6%.
[0006] As an achievable manner, the photoinitiator is one or more of photoinitiator 784, photoinitiator TPO, photoinitiator 1173, photoinitiator ITX, and photoinitiator 1101.
[0007] As an achievable manner, the polyethylene wax is AC6A.
[0008] As an achievable manner, the type of the photoinitiator is related to the light irradiation environment of the cracks in the polypropylene film.
[0009] As a feasible manner, when the illumination environment is natural light, the photoinitiator includes at least photoinitiator 784, photoinitiator ITX, and photoinitiator 1101, and the photoinitiator ITX and the photoinitiator 1101 are mixed in a mass fraction ratio of (95-98): (2-5), and then compounded with the photoinitiator 784 in a mass fraction ratio of 1:1.
[0010] As a feasible manner, the lighting environment is visible light, and the photoinitiator at least includes photoinitiator 784.
[0011] As an achievable manner, the polypropylene film has a tear fineness of 2000-2500D and a thickness of 49-51 μm.
[0012] As a feasible manner, the amount of the photoinitiator added to the cracks of the polypropylene film within each set interval is not completely the same.
[0013] According to the technical solution provided in the embodiment of the present application, by constructing the polypropylene film cracks into a skin-core structure, the inner core is prepared by polypropylene waste and a photoinitiator is added to the outer material. On the one hand, the higher strength of the outer layer is relied on to meet the bundling strength requirements of the polypropylene film cracks, and the photoinitiator in the outer layer only needs to meet the aging and degradation requirements of the outer layer to reduce the amount of photoinitiator used in the polypropylene film cracks. At the same time, polypropylene waste can also be used in the polypropylene film cracks, thereby reducing the preparation cost of the polypropylene film cracks and increasing the recycling and use of polypropylene waste. On the other hand, by adding a photoinitiator to the outer material, the photoinitiator is added to the polypropylene molecular chain. Under different lighting conditions, the photoinitiator forms different types of free radicals, causing aging and breaking of the polypropylene molecular chain. By adjusting the different addition amounts, the strength of the prepared film cracks can be quickly reduced to the required parameter value, so that during the harvesting process of the polypropylene film cracks, the harvesting can be carried out more conveniently and quickly without damaging the harvesting equipment. DETAILED DESCRIPTION
[0014] The present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.
[0015] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below in conjunction with the embodiments.
[0016] This embodiment provides a polypropylene film tear thread with controllable degradation, wherein the polypropylene film tear thread comprises an inner layer and an outer layer, wherein the outer layer wraps the inner layer. The inner layer material is polypropylene waste; The outer layer is composed of: polypropylene, photoinitiator, and polyethylene wax, wherein the mass percentage of the photoinitiator to the polypropylene is 0.2-6%, and the mass percentage of the polyethylene wax to the polypropylene is 3-6%.
[0017] The polypropylene film split wire provided in this embodiment is constructed into a skin-core structure, the inner core is prepared by polypropylene waste and a photoinitiator is added to the outer material. The inner layer of polypropylene waste is significantly lower in strength than the outer layer of new polypropylene material. On the one hand, the higher strength of the outer layer is relied on to meet the bundling strength requirements of the polypropylene film split wire, and the photoinitiator in the outer layer only needs to meet the aging and degradation requirements of the outer layer to reduce the amount of photoinitiator used in the polypropylene film split wire. At the same time, polypropylene waste can also be used in the polypropylene film split wire, thereby reducing the preparation cost of the polypropylene film split wire and increasing the recycling and use of polypropylene waste. On the other hand, by adding a photoinitiator to the outer material, the photoinitiator is added to the polypropylene molecular chain. Under different lighting conditions, the photoinitiator forms different types of free radicals, causing aging and breaking of the polypropylene molecular chain. By adjusting the different addition amounts, the strength of the prepared film split wire can be quickly reduced to the required parameter value, so that in the process of harvesting the polypropylene film split wire, it is more convenient and faster to harvest, and the harvesting equipment is not damaged.
[0018] Optionally, the photoinitiator is one or more of photoinitiator 784 (bis (2,6-difluoro-3-pyrrophenyl) titanocene), photoinitiator TPO (2,4,6-trimethylbenzoyl-diphenylphosphine oxide), photoinitiator 1173 (2-hydroxy-2-methyl-1-phenyl-1-propanone), photoinitiator ITX (isopropylthioxanthone), and photoinitiator 1101 (ethyl 4-(N,N-dimethylamino)benzoate).
[0019] In this embodiment, by adding a photoinitiator to the polypropylene material, the supported polypropylene film cracks are aged faster under light conditions and aged to a set parameter value within a user-set time, so that the polypropylene film cracks are easily broken during harvesting, and the harvesting process is more convenient and quick. Under different irradiation conditions, the photoinitiator in the polypropylene film cracks forms different types of free radicals, which rob the hydrogen atoms on the tertiary carbon to form new free radicals, thereby causing the aging and breaking of the polypropylene molecular chain.
[0020] Among them, photoinitiators of different components react differently to light of different colors, and different amounts of photoinitiators added will also affect the aging speed of polypropylene film cracks. The amount and type of photoinitiator added can be selected according to different user needs.
[0021] On the basis of meeting the preparation requirements of the polypropylene film cracks, the amount of photoinitiator added is proportional to the aging rate of the polypropylene film cracks, and the type of photoinitiator is related to the lighting environment of the polypropylene film cracks.
[0022] Optionally, if the lighting environment is natural light, the photoinitiator includes at least photoinitiator 784, photoinitiator ITX, and photoinitiator 1101, and the photoinitiator ITX and the photoinitiator 1101 are mixed in a mass fraction ratio of (95-98): (2-5), and then compounded with the photoinitiator 784 in a mass fraction ratio of 1:1.
[0023] The polypropylene film cracks disclosed in this embodiment are used in a visible light environment, such as when used outdoors, and the corresponding polypropylene film cracks are compounded with the photoinitiators of the above components, wherein the photoinitiator 784 is photoisomerized into a cyclic photoreaction intermediate to generate free radicals, which generally generate free radicals under the irradiation of visible light, and the photoinitiator ITX cooperates with the auxiliary initiator tertiary amine 1101 to form amine alkyl free radicals with high initiation activity and thioxanthone without initiation activity, and the photoinitiator ITX generates free radicals under the irradiation of ultraviolet light. Therefore, when conventional agricultural films are prepared, the photoinitiators with the above ratio are used, and various light rays in the visible light can be applied to the accelerated aging process of the polypropylene film cracks.
[0024] Optionally, if the illumination environment is visible light, the photoinitiator includes at least photoinitiator 784.
[0025] The visible light in this embodiment is blue light and / or red-orange light. Under these lights, the photoinitiator 784 can effectively accelerate the aging process of the cracks in the polypropylene film.
[0026] Optionally, if the illumination environment is ultraviolet light, the photoinitiator includes at least photoinitiator ITX and photoinitiator 1101, and the photoinitiator ITX and the photoinitiator 1101 are mixed in a mass fraction ratio of (95-98): (2-5); or at least includes photoinitiator TPO and photoinitiator 1173.
[0027] Because the photoinitiator TPO is combined with the photoinitiator 1173 to split into trimethylbenzoyl radicals and diphenylphosphonyl radicals with high initiation activity; the photoinitiator ITX is combined with the co-initiator tertiary amine 1101 to form amine alkyl radicals with high initiation activity and thioxanthone with no initiation activity, both of which can form different types of free radicals under the irradiation of ultraviolet light, snatching hydrogen atoms from the tertiary carbon to form new free radicals, thereby causing aging and breakage of the polypropylene molecular chain.
[0028] Optionally, the polyethylene wax is AC6A.
[0029] Optionally, the polypropylene film has a tear fineness of 2000-2500D and a thickness of 49-51 microns.
[0030] Optionally, the amount of the photoinitiator added within each set spacing of the polypropylene film cracks is not completely the same.
[0031] The polypropylene film cracks provided in this embodiment are mainly used for fixing during the growth of crops. When the crops need to be harvested, the polypropylene film cracks also need to be separated to facilitate the harvesting of the crops. By adding a photoinitiator to the polypropylene film cracks and controlling the type and amount of the photoinitiator to achieve different aging speeds, the severely aged polypropylene film cracks are easier to be torn off during the harvesting process, and are also more convenient for the harvesting of crops. In the harvesting process of the polypropylene film cracks, as long as a certain point of the film cracks is broken, it is easy to be torn off for harvesting. Therefore, this embodiment can also adjust the amount of photoinitiator added to the produced polypropylene film cracks, for example, the amount added within one end is increased to facilitate the section of the film cracks to be more easily torn off, and the film cracks at other positions are slightly stronger, not easy to break during the harvesting process, and are also convenient for the waste recovery work after the film cracks are broken. Different controlled degradable polypropylene film split threads are selected under different agricultural films and different growth cycles of fruits and vegetables. When the fruits and vegetables are ripe and harvested, there is no need to manually cut the binding ropes one by one. The recycling efficiency is high, which is conducive to mechanized operations and can well protect the recycling equipment to avoid soil pollution.
[0032] The polypropylene film filaments provided in this embodiment are prepared by extrusion through a twin-screw extruder, and the machine is provided with a plurality of side feeding ports, through which corresponding additives are added, so the amount of photoinitiator added can be adjusted in real time.
[0033] This embodiment also provides a method for preparing degradable controllable polypropylene film cracks, using a twin-screw extruder, first adding polypropylene into the main feeding barrel, and then adding polyethylene wax and photoinitiator into the main barrel in a mass fraction ratio of (3-6): (0.2-6) through a side feeding screw, and then extruding into a film after filtering, pressurizing, and metering, and then cooling, film lifting, cutting, stretching, opening the net, shaping, and then winding to obtain controllable degradable polypropylene film cracks.
[0034] The cooling method is water cooling, the cooling temperature is 28-32°C, and the stretching method is one-stage double-layer hot air oven stretching, and the stretching ratio is 8-12 times.
[0035] Five specific embodiments and one comparative example are given below: Embodiment 1 Using a twin-screw extruder, first add polypropylene to the main feed barrel, then add polyethylene wax and photoinitiator to the main machine at a mass fraction ratio of 3:6 through the side feeding screw, and the photoinitiator is TPO and 1173 compounded at a mass fraction ratio of 95:5. After filtering, pressurization, and metering, it is extruded into a film, and then cooled, filmed, cut, stretched, opened, and shaped before winding to obtain polypropylene film cracks. Among them, the cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracks is 2000D and the thickness is 50 microns.
[0036] Embodiment 2 Using a twin-screw extruder, first add polypropylene to the main feed barrel, then add polyethylene wax and photoinitiator to the main machine at a mass fraction ratio of 3:6 through the side feeding screw, and the photoinitiator is ITX and 1101 compounded at a mass fraction ratio of 95:5. After filtering, pressurization, and metering, it is extruded into a film, and then cooled, filmed, cut, stretched, opened, and shaped before winding to obtain polypropylene film cracks. Among them, the cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracks is 2000D and the thickness is 50 microns.
[0037] Embodiment 3 Using a twin-screw extruder, first add polypropylene to the main feed barrel, then add polyethylene wax and photoinitiator 784 to the main machine at a mass fraction ratio of 3:6 through a side feeding screw, extrude into a film after filtering, pressurization, and metering, and then cool, lift the film, cut, stretch, open the net, and shape it before winding to obtain polypropylene film cracks. Among them, the cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracks is 2000D and the thickness is 50 microns.
[0038] Embodiment 4 Using a twin-screw extruder, first add polypropylene to the main feed barrel, then add polyethylene wax and photoinitiator to the main machine at a mass fraction ratio of 3:6 through the side feeding screw, the photoinitiator is TPO and 1173 compounded at a mass fraction ratio of 95:5, and then compounded with photoinitiator 784 at a mass fraction ratio of 1:1. After filtering, pressurization, and metering, it is extruded into a film, and then cooled, filmed, cut, stretched, opened, and shaped before winding to obtain polypropylene film cracks. Among them, the cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracks is 2000D and the thickness is 50 microns.
[0039] Embodiment 5 Using a twin-screw extruder, first add polypropylene to the main feed barrel, then add polyethylene wax and photoinitiator to the main machine at a mass fraction ratio of 3:6 through the side feeding screw, the photoinitiator is ITX and 1101 compounded at a mass fraction ratio of 95:5, and then compounded with photoinitiator 784 at a mass fraction ratio of 1:1. After filtering, pressurization, and metering, it is extruded into a film, and then cooled, filmed, cut, stretched, opened, and shaped before winding to obtain polypropylene film cracks. Among them, the cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracks is 2000D and the thickness is 50 microns.
[0040] Comparative Example The polypropylene is added into the main feeding barrel by a twin-screw extruder, and then extruded into a film after filtering, pressurization, and metering, and then rolled up after cooling, film lifting, cutting, stretching, opening, shaping, and then obtaining the polypropylene film cracked filaments. The cooling method is water cooling, the cooling temperature is 30 ℃, and the stretching method is a first-level double-layer hot air oven stretching, and the stretching ratio is 10 times. The fineness of the polypropylene film cracked filaments is 2000D and the thickness is 50 microns.
[0041] The preparation methods used in the above examples and comparative examples are the same, both using a twin-screw extruder for melt extrusion, and the subsequent cooling and stretching methods are also the same, and the fineness and thickness of the prepared polypropylene film cracks are the same. The samples obtained in the above examples are subjected to accelerated aging tests: 1. Test environment: The products obtained in each embodiment were subjected to accelerated aging tests using different light sources. The strength retention of the open mesh was tested according to the JIS-L-1017:2002 test method. The illumination was 40-42 W / m2, the BPT blackboard temperature was 45°C, the humidity was 65%, the aging treatment time was 72 h, the outer cover was #320, and the inner cover was quartz.
[0042] 2. Test conditions of strength machine: gauge 250mm, speed 300mm / min, pre-tension 0.45mN / tex 3. Strength retention rate (%) = strength after treatment / original silk strength × 100% 4. Test results of strength retention rate The test results show that different photoinitiators will cause aging and breakage of polypropylene molecular chains under corresponding irradiation conditions.
[0043] Therefore, according to different photoinitiator addition amounts and different irradiation conditions, the intensity of the film crack line decreases rapidly to the desired parameter value.
[0044] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.
Claims
1. A degradation-controlled polypropylene film crack, characterized in that: The polypropylene film tear thread comprises an inner layer and an outer layer, wherein the outer layer wraps the inner layer. The inner layer material is polypropylene waste; The outer layer is composed of: polypropylene, photoinitiator, and polyethylene wax, wherein the mass percentage of the photoinitiator to the polypropylene is 0.2-6%, and the mass percentage of the polyethylene wax to the polypropylene is 3-6%.
2. The degradation-controlled polypropylene film crack according to claim 1, characterized in that: The photoinitiator is one or more of photoinitiator 784, photoinitiator TPO, photoinitiator 1173, photoinitiator ITX, and photoinitiator 1101.
3. The degradation-controlled polypropylene film crack according to claim 1, characterized in that: The polyethylene wax is AC6A.
4. The degradation-controlled polypropylene film crack according to claim 1, characterized in that: The type of the photoinitiator is related to the light irradiation environment of the polypropylene film cracks.
5. The degradation-controlled polypropylene film crack according to claim 4, characterized in that: When the illumination environment is natural light, the photoinitiator includes at least photoinitiator 784, photoinitiator ITX, and photoinitiator 1101, and the photoinitiator ITX and the photoinitiator 1101 are mixed in a mass fraction ratio of (95-98): (2-5), and then compounded with the photoinitiator 784 in a mass fraction ratio of 1:
1.
6. The degradation-controlled polypropylene film crack according to claim 4, characterized in that: When the illumination environment is visible light, the photoinitiator at least includes photoinitiator 784 .
7. The degradation-controlled polypropylene film crack according to claim 1, characterized in that: The polypropylene film has a tear fineness of 2000-2500D and a thickness of 49-51 microns.
8. The degradation-controlled polypropylene film crack according to claim 1, characterized in that: The amount of the photoinitiator added to the polypropylene film cracks within the set intervals is not completely the same.
Citation Information
Patent Citations
Preparation method of rapid-degradable plastic woven bag
CN109836789A
Production formula and production process of high-strength stretching wrapping film
CN112391001A
Photodegradable polypropylene material and preparation method thereof
CN114395190A
Spunbond nonwoven fabrics from reclaimed polymer and the manufacture thereof
CN1564885A
Degradable polypropylene adhesive rope
CN220246541U