Polyacrylonitrile-based carbon fiber and preparation method thereof
Through multi-stage preoxidation and low-temperature carbonization treatment processes, combined with high-temperature carbonization zone optimization, the problems of high-voltage and unstable performance of polyacrylonitrile-based carbon fibers are solved, and high-performance and low-cost carbon fiber production are achieved.
Patent Information
- Application Number
- CN202410942999.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
The existing polyacrylonitrile-based carbon fiber production process is costly and unstable, making it difficult to maintain high performance while reducing production costs.
Using multi-stage preoxidation and low-temperature carbonization treatment processes, the temperature and draft ratio of the oxidation temperature zone are finely controlled, the preoxidation treatment time is shortened, the fiber operation speed is improved, and the temperature zone setting is optimized during the high-temperature carbonization stage to ensure timely emission of waste gas and reduce Structural defects.
It realizes high-performance production of polyacrylonitrile-based carbon fiber, reduces production costs, increases the strength and modulus of fibers, and is suitable for industrial mass production.
Smart Images

Figure CN118880495A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fibers, and in particular to a polyacrylonitrile-based carbon fiber and a preparation method thereof. Background Art
[0002] Since the 1950s, carbon fiber has been continuously researched and developed by scientific researchers. At present, there are roughly three types of viscose fiber, asphalt fiber, and polyacrylonitrile fiber. Due to its high strength, high modulus, high temperature resistance, corrosion resistance, friction resistance, thermal conductivity and other excellent properties, polyacrylonitrile fiber has gradually become the mainstream production of the carbon fiber industry, and is widely used in defense fields such as aerospace, as well as civilian fields such as the automotive industry and wind power generation.
[0003] In the field of polyacrylonitrile-based carbon fiber production, the current industrial production operation is to pre-oxidize the PAN precursor through an air oxidation furnace with a temperature gradient (temperature range of 180-300°C), and then carbonize the pre-oxidized fiber in high-purity nitrogen at a maximum temperature of 1400-1600°C. If the pre-oxidized fiber is directly carbonized at a temperature above 1000°C, the strong thermal shock will cause damage to the fiber structure. In order to avoid this damage, the pre-oxidized fiber is first subjected to a medium-low temperature carbonization heat treatment of 300-900°C before high-temperature carbonization, collectively referred to as low-temperature carbonization.
[0004] Among them, in the pre-oxidation process, especially in the initial stage, the fiber should be properly stretched to inhibit the shrinkage of PAN macromolecules and maintain the orientation of PAN macromolecule chains to the fiber axis. At the same time, as the pre-oxidation temperature increases, complex chemical reactions such as cyclization, dehydrogenation and oxidation of PAN macromolecules first occur in the amorphous region and then in the ordered region inside the fiber, releasing a large amount of heat, and finally forming an axially oriented, rigid, stable trapezoidal high molecular weight polymer structure, so that the fiber has the ability to not melt or burn during high temperature carbonization and continue to maintain the fiber shape.
[0005] The low-temperature carbonization process is the transition stage between the pre-oxidation process and the high-temperature carbonization process. As the low-temperature carbonization temperature increases, the fiber undergoes a cracking reaction, non-carbon elements are gradually removed, and small molecular gases such as H 2 , H 2 O, NH 3 , HCN, CO 2 ,CO,N 2 The smaller trapezoidal structures in the pre-oxidized fibers are cross-linked to initially form carbon-based surfaces. Carbonization at high temperatures above 1000°C causes the carbon-based surfaces to grow further, and polycondensation occurs to release a large amount of HCN and N 2, so that the carbon content in the fiber reaches more than 90%, forming a two-dimensional ordered layered network graphite structure. The cross-linking and network of the molecular structure inside the fiber enhances the intermolecular force and reduces the activity of the molecular chain, thereby greatly improving the strength and modulus of the fiber.
[0006] Among them, when the pre-oxidation temperature is relatively fixed, increasing the wire feeding speed will shorten the residence time of the tow in the pre-oxidation furnace, reduce the degree of cyclization reaction, reduce the pre-oxidation degree of PAN fiber, and reduce the bulk density; on the other hand, the increase in wire feeding speed will also cause the air atmosphere in the pre-oxidation furnace to change, and oxygen cannot fully diffuse into the tow, which will also lead to the formation of the pre-oxidation fiber skin-core structure and affect the mechanical properties of the final carbon fiber. Pre-oxidation temperature and wire feeding speed are two important influencing factors in the pre-oxidation process. Increasing the pre-oxidation temperature is conducive to improving the fiber bulk density; and when the increase in wire feeding speed causes the bulk density to decrease, the deficiency of the pre-oxidation reaction can also be compensated by increasing the pre-oxidation temperature to ensure that the fiber has a higher bulk density after pre-oxidation treatment. After pre-oxidation treatment, the fiber will contain a large number of linear uncyclized molecular chain structures, and cyclization and cross-linking reactions will continue to occur in the subsequent low-temperature carbonization stage, which will help to make the fiber structure dense in the carbonization stage. The pre-oxidation filament density is high. When the pre-oxidation degree is too high, it is easy to cause overoxidation of PAN fiber, destroy the molecular structure of the ladder polymer, thereby limiting the formation of carbon-based plane length and stacking height in the carbonization stage, and it is easy to produce a skin-core structure in the radial direction of the fiber, resulting in a decrease in the body density of the carbon fiber. With the decrease in the pre-oxidation filament density, the tensile strength of the carbon fiber has a trend of increasing first and then decreasing. The reason is that although the fiber with a low pre-oxidation degree can prepare high-density carbon fiber, due to insufficient pre-oxidation in the early stage, the fiber is prone to fusion in the high-temperature carbonization stage, resulting in obvious structural defects in the carbon fiber, so the tensile strength of the carbon fiber decreases. When the pre-oxidation degree is too high, the skin-core structure inside the fiber is aggravated after carbonization treatment, which will also cause a decrease in the tensile strength of the carbon fiber.
[0007] The carbonization process conditions have a direct impact on the strength of the final carbon fiber and are quite sensitive. From the perspective of equipment, tar and cracking waste gas, the purity of protective gas, and the sealing of the furnace body are the main factors affecting the final carbon fiber performance, and from the perspective of process parameters, the gradient distribution of the carbonization furnace temperature and the cooling rate of the fiber are the main factors. Generally speaking, the tensile strength of carbon fiber is determined by defects in the structure, which may be caused by impurity atoms in the fiber and bubbles generated when the gas is discharged. Below 1400-1600℃, as the carbonization temperature increases, the tensile strength of the carbon fiber gradually increases, reaches the maximum value, and then begins to decline. In addition to the maximum carbonization temperature, the low temperature carbonization temperature will also affect the strength of the carbon fiber.
[0008] At present, in the field of polyacrylonitrile-based carbon fiber technology, it is necessary to improve the comprehensive performance of carbon fiber and reduce its production cost. The production process of carbon fiber can be divided into polyacrylonitrile fiber (precursor), pre-oxidation process and carbonization process. Pre-oxidation is an important intermediate process in the production of polyacrylonitrile-based carbon fiber. It serves as a bridge from the conversion of precursor to carbon fiber. Pre-oxidation not only controls the quality of carbon fiber, but also controls the output of carbon fiber. Similarly, the pre-oxidation furnace in the pre-oxidation stage is also a key equipment for carbon fiber production. It is also the equipment with the longest time and the highest energy consumption. The operating temperature is 180-300°C, and the fiber treatment time in the pre-oxidation furnace is generally 70-120 minutes. Therefore, the key to reducing the production cost of carbon fiber and improving the quality lies in the pre-oxidation stage of carbonization.
[0009] In summary, there is an urgent need for a method for preparing polyacrylonitrile-based carbon fiber, which can reduce its production cost while ensuring the performance of the polyacrylonitrile-based carbon fiber. Summary of the invention
[0010] In view of this, the present invention provides a polyacrylonitrile-based carbon fiber and a preparation method thereof, the main purpose of which is to reduce the production cost of the polyacrylonitrile-based carbon fiber while ensuring the performance of the polyacrylonitrile-based carbon fiber.
[0011] In order to achieve the above object, the present invention mainly provides the following technical solutions:
[0012] On the one hand, an embodiment of the present invention provides a method for preparing polyacrylonitrile-based carbon fiber, which comprises the following steps:
[0013] Pre-oxidation treatment: pre-oxidation treatment is performed on the polyacrylonitrile-based fiber to obtain pre-oxidized fiber;
[0014] Low-temperature carbonization treatment: performing low-temperature carbonization treatment on the pre-oxidized fiber to obtain low-temperature carbonized fiber;
[0015] High-temperature carbonization treatment: subjecting the low-temperature carbonized fiber to high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fiber;
[0016] Among them, during the pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment, the fiber running speed is 600-900 m / h;
[0017] Among them, in the pre-oxidation treatment step: the polyacrylonitrile fiber is sequentially passed through a first pre-oxidation temperature zone, a second pre-oxidation temperature zone, a third pre-oxidation temperature zone, and a fourth pre-oxidation temperature zone for pre-oxidation treatment to obtain pre-oxidized fiber; wherein, in the first pre-oxidation temperature zone: the temperature is 250-255°C, and the total stretch ratio applied to the fiber is 2%-3%; in the second pre-oxidation temperature zone: the temperature is 256-260°C, and the total stretch ratio applied to the fiber is 0%-2%; in the third pre-oxidation temperature zone: the temperature is 261-264°C, and the total stretch ratio applied to the fiber is -2.0%-0%; in the fourth pre-oxidation temperature zone: the temperature is 265-275°C, and the total stretch ratio applied to the fiber is -4.0%-2.0%.
[0018] Preferably, multiple layers are arranged in each of the first pre-oxidation temperature zone, the second pre-oxidation temperature zone, the third pre-oxidation temperature zone, and the fourth pre-oxidation temperature zone from bottom to top, so that the fiber passes through each pre-oxidation temperature zone layer by layer from bottom to top; wherein, when the fiber passes through each pre-oxidation temperature zone layer by layer, the tension applied to the fiber increases layer by layer, so that the draft ratio decreases layer by layer; preferably, the tension of the latter pre-oxidation temperature zone is 100-200CN higher than that of the previous pre-oxidation temperature zone.
[0019] Preferably, when the polyacrylonitrile fiber passes through the first pre-oxidation temperature zone, the fiber color gradually changes from white to light yellow and then gradually changes to dark yellow; when passing through the second pre-oxidation temperature zone, the fiber color gradually changes from dark yellow to brown-black; when passing through the third pre-oxidation temperature zone, the fiber color gradually changes from brown-black to black; and when passing through the fourth pre-oxidation temperature zone, the black color of the fiber gradually deepens.
[0020] Preferably, in the first pre-oxidation temperature zone, the fiber tension is controlled at 718-1019CN by controlling the temperature and the draft ratio; in the second pre-oxidation temperature zone, the fiber tension is controlled at 904-1254CN by controlling the temperature and the draft ratio; in the third pre-oxidation temperature zone, the fiber tension is controlled at 1233-1497CN by controlling the temperature and the draft ratio; in the fourth pre-oxidation temperature zone, the fiber tension is controlled at 1316-1500CN by controlling the temperature and the draft ratio;
[0021] Preferably, 7 temperature zones are arranged in sequence from bottom to top in the first pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 718-762CN, the tension of the fiber in the second temperature zone is 797-831CN, the tension of the fiber in the third temperature zone is 837-846CN, the tension of the fiber in the fourth temperature zone is 942-954CN, the tension of the fiber in the fifth temperature zone is 967-980CN, the tension of the fiber in the sixth temperature zone is 1012-1073CN, and the tension of the fiber in the seventh temperature zone is 1008-1019CN; preferably, the Seven temperature zones are arranged in sequence from bottom to top in the second pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 904-971CN, the tension of the fiber in the second temperature zone is 986-1072CN, the tension of the fiber in the third temperature zone is 1013-1083CN, the tension of the fiber in the fourth temperature zone is 1143-1191CN, the tension of the fiber in the fifth temperature zone is 1121-1168CN, the tension of the fiber in the sixth temperature zone is 1208-1239CN, and the tension of the fiber in the seventh temperature zone is 1220-1254CN; preferably, the The third pre-oxidation temperature zone is provided with 7 temperature zones from bottom to top, the tension of the fiber in the first temperature zone is 1233-1253CN, the tension of the fiber in the second temperature zone is 1318-1334CN, the tension of the fiber in the third temperature zone is 1308-1315CN, the tension of the fiber in the fourth temperature zone is 1403-1415CN, the tension of the fiber in the fifth temperature zone is 1415-1438CN, the tension of the fiber in the sixth temperature zone is 1434-1458CN, and the tension of the fiber in the seventh temperature zone is 1467-1497CN; preferably , 7 temperature zones are arranged from bottom to top in the fourth pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 1316-1362CN, the tension of the fiber in the second temperature zone is 1365-1400CN, the tension of the fiber in the third temperature zone is 1400-1432CN, the tension of the fiber in the fourth temperature zone is 1422-1442CN, the tension of the fiber in the fifth temperature zone is 1438-1466CN, the tension of the fiber in the sixth temperature zone is 1456-1486CN, and the tension of the fiber in the seventh temperature zone is 1486-1500CN.
[0022] Preferably, the bulk density of the polyacrylonitrile fiber is 1.185-1.195 g / cm 3 , diameter is 8 to 12 μm.
[0023] Preferably, the formic acid solubility of the pre-oxidized fiber is 1.0% to 5.0%, and the density of the pre-oxidized fiber body is 1.360 to 1.365 g / cm 3 , tensile strength is 385~410MPa, elongation at break is 7.5~8.5%, and elastic modulus is 10~11Gpa.
[0024] Preferably, the total residence time of the pre-oxidation treatment is 30 to 38 minutes, and the residence time of the fiber in each pre-oxidation temperature zone is 7.5 to 9 minutes.
[0025] Preferably, in the pre-oxidation step, the pre-oxidation furnace used is a side-blown hot air circulation oxidation furnace; wherein, during the pre-oxidation process: the circulating air volume of the oxidation furnace is controlled to be 200000-300000m 3 / h, wind speed is controlled at 2-3m / s.
[0026] Preferably, during the low-temperature carbonization treatment: the pre-oxidized fiber is sequentially passed through the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone, and the sixth temperature zone for low-temperature carbonization treatment to obtain low-temperature carbonized fiber; wherein the temperature of the first temperature zone is 420-450°C, the temperature of the second temperature zone is 460-490°C, the temperature of the third temperature zone is 500-520°C, the temperature of the fourth temperature zone is 530-570°C, the temperature of the fifth temperature zone is 600-700°C, and the temperature of the sixth temperature zone is 700-800°C; preferably, the residence time of the fiber in each temperature zone is 12-20s.
[0027] Preferably, during the low-temperature carbonization treatment, the draft ratio applied to the fiber is 0-5%, and the tension applied to the fiber is 1200-1500 CN.
[0028] Preferably, during the high-temperature carbonization treatment: the low-temperature carbonized fiber is sequentially passed through a first temperature zone, a second temperature zone, a third temperature zone, and a fourth temperature zone for high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fiber; wherein the temperature of the first temperature zone is 1000-1200°C, the temperature of the second temperature zone is 1300-1400°C, the temperature of the third temperature zone is 1400-1500°C, and the temperature of the fourth temperature zone is 1200-1300°C; preferably, the residence time of the fiber in each temperature zone is 12-15s.
[0029] Preferably, during the high-temperature carbonization treatment, the draft ratio applied to the fiber is -4.0 to 0%, and the tension applied to the fiber is 1900 to 2200 CN.
[0030] In another aspect, an embodiment of the present invention provides a polyacrylonitrile-based carbon fiber, wherein the bulk density of the polyacrylonitrile-based carbon fiber is 1.790 to 1.810 g / cm 3 The strength is 1392~1450N, the tensile strength is 5.49~5.84Gpa, the elongation at break is 2.2~2.4%, and the tensile modulus is 230~238Gpa.
[0031] Compared with the prior art, the polyacrylonitrile-based carbon fiber and the preparation method thereof of the present invention have at least the following beneficial effects:
[0032] On the one hand, an embodiment of the present invention provides a method for preparing polyacrylonitrile-based carbon fiber, wherein the polyacrylonitrile-based fiber is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fiber; here, the embodiment of the present invention reasonably designs the temperature and the drawing ratio of the oxidation temperature zone, which can not only achieve sufficient pre-oxidation and ensure the performance of the pre-oxidized fiber, but also shorten the residence time of the pre-oxidation treatment, so that the running speed of the fiber can reach 600-900m / h, which can greatly reduce the production cost of the carbon fiber and is suitable for industrial production. Specifically, the temperature and the stretch ratio of the oxidation temperature zone are designed as follows: the polyacrylonitrile fiber is sequentially passed through a first pre-oxidation temperature zone, a second pre-oxidation temperature zone, a third pre-oxidation temperature zone, and a fourth pre-oxidation temperature zone for pre-oxidation treatment to obtain pre-oxidized fiber; wherein, in the first pre-oxidation temperature zone: the temperature is 250-255°C, and the total stretch ratio applied to the fiber is 2%-3%; in the second pre-oxidation temperature zone: the temperature is 256-260°C, and the total stretch ratio applied to the fiber is 0%-2%; in the third pre-oxidation temperature zone: the temperature is 261-264°C, and the total stretch ratio applied to the fiber is -2.0%-0%; in the fourth pre-oxidation temperature zone: the temperature is 265-275°C, and the total stretch ratio applied to the fiber is -4.0%-2.0%. Here, in the first pre-oxidation temperature zone, in the air atmosphere, the chemical reaction just begins to occur. In order to prevent the physical shrinkage of the original silk and to improve the orientation of the fiber, the total draft ratio is controlled at 2% to 3%. At the same time, the reaction rate is increased, and the temperature of the first oxidation temperature zone is controlled at 250 to 255°C, so that the fiber gradually changes from white to light yellow and then gradually changes to dark yellow. Then, in the second pre-oxidation temperature zone, the draft ratio is gradually reduced layer by layer to ensure that the tension increases smoothly, and the temperature is appropriately increased so that the fiber gradually changes from dark yellow to brown-black. Then, enter the third pre-oxidation temperature zone, which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature is controlled at 261 to 264°C, the total draft ratio is controlled at -2.0% to 0%, and the draft ratio of each layer in the oxidation temperature zone is reduced layer by layer, so that the chemical reaction proceeds smoothly, and the fiber color gradually changes from brown-black to black. Finally, enter the fourth pre-oxidation temperature zone, which determines the performance of the final pre-oxidation silk and is the most sensitive area for chemical reactions. Here, the gradient difference between the fourth pre-oxidation temperature zone and the third pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and causing the formation of an obvious skin-core structure. The temperature of the fourth pre-oxidation temperature zone is controlled at 265-275°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total drafting ratio is controlled at -4.0% to -2.0%. The drafting ratio of each layer in the oxidation temperature zone decreases layer by layer, and the black degree of the fiber gradually deepens. Through the above pre-oxidation treatment process, polyacrylonitrile fiber (with a bulk density of 1.185-1.195 g / cm 3, diameter 8 to 12 μm) pre-oxidized into "formic acid solubility of 1.0% to 5.0%, pre-oxidized fiber body density of 1.360 to 1.365 g / cm 3 , tensile strength of 385-410MPa, elongation at break of 7.5-8.5%, and elastic modulus of 10-11Gpa" pre-oxidized fiber. At the same time, the total residence time of the pre-oxidation treatment is 30-38min, which greatly shortens the residence time, thereby greatly reducing energy consumption and production costs.
[0033] Furthermore, an embodiment of the present invention provides a method for preparing polyacrylonitrile-based carbon fiber. By setting the temperature of the temperature zone for low-carbon treatment, it is ensured that the waste gas and oligomers generated by low-temperature carbonization can be discharged instantly, avoiding the reduction of fiber strength after high-temperature carbonization. The residence time in each temperature zone is 12 to 20 seconds, the low-temperature carbonization draft is controlled at 0 to 5%, and the low carbon fiber tension is controlled to 1200 to 1500CN. Through the large draft ratio, the crystallites in the low-carbon filament structure are more closely combined with each other, and the fiber densification degree is higher, so that the fiber structure is more uniform, which is beneficial to the improvement of the mechanical properties of the carbon fiber.
[0034] Furthermore, a method for preparing polyacrylonitrile-based carbon fiber provided in an embodiment of the present invention ensures that the waste gas generated by high-temperature carbonization is discharged in time through the temperature setting of the high-carbon treatment temperature zone, which is beneficial to improving the performance of the carbon fiber and reducing the equipment manufacturing and operation and maintenance costs. The residence time in each temperature zone is 12 to 15 seconds, the draft ratio applied to the fiber is -4.0 to 0%, and the tension applied to the fiber is 1900 to 2200CN, so that the aromatic ring structure is rearranged to form a carbon network structure, that is, a chaotic graphite structure, and the orientation is further improved, which is beneficial to improving the strength and modulus of the fiber.
[0035] In summary, the scheme of the present invention is suitable for the industrial mass production of 6K and 12K high-performance polyacrylonitrile-based carbon fibers, which breaks through the problems of slow operating speed, low qualified rate and high production cost of enterprises in the current domestic polyacrylonitrile-based carbonization process, provides important process data for expanding the production scale, and provides a process debugging idea.
[0036] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 These are electron microscope photos of the polyacrylonitrile-based carbon fibers prepared in Example 1 at different positions and different magnifications. DETAILED DESCRIPTION
[0038] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.
[0039] The present invention reduces the production cost of carbon fiber by increasing the fiber running speed of the pre-oxidation carbonization process route, reducing the pre-oxidation time and carbonization time, and at the same time reduces the pre-oxidation time and ensures the pre-oxidation degree of the fiber by controlling the pre-oxidation temperature and its distribution gradient, tension drafting. In addition, in addition to the carbonization temperature, the application of drafting is also very important as a factor affecting the carbonization process. Under the action of the drafting force, the graphite layers are arranged along the fiber axis, and the preferred orientation is further improved, thereby greatly improving the modulus. The carbonization time is effectively reduced by matching the carbonization temperature and the drafting.
[0040] The embodiment of the present invention provides a method for preparing polyacrylonitrile-based carbon fiber, which comprises the following steps:
[0041] Pre-oxidation treatment: pre-oxidation treatment is performed on the polyacrylonitrile-based fiber to obtain pre-oxidized fiber; wherein the bulk density of the polyacrylonitrile-based fiber (raw fiber) is 1.185-1.195 g / cm 3 , polyacrylonitrile-based fibers (raw fibers) with a diameter of 8 to 12 μm.
[0042] Low-temperature carbonization treatment: performing low-temperature carbonization treatment on the pre-oxidized fiber to obtain low-temperature carbonized fiber;
[0043] High-temperature carbonization treatment: subjecting the low-temperature carbonized fiber to high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fiber;
[0044] In the process of pre-oxidation treatment, low-temperature carbonization treatment and high-temperature carbonization treatment, the fiber running speed is 600-900 m / h.
[0045] Here, the above steps need to be explained as follows:
[0046] First, about pre-oxidation treatment:
[0047] The pre-oxidation gradient temperature is an important parameter of the pre-oxidation process. Whether or not an excellent pre-oxidation fiber suitable for carbonization can be prepared, the gradient temperature is a key, and the range of the gradient temperature, that is, the setting of the pre-oxidation start and end temperatures, is the first problem to be solved. If the starting temperature is too low, it will not contribute to the pre-oxidation process, and it will take time and increase the cost. However, if the starting temperature is too high, the violent reaction exotherm will cause the PAN macromolecular chain without heat resistance to melt. If the ending temperature is too high, the concentrated heat release will destroy the structure of the pre-oxidation fiber and cause excessive pre-oxidation, which is not conducive to the preparation of high-strength carbon fiber. However, if the ending temperature is too low, the precursor may not be fully pre-oxidized. The inventor of the present invention has found through research that the exothermic reaction of general polyacrylonitrile-based fibers (i.e., precursors) starts at about 200°C, indicating that the cyclization and oxidation reactions begin. The heat release is slow at first, and the heat release rate increases at 220°C. As the temperature rises further, the cyclization and oxidation reactions become more and more intense, so that after 240°C, the heat release rate increases rapidly and reaches a maximum value at 290°C. The fiber also begins to lose a lot of weight. In view of the above research results, the present invention sets the starting temperature of the pre-oxidation temperature gradient at about 250°C. In order to avoid damage to the fiber caused by intense heat release, the ending temperature of the gradient temperature should be lower than the intense thermal weight loss temperature of 290°C.
[0048] According to the above analysis, the temperature gradient and draft of the pre-oxidation treatment are matched and designed:
[0049] In the pre-oxidation step, the polyacrylonitrile fiber is sequentially subjected to the first pre-oxidation temperature zone, the second pre-oxidation temperature zone, the third pre-oxidation temperature zone, and the fourth pre-oxidation temperature zone for pre-oxidation treatment to obtain pre-oxidized fiber. The temperature of the first pre-oxidation temperature zone is 250-255°C, and the total draft ratio applied to the fiber is 2%-3%; the temperature of the second pre-oxidation temperature zone is 256-260°C, and the total draft ratio applied to the fiber is 0%-2%; the temperature of the third pre-oxidation temperature zone is 261-264°C, and the total draft ratio applied to the fiber is -2.0%-0%; the temperature of the fourth pre-oxidation temperature zone is 265-275°C, and the total draft ratio applied to the fiber is -4.0%-2.0%.
[0050] When the polyacrylonitrile fiber passes through the first pre-oxidation temperature zone, the color of the fiber gradually changes from white to light yellow and then gradually to dark yellow; when passing through the second pre-oxidation temperature zone, the color of the fiber gradually changes from dark yellow to brown-black; when passing through the third pre-oxidation temperature zone, the color of the fiber gradually changes from brown-black to black; when passing through the fourth pre-oxidation temperature zone, the black color of the fiber gradually deepens.
[0051] Through reasonable oxidation temperature zone setting and optimized distribution of temperature zone drafting ratio, precise control of the tension of each layer can be achieved, which can effectively reduce the fiber discrete coefficient and ensure the structural formation of the pre-oxidized yarn.
[0052] Preferably, taking each pre-oxidation temperature zone as seven layers, the filament bundle enters from the first layer, and then passes through the second layer, the third layer, the fourth layer, the fifth layer, the sixth layer, and the seventh layer in sequence before exiting the pre-oxidation temperature zone. The tension control of the four temperature zones is shown in Table 1.
[0053] Table 1
[0054] The first pre-oxidation temperature zone CN First floor 718~762 Second floor 797~831 Third floor 837~846 Fourth floor 942~954 Fifth floor 967~980 Sixth floor 1012~1073 Seventh floor 1008~1019 The second pre-oxidation temperature zone First floor 904~971 Second floor 986~1072 Third floor 1013~1083 Fourth floor 1143~1191 Fifth floor 1121~1168 Sixth floor 1208~1239 Seventh floor 1220~1254 The third and oxidation temperature zone First floor 1233~1253 Second floor 1318~1334 Third floor 1308~1315 Fourth floor 1403~1415 Fifth floor 1415~1438 Sixth floor 1434~1458 Seventh floor 1467~1497 Fourth pre-oxidation temperature zone First floor 1316~1362 Second floor 1365~1400 Third floor 1400~1432 Fourth floor 1422~1442 Fifth floor 1438~1466 Sixth floor 1456~1486 Seventh floor 1486~1500
[0055] Here, the formic acid solubility of the pre-oxidized fiber is finally controlled to 1.0% to 5.0%. The mechanical properties of the pre-oxidized fiber are shown in Table 2:
[0056] Table 2
[0057] <![CDATA[Body density / g·cm -3 > Tensile strength / MPa Elongation at break / % Elastic modulus / Gpa 1.360~1.365 385~410 7.5~8.5 10~11
[0058] In addition, the formic acid solubility of pre-oxidized fiber is explained as follows: In the preparation process of carbon fiber, pre-oxidation treatment is a key link that affects the performance of carbon fiber. The plastic PAN linear molecular chain undergoes molecular cyclization, intermolecular cross-linking and oxidation reactions, and is converted into a non-plastic heat-resistant trapezoidal structure. In this process, due to the rapid cyclization of the outer layer of the fiber to form a dense structure, the transmission of oxygen molecules along the radial direction of the fiber to the inside of the fiber is hindered, so that there is a difference in the degree of pre-oxidation between the outer layer and the inside of the fiber. This difference in the degree of pre-oxidation between the skin and the inside is the skin-core structure. In the subsequent carbonization process, the core with a low degree of oxidation forms more defects, which ultimately affects the performance of the carbon fiber. The pre-oxidized fiber that has been converted into a heat-resistant trapezoidal structure is no longer dissolved in the formic acid solution, and the unconverted one is still dissolved in the formic acid solution. The calculated results can accurately reflect the oxidation degree of the pre-oxidized fiber, and provide accurate and quantitative guidance for the adjustment of pre-oxidation process parameters in industrial production.
[0059] In addition, the present invention adopts a side-blown hot air circulation oxidation furnace, which is perpendicular to the filament bundle and provides the oxygen required for the pre-oxidation of polyacrylonitrile precursor, which is conducive to instantly taking away small molecules and heat from chemical reactions, improving the pre-oxidation efficiency and shortening the pre-oxidation time. The circulating air volume of the oxidation furnace is 200,000-300,000m 3 / h, corresponding to a wind speed of 2-3m / s.
[0060] The present invention adopts a relatively high pre-oxidation starting temperature to quickly reach the effective pre-oxidation temperature of polyacrylonitrile fiber (raw fiber), shortening the pre-oxidation time, and staying in each temperature zone for 7.5 to 9 minutes. The present invention precisely controls the tension of each layer of pre-oxidized fiber to avoid the generation of fiber hair or broken fibers, thereby achieving continuous and stable production.
[0061] Second, about low temperature carbonization treatment:
[0062] Fully pre-oxidized fibers are the prerequisite for producing high-performance carbon fibers. Low-temperature carbonization treatment is the bridge to high-temperature carbonization. At this stage, non-carbon elements in the pre-oxidized fiber structure are gradually removed, and the pre-oxidized fibers are cross-linked with a small trapezoidal structure to initially form a carbon network. The low-temperature carbonization treatment of the present invention adopts 6 temperature zones: 420-450°C, 460-490°C, 500-520°C, 530-570°C, 600-700°C, 700-800°C, because the NH generated by low-carbon cracking 3 The concentrated heat release temperature of HCN is 300-600℃, the concentrated heat release temperature of HCN is 300-500℃, the thermal decomposition temperature of the original silk oil is usually 300-500℃, the process temperature design exhaust gas discharge point is usually set at 300-520℃, and the setting position is between temperature zone 1 and temperature zone 2. The low carbon temperature is set to ensure that the exhaust gas and oligomers generated by low temperature carbonization can be discharged instantly to avoid reducing the strength of the fiber after high temperature carbonization. The residence time in each temperature zone is 12-20s, the low temperature carbonization draft is controlled at 0-5%, and the low carbon fiber tension is controlled to 1200-1500CN. The large draft ratio makes the microcrystals in the low carbon fiber structure more closely combined with each other, and the fiber densification degree is higher, so that the fiber structure is more uniform, which is conducive to the improvement of the mechanical properties of carbon fiber.
[0063] Third, about high temperature carbonization treatment:
[0064] The carbon network formed in the early stage grows further during the high-temperature carbonization process, and undergoes a polycondensation reaction. The intermolecular force inside the fiber is further enhanced, so that the strength of the low-carbon filament is instantly increased after high-temperature carbonization. The final modulus of the carbon fiber is jointly affected by the temperature in the highest temperature zone of high-temperature carbonization and the high-temperature carbonization drawing ratio. Because under the action of a suitable drawing ratio, the preferred orientation of the graphite layer along the fiber axis is further improved.
[0065] The high carbon furnace usually has the highest temperature in the middle section and relatively low temperatures at both ends, which plays a role in maintaining the high temperature in the middle section. High temperature carbonization is controlled in four temperature zones: 1000-1200°C, 1300-1400°C, 1400-1500°C, and 1200-1300°C. The main component released by the reaction during the high temperature carbonization process is N 2 , N 2 The release is concentrated at 1000-1200℃, and the exhaust gas emission point is generally set between 1000-1200℃, which is conducive to the instantaneous discharge of oligomers, reducing the generation of hairy fibers and improving the strength of carbon fibers. The residence time in each temperature zone is 12-15s, the draft ratio is -4.0-0.0%, and the carbon fiber tension is controlled to 1900-2200CN.
[0066] The average mechanical properties of the final carbon fibers obtained after low-temperature carbonization treatment are shown in Table 3 after high-temperature carbonization treatment under the above process conditions, surface treatment, washing, sizing, drying, winding, etc.
[0067] Table 3
[0068]
[0069] What needs to be explained about the above steps of the present invention is that the present invention achieves a residence time of 12-20s in each temperature zone of low-temperature carbonization treatment and 48-60s in high-temperature carbonization treatment (the residence time in each temperature zone is 12-15s) through the temperature zone setting of low-temperature carbonization treatment and high-temperature carbonization treatment. The present invention avoids the generation of fiber filaments or broken fibers and realizes continuous and stable production through precise tension control of low-temperature carbonization treatment and high-temperature carbonization treatment (setting the tension value through a tension sensor and the speed difference of the front and rear drafting rollers). The pre-oxidation process of the present invention significantly shortens the time consumption, effectively reduces energy consumption, realizes rapid pre-oxidation and carbonization with low cost and high yield, and greatly reduces industrial production costs. The strength of the carbon fiber formed after carbonization treatment reaches above 5.49Gpa, and has excellent quality.
[0070] The advantage of the present invention is that by adjusting the temperature range and temperature gradient of the pre-oxidation temperature zone and the stretch ratio value, by adjusting the low-temperature carbonization treatment, the high-temperature carbonization treatment and optimizing the stretch ratio, a total oxidation residence time of 30 to 38 minutes, a low-temperature carbonization residence time of 72 to 90 seconds, and a high-temperature carbonization residence time of 12 to 15 seconds in each temperature zone can be achieved, thereby providing important process parameters and debugging ideas for later industrial large-scale production of 1,000 tons or even 10,000 tons, reducing the production costs of enterprises, and improving the competitiveness and survival ability of enterprises.
[0071] In summary, the present invention has successfully developed a new rapid pre-oxidation carbonization process by formulating a reasonable process technology route on the existing production line, and applied it to the actual production of T800. The average strength of the produced carbon filaments is 5.59GPa, the apparent modulus is 232GPa, the CV value of the mechanical properties of the carbon filaments is within 5%, the performance of the uniaxial carbon filaments is stable in the long-range direction, and the full-load operation of the production line is not affected by the station effect. The self-produced carbon fiber has excellent performance in various aspects, which fully meets the needs of customers for composite materials, solves the long-term technical bottleneck of high energy consumption and low operating speed of domestic carbon fiber, reduces the production cost of the enterprise, and can provide positive and beneficial ideas for the production process debugging for the future expansion of production scale, accumulate a large amount of process data and debugging experience, and indicate the debugging direction.
[0072] The present invention is further described below through specific experimental examples and comparative examples:
[0073] Example 1
[0074] The bulk density of this embodiment is 1.185-1.195 g / cm 3 6K polyacrylonitrile-based fiber (precursor) with a diameter of 8 μm and a linear density of 890-920 g / km is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to prepare polyacrylonitrile-based carbon fiber. The main steps are as follows:
[0075] Pre-oxidation treatment steps: the polyacrylonitrile fiber (raw fiber) is firstly introduced into the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at a speed of 600 m / h. In the air atmosphere, the chemical reaction just begins to occur. In order to prevent the raw fiber from physical shrinkage and improve the orientation degree of the fiber, the tension of each layer in the No. 1 pre-oxidation temperature zone is controlled according to the data in Table 1, and the total draft ratio of the No. 1 pre-oxidation temperature zone is controlled at 3%. Then, the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 256°C, the cyclization reaction is accelerated, the fiber color is deepened, the total draft ratio is controlled at 2%, and the single-layer draft ratio of the No. 2 pre-oxidation temperature zone decreases layer by layer to ensure that the tension increases smoothly layer by layer. Then it enters the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone), which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature of the No. 3 pre-oxidation temperature zone is controlled at 261°C, the total draft ratio is controlled at 0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer, so that the chemical reaction proceeds smoothly; finally, it enters the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), which determines the performance of the final pre-oxidation yarn and is the most sensitive area for chemical reactions. Here, the gradient difference between the No. 4 pre-oxidation temperature zone and the No. 3 pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and leading to the formation of an obvious skin-core structure. The temperature of the No. 4 pre-oxidation temperature zone is controlled at 265°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total draft ratio is controlled at -2.0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer. Among them, the residence time of the fiber in each pre-oxidation temperature zone is 9 minutes, and the formic acid solubility of the pre-oxidized fiber is controlled to 1.3% to 1.5%.
[0076] The mechanical properties of the pre-oxidized fibers prepared by the above process are shown in Table 4:
[0077] Table 4
[0078]
[0079] Low temperature carbonization treatment and high temperature carbonization treatment steps: The pre-oxidized fiber is subjected to low temperature carbonization treatment, high temperature carbonization treatment and subsequent process forming to obtain polyacrylonitrile-based carbon fiber. Among them, the draft ratio of the low temperature carbonization treatment is 0%, and the tension control of the low temperature carbonization treatment is 1200CN. The draft ratio of the high temperature carbonization treatment is -4.0%, and the tension control of the high temperature carbonization treatment is 1900CN. Among them, the temperature zone of the low temperature carbonization treatment and the temperature zone of the high temperature carbonization treatment are designed as shown in Table 5:
[0080] Table 5
[0081]
[0082] The self-produced polyacrylonitrile-based carbon fiber was wound and the mechanical properties of the carbon fiber were tested using a universal material testing machine. The average value of ten groups of samples was taken, and the density of the carbon fiber was tested using the density gradient method. The test results are shown in Table 6:
[0083] Table 6
[0084]
[0085] Figure 1 This is an electron microscope photo of the polyacrylonitrile-based carbon fiber prepared in Example 1. It can be seen that the diameter of the single fiber of the polyacrylonitrile-based carbon fiber is 5-6 μm, and there are grooves on the fiber surface. The carbon content and other contents of the high-performance polyacrylonitrile carbon fiber prepared in Example 1 are shown in Table 7.
[0086] Table 7
[0087]
[0088] It can be seen from Table 7 that the polyacrylonitrile-based carbon fiber prepared by the present invention has significantly reduced ash content compared with the T800 standard sample, and other indicators are equivalent. It should be noted that the present invention uses low-temperature carbonization treatment and high-temperature carbonization treatment processes to instantly discharge waste gas and oligomers generated by low-temperature carbonization and high-temperature carbonization, completely remove the raw fiber oiling agent, reduce the generation of impurities, and reduce the ash content.
[0089] Therefore, the preparation method of polyacrylonitrile-based carbon fiber provided in the embodiment of the present invention shortens the total residence time of the pre-oxidation treatment, greatly shortens the residence time, thereby greatly reducing energy consumption and production costs; at the same time, it also ensures the performance of the polyacrylonitrile-based carbon fiber.
[0090] Example 2
[0091] The bulk density of this embodiment is 1.185-1.195 g / cm 36K polyacrylonitrile-based fiber (precursor) with a diameter of 8 μm and a linear density of 890-920 g / km is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to prepare polyacrylonitrile-based carbon fiber. The main steps are as follows:
[0092] Pre-oxidation treatment steps: the polyacrylonitrile fiber (raw fiber) first enters the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at 255°C at a speed of 900m / h. In the air atmosphere, the chemical reaction just begins to occur. In order to prevent the raw fiber from physical shrinkage and improve the orientation degree of the fiber, the tension of each layer in the No. 1 pre-oxidation temperature zone is controlled according to the data in Table 1, and the total draft ratio of the No. 1 pre-oxidation temperature zone is controlled at 2%. Then, the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 260°C, the cyclization reaction is accelerated, the fiber color is deepened, the total draft ratio is controlled at 0%, and the single-layer draft ratio of the No. 2 pre-oxidation temperature zone decreases layer by layer to ensure that the tension increases smoothly layer by layer. Then enter the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone), which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature of the No. 3 pre-oxidation temperature zone is controlled at 264°C, the total draft ratio is controlled at -2%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer, so that the chemical reaction proceeds smoothly; finally enter the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), which determines the performance of the final pre-oxidation yarn and is the most sensitive area for chemical reactions. Here, the gradient difference between the No. 4 pre-oxidation temperature zone and the No. 3 pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and leading to the formation of an obvious skin-core structure. The temperature of the No. 4 pre-oxidation temperature zone is controlled at 275°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total draft ratio is controlled at -4.0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer. Among them, the fiber stays in each pre-oxidation temperature zone for 7.5 minutes, and the formic acid solubility of the pre-oxidized fiber is controlled to 2.5% to 3.5%.
[0093] The mechanical properties of the pre-oxidized fibers prepared by the above process are shown in Table 8:
[0094] Table 8
[0095]
[0096] Low temperature carbonization treatment and high temperature carbonization treatment steps: The pre-oxidized fiber is subjected to low temperature carbonization treatment, high temperature carbonization treatment and subsequent process forming to obtain polyacrylonitrile-based carbon fiber. Among them, the draft ratio of the low temperature carbonization treatment is 0%, and the tension control of the low temperature carbonization treatment is 1200CN. The draft ratio of the high temperature carbonization treatment is -4.0%, and the tension control of the high temperature carbonization treatment is 1900CN. Among them, the temperature zone of the low temperature carbonization treatment and the temperature zone of the high temperature carbonization treatment are designed as shown in Table 9:
[0097] Table 9
[0098]
[0099] The self-produced polyacrylonitrile-based carbon fiber was wound and the mechanical properties of the carbon fiber were tested using a universal material testing machine. The average value of ten groups of samples was taken, and the density of the carbon fiber was tested using the density gradient method. The test results are shown in Table 10:
[0100] Table 10
[0101]
[0102] Example 3
[0103] The bulk density of this embodiment is 1.185-1.195 g / cm 3 6K polyacrylonitrile-based fiber (precursor) with a diameter of 8 μm and a linear density of 890-920 g / km is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to prepare polyacrylonitrile-based carbon fiber. The main steps are as follows:
[0104] Pre-oxidation treatment steps: the polyacrylonitrile fiber (raw fiber) is firstly introduced into the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at a speed of 600 m / h. In the air atmosphere, the chemical reaction just begins to occur. In order to prevent the raw fiber from physical shrinkage and improve the orientation degree of the fiber, the tension of each layer in the No. 1 pre-oxidation temperature zone is controlled according to the data in Table 1, and the total draft ratio of the No. 1 pre-oxidation temperature zone is controlled at 3%. Then, the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 256°C, the cyclization reaction is accelerated, the fiber color is deepened, the total draft ratio is controlled at 2%, and the single-layer draft ratio of the No. 2 pre-oxidation temperature zone decreases layer by layer to ensure that the tension increases smoothly layer by layer. Then it enters the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone), which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature of the No. 3 pre-oxidation temperature zone is controlled at 261°C, the total draft ratio is controlled at 0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer, so that the chemical reaction proceeds smoothly; finally, it enters the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), which determines the performance of the final pre-oxidation yarn and is the most sensitive area for chemical reactions. Here, the gradient difference between the No. 4 pre-oxidation temperature zone and the No. 3 pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and leading to the formation of an obvious skin-core structure. The temperature of the No. 4 pre-oxidation temperature zone is controlled at 265°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total draft ratio is controlled at -2.0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer. Among them, the residence time of the fiber in each pre-oxidation temperature zone is 9 minutes, and the formic acid solubility of the pre-oxidized fiber is controlled to 1.3% to 1.5%.
[0105] The mechanical properties of the pre-oxidized fibers prepared by the above process are shown in Table 11:
[0106] Table 11
[0107]
[0108] Low-temperature carbonization treatment and high-temperature carbonization treatment steps: The pre-oxidized fiber is subjected to low-temperature carbonization treatment, high-temperature carbonization treatment and subsequent process forming to obtain polyacrylonitrile-based carbon fiber. Among them, the draft ratio of the low-temperature carbonization treatment is 5%, and the tension control of the low-temperature carbonization treatment is 1500CN. The draft ratio of the high-temperature carbonization treatment is -4.0%, and the tension control of the high-temperature carbonization treatment is 1900CN. Among them, the temperature zone of the low-temperature carbonization treatment and the temperature zone of the high-temperature carbonization treatment are designed as shown in Table 12:
[0109] Table 12
[0110]
[0111] The self-produced polyacrylonitrile-based carbon fiber was wound and the mechanical properties of the carbon fiber were tested using a universal material testing machine. The average value of ten groups of samples was taken, and the density of the carbon fiber was tested using the density gradient method. The test results are shown in Table 13:
[0112] Table 13
[0113]
[0114] Example 4
[0115] The bulk density of this embodiment is 1.185-1.195 g / cm 3 6K polyacrylonitrile-based fiber (precursor) with a diameter of 8 μm and a linear density of 890-920 g / km is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to prepare polyacrylonitrile-based carbon fiber. The main steps are as follows:
[0116] Pre-oxidation treatment steps: the polyacrylonitrile fiber (raw fiber) is firstly introduced into the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at a speed of 600 m / h. In the air atmosphere, the chemical reaction just begins to occur. In order to prevent the raw fiber from physical shrinkage and improve the orientation degree of the fiber, the tension of each layer in the No. 1 pre-oxidation temperature zone is controlled according to the data in Table 1, and the total draft ratio of the No. 1 pre-oxidation temperature zone is controlled at 3%. Then, the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 256°C, the cyclization reaction is accelerated, the fiber color is deepened, the total draft ratio is controlled at 2%, and the single-layer draft ratio of the No. 2 pre-oxidation temperature zone decreases layer by layer to ensure that the tension increases smoothly layer by layer. Then it enters the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone), which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature of the No. 3 pre-oxidation temperature zone is controlled at 261°C, the total draft ratio is controlled at 0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer, so that the chemical reaction proceeds smoothly; finally, it enters the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), which determines the performance of the final pre-oxidation yarn and is the most sensitive area for chemical reactions. Here, the gradient difference between the No. 4 pre-oxidation temperature zone and the No. 3 pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and leading to the formation of an obvious skin-core structure. The temperature of the No. 4 pre-oxidation temperature zone is controlled at 265°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total draft ratio is controlled at -2.0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer. Among them, the residence time of the fiber in each pre-oxidation temperature zone is 9 minutes, and the formic acid solubility of the pre-oxidized fiber is controlled to 1.3% to 1.5%.
[0117] The mechanical properties of the pre-oxidized fibers prepared by the above process are shown in Table 14:
[0118] Table 14
[0119]
[0120] Low temperature carbonization treatment and high temperature carbonization treatment steps: The pre-oxidized fiber is subjected to low temperature carbonization treatment, high temperature carbonization treatment and subsequent process forming to obtain polyacrylonitrile-based carbon fiber. Among them, the draft ratio of the low temperature carbonization treatment is 5%, and the tension control of the low temperature carbonization treatment is 1500CN. The draft ratio of the high temperature carbonization treatment is 0%, and the tension control of the high temperature carbonization treatment is 2200CN. Among them, the temperature zone of the low temperature carbonization treatment and the temperature zone of the high temperature carbonization treatment are designed as shown in Table 15:
[0121] Table 15
[0122]
[0123] The self-produced polyacrylonitrile-based carbon fiber was wound and the mechanical properties of the carbon fiber were tested using a universal material testing machine. The average value of ten groups of samples was taken, and the density of the carbon fiber was tested using the density gradient method. The test results are shown in Table 16:
[0124] Table 16
[0125]
[0126] Example 5
[0127] The bulk density of this embodiment is 1.185-1.195 g / cm 3 6K polyacrylonitrile-based fiber (precursor) with a diameter of 8 μm and a linear density of 890-920 g / km is subjected to pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment to prepare polyacrylonitrile-based carbon fiber. The main steps are as follows:
[0128] Pre-oxidation treatment steps: the polyacrylonitrile fiber (raw fiber) is firstly introduced into the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at a speed of 600 m / h. In the air atmosphere, the chemical reaction just begins to occur. In order to prevent the raw fiber from physical shrinkage and improve the orientation degree of the fiber, the tension of each layer in the No. 1 pre-oxidation temperature zone is controlled according to the data in Table 1, and the total draft ratio of the No. 1 pre-oxidation temperature zone is controlled at 3%. Then, the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 256°C, the cyclization reaction is accelerated, the fiber color is deepened, the total draft ratio is controlled at 2%, and the single-layer draft ratio of the No. 2 pre-oxidation temperature zone decreases layer by layer to ensure that the tension increases smoothly layer by layer. Then it enters the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone), which is a violent reaction zone. The oxidation reaction begins to dominate the cyclization reaction. In order to prevent the premature formation of the skin-core structure, the temperature of the No. 3 pre-oxidation temperature zone is controlled at 261°C, the total draft ratio is controlled at 0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer, so that the chemical reaction proceeds smoothly; finally, it enters the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), which determines the performance of the final pre-oxidation yarn and is the most sensitive area for chemical reactions. Here, the gradient difference between the No. 4 pre-oxidation temperature zone and the No. 3 pre-oxidation temperature zone cannot be large to prevent the heating rate from being too fast, affecting the double diffusion of oxygen, and leading to the formation of an obvious skin-core structure. The temperature of the No. 4 pre-oxidation temperature zone is controlled at 265°C, and each layer adopts negative drafting to facilitate full fiber oxidation. The total draft ratio is controlled at -2.0%, and the draft ratio of each layer in the oxidation temperature zone decreases layer by layer. Among them, the residence time of the fiber in each pre-oxidation temperature zone is 9 minutes, and the formic acid solubility of the pre-oxidized fiber is controlled to 1.3% to 1.5%.
[0129] The mechanical properties of the pre-oxidized fibers prepared by the above process are shown in Table 17:
[0130] Table 17
[0131]
[0132] Low temperature carbonization treatment and high temperature carbonization treatment steps: The pre-oxidized fiber is subjected to low temperature carbonization treatment, high temperature carbonization treatment and subsequent process forming to obtain polyacrylonitrile-based carbon fiber. Among them, the draft ratio of the low temperature carbonization treatment is 5%, and the tension control of the low temperature carbonization treatment is 1500CN. The draft ratio of the high temperature carbonization treatment is -0.0%, and the tension control of the high temperature carbonization treatment is 2200CN. Among them, the temperature zone of the low temperature carbonization treatment and the temperature zone of the high temperature carbonization treatment are designed as shown in Table 18:
[0133] Table 18
[0134]
[0135] The self-produced polyacrylonitrile-based carbon fiber was wound and the mechanical properties of the carbon fiber were tested using a universal material testing machine. The average value of ten groups of samples was taken, and the density of the carbon fiber was tested using the density gradient method. The test results are shown in Table 19:
[0136] Table 19
[0137]
[0138] Comparing Example 1 to Example 5, the fiber running speed is 600-900m / h, the temperature of the first pre-oxidation temperature zone is controlled at 250-255℃, the total draft ratio is controlled at 2-3%, and the fiber color changes from white to light yellow and then gradually to dark yellow; the temperature of the second pre-oxidation temperature zone is controlled at 256-260℃, the total draft ratio is controlled at 0.0-2%, and the fiber color gradually changes to brown-black; the temperature of the third pre-oxidation temperature zone is controlled at 261-264℃, the total draft ratio is -2.0-0.0%, and the fiber color becomes black; the temperature of the fourth pre-oxidation temperature zone is controlled at 265-275℃, the total draft ratio is -4.0-2.0%, and the degree of black is further deepened. Each pre-oxidation temperature zone stays for 7.5-9min. Through the above-mentioned reasonable pre-oxidation temperature zone setting and the optimized distribution of the draft ratio of the temperature zone, the precise control of the tension of each layer is achieved. The low-temperature carbonization temperature is set to ensure that the waste gas and oligomers generated by low-temperature carbonization can be discharged instantly to avoid reducing the strength of the fiber after high-temperature carbonization. The residence time in each temperature zone is 12 to 20 seconds. The draft of low-temperature carbonization is controlled at 0 to 5%, and the tension of low-temperature carbonization is controlled to 1200 to 1500. The high-temperature carbonization treatment adopts 4 temperature zones: 1000 to 1200°C, 1300 to 1400°C, 1400 to 1500°C, and 1200 to 1300°C. The main component released by the reaction during the high-temperature carbonization treatment is N 2 , N 2The release is concentrated at 1000-1200℃, and the exhaust gas emission point is generally set between 1000-1200℃, which is conducive to the instantaneous discharge of oligomers, reducing the generation of hair, and improving the strength of carbon fibers. The residence time of each high-temperature carbonization temperature zone is 12-15s, the draft ratio is -4.0%-0.0%, and the carbon fiber tension is controlled to 1900-2200CN. The strength of the carbon fiber formed after carbonization reaches more than 5.49Gpa, and the strength CV is below 5, which has excellent quality.
[0139] Comparative Example 1
[0140] Comparative Example 1 prepares a polyacrylonitrile-based carbon fiber, which differs from Example 1 in that the pre-oxidation treatment step is different. Other steps (low-temperature carbonization treatment, high-temperature carbonization treatment) and parameters are consistent with Example 1.
[0141] The conventional pre-oxidation process used in the pre-oxidation step of Comparative Example 1 is as follows:
[0142] The starting temperature of pre-oxidation is 230°C, the ending temperature is 260°C, and the temperature gradient is 10°C. The running speed of the tow is 200m / h. The total time of pre-oxidation treatment is 75min. The total draft ratio of pre-oxidation treatment is 3%.
[0143] The bulk density of the pre-oxidized fiber prepared in Comparative Example 1 is 1.34-1.36 g.cm - 3. The strength of the carbon fiber product obtained after the pre-oxidized fiber is treated by low-temperature carbonization and high-temperature carbonization is 5075MPa, and the strength CV value is 2.4%.
[0144] Comparative Example 2
[0145] Comparative Example 2 prepares a polyacrylonitrile-based carbon fiber, which differs from Example 1 in that the pre-oxidation treatment step is different, while the other steps and parameters are the same.
[0146] The conventional pre-oxidation process used in the pre-oxidation step of Comparative Example 2 is as follows:
[0147] The starting temperature of pre-oxidation is 200°C, the ending temperature is 260°C, and the temperature gradient is 15°C. The running speed of the tow is 180m / h. The total time of pre-oxidation treatment is 120min. The total draft ratio of pre-oxidation treatment is 3%.
[0148] Among them, the bulk density of the pre-oxidized fiber prepared in Comparative Example 2 is 1.34-1.36 g.cm - 3. The strength of the carbon fiber product obtained after the pre-oxidized fiber is treated by low-temperature carbonization and high-temperature carbonization is 4975MPa, and the strength CV value is 3.2%.
[0149] Comparative Example 3
[0150] Comparative Example 3 prepares a polyacrylonitrile-based carbon fiber, which differs from Example 1 in that the pre-oxidation treatment step is different, while the other steps and parameters are the same.
[0151] The pre-oxidation treatment steps of Comparative Example 3 are as follows:
[0152] The starting temperature of pre-oxidation is 235°C, the ending temperature is 265°C, and the temperature gradient is 10°C. The running speed of the tow is 420m / h. The total time of pre-oxidation treatment is 60min. The total draft ratio of pre-oxidation treatment is 3%.
[0153] Among them, the bulk density of the pre-oxidized fiber prepared in Comparative Example 3 is 1.34-1.36 g.cm - 3. The strength of the carbon fiber product obtained after the pre-oxidized fiber is treated by low-temperature carbonization and high-temperature carbonization is 5119 MPa, and the strength CV value is 3.1%.
[0154] By comparing Example 1 and Comparative Examples 1 to 3, it can be seen that: compared with the embodiments of the present invention, the total pre-oxidation time of the traditional pre-oxidation process adopted in the comparative examples is relatively long, resulting in a higher preparation cost; and the pre-oxidized fiber prepared by the traditional pre-oxidation process used in the comparative examples, the carbon fiber strength formed after carbonization is not as good as the carbon fiber strength of the embodiments of the present invention.
[0155] Comparative Example 4
[0156] Comparative Example 4 prepares a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the pre-oxidation treatment step is different. Other steps and parameters are the same.
[0157] The conventional pre-oxidation process used in the pre-oxidation step of Comparative Example 4 is as follows:
[0158] The starting temperature of pre-oxidation is 260°C, the ending temperature is 280°C, and the temperature gradient is 5°C. The running speed of the tow is 720m / h. The total time of pre-oxidation treatment is 30min. Among them, in the first pre-oxidation temperature zone, the total draft ratio applied to the fiber is 2% to 3%; in the second pre-oxidation temperature zone, the total draft ratio applied to the fiber is 0% to 2%; in the third pre-oxidation temperature zone, the total draft ratio applied to the fiber is -2.0% to 0%; in the fourth pre-oxidation temperature zone, the total draft ratio applied to the fiber is -4.0% to -2.0%. The total draft of pre-oxidation is -4% to 3%. The tension of each layer is not controlled.
[0159] Among them, the bulk density of the pre-oxidized fiber prepared in Comparative Example 4 is 1.34-1.36 g.cm - 3. The strength of the carbon fiber product obtained after the pre-oxidized fiber is treated by low-temperature carbonization and high-temperature carbonization is 4924MPa, and the strength CV value is 5.6%.
[0160] By comparing Example 1 and Comparative Example 4, it can be seen that when the starting temperature and the ending temperature of the pre-oxidation treatment in Comparative Example 4 are too high, although the total pre-oxidation time is reduced, the strength of the carbon fiber formed after the carbonization of the pre-oxidized fiber decreases significantly, the CV value increases significantly, and the strength fluctuates greatly.
[0161] Comparative Example 5
[0162] Comparative Example 5 prepares a polyacrylonitrile-based carbon fiber, which differs from Example 1 in that the pre-oxidation treatment steps are different, as follows:
[0163] Pre-oxidation treatment step: the polyacrylonitrile fiber (protofilament) first enters the No. 1 pre-oxidation temperature zone (i.e., the first pre-oxidation temperature zone) at 250°C at a speed of 600m / h, then the fiber enters the No. 2 pre-oxidation temperature zone (the second pre-oxidation temperature zone) at 256°C, then enters the No. 3 pre-oxidation temperature zone (the third pre-oxidation temperature zone) at 261°C, and finally enters the No. 4 pre-oxidation temperature zone (the fourth pre-oxidation temperature zone), and the residence time of the fiber in each pre-oxidation temperature zone is 9min. At the same time, the total draft ratio is controlled at -4.0% to -2.0%.
[0164] Other steps and parameters are consistent with those in Example 1.
[0165] Among them, the bulk density of the pre-oxidized fiber prepared in Comparative Example 5 is 1.34-1.36 g.cm - 3. The strength of the carbon fiber product obtained after the pre-oxidized fiber is treated by low-temperature carbonization and high-temperature carbonization is 4984MPa, and the strength CV value is 5.5%.
[0166] By comparing Example 1 and Comparative Example 5, it can be seen that: although the pre-oxidation temperature and residence time are the same, Comparative Example 1 does not accurately control the drafting in each temperature zone, so that the strength of the carbon fiber formed after the carbonization of the pre-oxidized fiber decreases significantly, the CV value increases significantly, and the strength fluctuates greatly.
[0167] Comparative Example 6
[0168] Comparative Example 6 prepares a polyacrylonitrile-based carbon fiber, which is different from Example 1 in that the pre-oxidation treatment step and the low-temperature carbonization step are the same. However, the high-temperature carbonization step is different. The temperature zones of the high-temperature carbonization treatment in Comparative Example 6 are 1000°C, 1150°C, 1350°C, and 1500°C, respectively, with a temperature gradient of 150°C.
[0169] The strength of the carbon fiber product prepared in Comparative Example 6 is 5494 MPa, and the strength CV value is 5.6%. In addition, the carbon content and other contents of the high-performance polyacrylonitrile carbon fiber prepared in Comparative Example 6 and Example 1 are shown in Table 20.
[0170] Table 20
[0171] content C(%) H(%) N(%) Ash Water absorption Example 1 95.21~95.90 0.272~0.310 3.240~3.428 0.116~0.154 0.01~0.02 Comparative Example 6 92.37~94.42 0.245~0.358 4.725~6.795 0.259~0.332 0.01~0.02
[0172] By comparing Example 1 and Comparative Example 6, Table 7 and Table 20, it can be seen that: under the same conditions of pre-oxidation treatment and low-temperature carbonization treatment, but without precise control of the temperature of the high-temperature carbonization treatment, the strength CV value of the carbon fiber is larger, the C% content is also reduced, and the ash content is increased (the temperature setting of the high-temperature carbonization treatment in Comparative Example 6 is not conducive to the removal of non-carbon units of waste gas oligomers, so the ash content is higher).
[0173] The above embodiments and comparative examples illustrate that the pre-oxidation step of the present invention can significantly improve the performance of polyacrylonitrile-based carbon fibers. On this basis, the carbonization step of the present invention can further improve the performance of polyacrylonitrile-based carbon fibers.
[0174] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A method for preparing polyacrylonitrile-based carbon fiber, characterized in that: It includes the following steps: Pre-oxidation treatment: pre-oxidation treatment is performed on the polyacrylonitrile-based fiber to obtain pre-oxidized fiber; Low-temperature carbonization treatment: performing low-temperature carbonization treatment on the pre-oxidized fiber to obtain low-temperature carbonized fiber; High-temperature carbonization treatment: subjecting the low-temperature carbonized fiber to high-temperature carbonization treatment to obtain polyacrylonitrile-based carbon fiber; Among them, during the pre-oxidation treatment, low-temperature carbonization treatment, and high-temperature carbonization treatment, the fiber running speed is 600-900 m / h; Among them, in the pre-oxidation treatment step: the polyacrylonitrile fiber is sequentially passed through a first pre-oxidation temperature zone, a second pre-oxidation temperature zone, a third pre-oxidation temperature zone, and a fourth pre-oxidation temperature zone for pre-oxidation treatment to obtain pre-oxidized fiber; wherein, in the first pre-oxidation temperature zone: the temperature is 250-255°C, and the total stretch ratio applied to the fiber is 2%-3%; in the second pre-oxidation temperature zone: the temperature is 256-260°C, and the total stretch ratio applied to the fiber is 0%-2%; in the third pre-oxidation temperature zone: the temperature is 261-264°C, and the total stretch ratio applied to the fiber is -2.0%-0%; in the fourth pre-oxidation temperature zone: the temperature is 265-275°C, and the total stretch ratio applied to the fiber is -4.0%-2.0%.
2. The method for preparing polyacrylonitrile-based carbon fiber according to claim 1, characterized in that: Each of the first pre-oxidation temperature zone, the second pre-oxidation temperature zone, the third pre-oxidation temperature zone, and the fourth pre-oxidation temperature zone is provided with multiple layers from bottom to top, so that the fiber passes through each pre-oxidation temperature zone layer by layer from bottom to top; wherein, when the fiber passes through each pre-oxidation temperature zone layer by layer, the tension applied to the fiber increases layer by layer, so that the draft ratio decreases layer by layer; Preferably, the tension in the latter pre-oxidation temperature zone is 100-200CN higher than that in the former pre-oxidation temperature zone.
3. The method for preparing polyacrylonitrile-based carbon fiber according to claim 1, characterized in that: When the polyacrylonitrile fiber passes through the first pre-oxidation temperature zone, the color of the fiber gradually changes from white to light yellow and then gradually to dark yellow; when passing through the second pre-oxidation temperature zone, the color of the fiber gradually changes from dark yellow to brown-black; when passing through the third pre-oxidation temperature zone, the color of the fiber gradually changes from brown-black to black; when passing through the fourth pre-oxidation temperature zone, the black color of the fiber gradually deepens.
4. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 3, characterized in that: In the first pre-oxidation temperature zone, the fiber tension is controlled at 718-1019CN by controlling the temperature and the draft ratio; In the second pre-oxidation temperature zone, the fiber tension is controlled at 904-1254CN by controlling the temperature and the draft ratio; In the third pre-oxidation temperature zone, the fiber tension is controlled within a range of 1233-1497 CN by controlling the temperature and the draft ratio; In the fourth pre-oxidation temperature zone, the fiber tension is controlled within a range of 1316-1500 CN by controlling the temperature and the draft ratio; Preferably, 7 temperature zones are arranged in sequence from bottom to top in the first pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 718-762CN, the tension of the fiber in the second temperature zone is 797-831CN, the tension of the fiber in the third temperature zone is 837-846CN, the tension of the fiber in the fourth temperature zone is 942-954CN, the tension of the fiber in the fifth temperature zone is 967-980CN, the tension of the fiber in the sixth temperature zone is 1012-1073CN, and the tension of the fiber in the seventh temperature zone is 1008-1019CN; Preferably, 7 temperature zones are sequentially arranged from bottom to top in the second pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 904-971CN, the tension of the fiber in the second temperature zone is 986-1072CN, the tension of the fiber in the third temperature zone is 1013-1083CN, the tension of the fiber in the fourth temperature zone is 1143-1191CN, the tension of the fiber in the fifth temperature zone is 1121-1168CN, the tension of the fiber in the sixth temperature zone is 1208-1239CN, and the tension of the fiber in the seventh temperature zone is 1220-1254CN; Preferably, 7 temperature zones are arranged in sequence from bottom to top in the third pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 1233-1253CN, the tension of the fiber in the second temperature zone is 1318-1334CN, the tension of the fiber in the third temperature zone is 1308-1315CN, the tension of the fiber in the fourth temperature zone is 1403-1415CN, the tension of the fiber in the fifth temperature zone is 1415-1438CN, the tension of the fiber in the sixth temperature zone is 1434-1458CN, and the tension of the fiber in the seventh temperature zone is 1467-1497CN; Preferably, 7 temperature zones are arranged from bottom to top in the fourth pre-oxidation temperature zone, the tension of the fiber in the first temperature zone is 1316-1362CN, the tension of the fiber in the second temperature zone is 1365-1400CN, the tension of the fiber in the third temperature zone is 1400-1432CN, the tension of the fiber in the fourth temperature zone is 1422-1442CN, the tension of the fiber in the fifth temperature zone is 1438-1466CN, the tension of the fiber in the sixth temperature zone is 1456-1486CN, and the tension of the fiber in the seventh temperature zone is 1486-1500CN.
5. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 4, characterized in that: The bulk density of the polyacrylonitrile fiber is 1.185-1.195 g / cm 3 , diameter is 8 to 12 μm.
6. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 5, characterized in that: The formic acid solubility of the pre-oxidized fiber is 1.0% to 5.0%, and the density of the pre-oxidized fiber body is 1.360 to 1.365 g / cm 3 , tensile strength is 385~410MPa, elongation at break is 7.5~8.5%, and elastic modulus is 10~11Gpa.
7. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 6, characterized in that: The total residence time of the pre-oxidation treatment is 30 to 38 minutes, and the residence time of the fiber in each pre-oxidation temperature zone is 7.5 to 9 minutes; and / or In the pre-oxidation step, the pre-oxidation furnace used is a side-blown hot air circulation oxidation furnace; wherein, during the pre-oxidation process: the circulating air volume of the oxidation furnace is controlled to be 200000-300000m 3 / h, wind speed is controlled at 2-3m / s.
8. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 7, characterized in that: During the low-temperature carbonization treatment: the pre-oxidized fiber is sequentially subjected to the first temperature zone, the second temperature zone, the third temperature zone, the fourth temperature zone, the fifth temperature zone, and the sixth temperature zone for low-temperature carbonization treatment to obtain low-temperature carbonized fiber; wherein the temperature of the first temperature zone is 420-450°C, the temperature of the second temperature zone is 460-490°C, the temperature of the third temperature zone is 500-520°C, the temperature of the fourth temperature zone is 530-570°C, the temperature of the fifth temperature zone is 600-700°C, and the temperature of the sixth temperature zone is 700-800°C; preferably, the residence time of the fiber in each temperature zone is 12-20s, and / or During the low-temperature carbonization treatment, the draft ratio applied to the fiber is 0-5%, and the tension applied to the fiber is 1200-1500CN.
9. The method for preparing polyacrylonitrile-based carbon fiber according to any one of claims 1 to 8, characterized in that: During the high-temperature carbonization treatment: the low-temperature carbonized fiber is sequentially subjected to high-temperature carbonization treatment in a first temperature zone, a second temperature zone, a third temperature zone, and a fourth temperature zone to obtain polyacrylonitrile-based carbon fiber; wherein the temperature of the first temperature zone is 1000-1200°C, the temperature of the second temperature zone is 1300-1400°C, the temperature of the third temperature zone is 1400-1500°C, and the temperature of the fourth temperature zone is 1200-1300°C; preferably, the residence time of the fiber in each temperature zone is 12-15s; and / or During the high-temperature carbonization treatment, the draft ratio applied to the fiber is -4.0 to 0%, and the tension applied to the fiber is 1900 to 2200 CN.
10. A polyacrylonitrile-based carbon fiber, characterized in that: The bulk density of the polyacrylonitrile-based carbon fiber is 1.790 to 1.810 g / cm 3 The strength is 1392~1450N, the tensile strength is 5.49~5.84Gpa, the elongation at break is 2.2~2.4%, and the tensile modulus is 230~238Gpa.
Citation Information
Cited By
Characterization method for ash morphology of carbon fiber
CN119619184A