Flexible conductive hydrophobic material and preparation method thereof

Through normal pressure plasma pretreatment and polydimethylsiloxane cross-linking film formation technology, the problems of uniform dispersion and unstable conductivity of liquid metals in flexible materials are solved, and efficient improvement of conductivity and hydrophobic properties are achieved to ensure that The overall performance of the material.

CN118880602AActive Publication Date: 2024-11-01NANTONG UNIV

Patent Information

Application Number
CN202410948379.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

The electrical conductivity of existing flexible materials is unstable, poor hydrophobicity, poor waterproofness and overall performance. The poor wetting of liquid metal on the substrate leads to easy shedding. The use of water-based polyurethane to improve the binding performance will affect the hand feel and part of the fiber performance. Liquid metal The surface tension causes uneven coating and reduced conductivity, and the preparation of spinning liquid requires the use of organic solvents, which affects the mechanical properties.

Method used

Pretreatment and activation of flexible fabrics with normal pressure plasma, brush the liquid metal and induced cross-linking in the plasma discharge cavity to form a coating, use polydimethylsiloxane to form a coating, and pass plasma or chemical cross-linking. The agent forms a cross-linked film to ensure uniform dispersion and adhesion of liquid metals, and improves electrical conductivity and hydrophobicity.

Benefits of technology

The uniform dispersion and stable adhesion of liquid metal on the surface of the material is achieved, the conductive properties and hydrophobicity are improved, the conductive stability of the material is protected, and the overall performance of the fiber is ensured, especially the conductive properties under deformation conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880602A_ABST
    Figure CN118880602A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a flexible conductive hydrophobic material. The preparation method comprises the following steps: step 1, performing normal-pressure plasma pretreatment activation on a flexible fabric; step 2, brushing liquid metal on the surface of the activated flexible fabric; step 3, blade-coating polydimethylsiloxane on the flexible surface brushed with the liquid metal, and performing crosslinking film formation to obtain a flexible conductive hydrophobic material; according to the method, the surface of the fiber / yarn / fabric is subjected to normal-pressure plasma pretreatment by using a normal-pressure plasma method, so that liquid metal can be uniformly distributed on the surface of the fiber / yarn / fabric, an organic silicon polymer is attached to the surface of the fiber / yarn / fabric, and the coating is formed by inducing crosslinking under the action of plasma or a chemical crosslinking agent; the liquid metal on the surface of the fiber / yarn can be effectively prevented from being agglomerated, the yarn / fiber can be endowed with a certain waterproof function, the conductive stability of the material is further protected, and meanwhile the overall performance of the fiber / yarn cannot be affected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of flexible conductive hydrophobic materials, and in particular to a flexible conductive hydrophobic material and a preparation method thereof. Background Art

[0002] People have been studying hydrophobic materials for a long time. Super-hydrophobic materials refer to materials whose surface water contact angle is greater than 90° and water cannot penetrate. At present, one of the research hotspots on hydrophobic materials is multifunctional hydrophobic materials, and flexible conductive hydrophobic materials are one of them. Flexible conductive hydrophobic materials have excellent hydrophobicity and conductivity, and can be used in waterproof sensors, anti-ice melting, electromagnetic shielding materials and other fields that have special requirements on the deformation properties of materials. The presence of hydrophobic properties can further improve the service life and expand the application scenarios.

[0003] In the article "Preparation and Properties of Liquid Metal / Polyurethane Composite Elastic Conductive Fibers", highly elastic thermoplastic polyurethane (TPU) fibers were prepared by wet spinning; then water-based polyurethane (WPU) was dip-coated as a bonding layer to improve the wettability between TPU and liquid metal (LM), and LM was coated in a pre-stretched state to improve the resistance stability of the fiber; finally, the LM layer was encapsulated in the WPU coating by dip coating to obtain a composite elastic conductive fiber; at the same time, in the article "Preparation and Properties of Polyurethane-Based Carbon Nanotube-Liquid Metal Conductive Fibers", in order to improve the problem of insufficient elastic properties of carbon nanotubes (CNTs) as conductive fillers, CNTs and liquid metal (LM) were used as conductive fillers, thermoplastic polyurethane (TPU) was used as the matrix, N, N-dimethylformamide (DMF) was selected as the solvent, and deionized water was used as the coagulation bath. (CNT)LM / TPU conductive fibers were prepared by wet spinning, and LM and The influence of two kinds of conductive fillers, CNT, on the fiber structure and performance; however, the wettability of liquid metal to the flexible substrate is very poor, so it is easy to fall off the substrate. The existing technology uses water-based polyurethane (TPU) to improve the bonding performance between liquid metal and the flexible substrate, but the use of TPU will affect the feel and some performance of the fiber material; at the same time, liquid metal has a large surface tension (>450N / m), and it is easy to agglomerate under the action of internal stress during use, resulting in uneven coating and decreased conductivity. The existing technology mainly solves the problem by coating with water-based polyurethane or mixing with spinning solution. The preparation of spinning solution requires the use of organic solvents. In order to obtain better conductivity, more liquid metal needs to be added, which will reduce the mechanical properties of the fiber to a certain extent; in order to reduce the amount of liquid metal used, it needs to be mixed with carbon nanotubes, which will make the preparation of uniform spinning solution more difficult and increase the difficulty of spinning. In the prior art, the fibers produced by the mixed spinning method cannot be used directly for weaving and need to be twisted to form yarns. The fibers will be worn during the processing. The uneven and rough fiber surface or poor uniformity along the length direction will affect the yarn performance. Summary of the invention

[0004] The present invention designs and develops a flexible conductive hydrophobic material, the purpose of the present invention is to solve the problems of unstable conductive performance, poor hydrophobicity, poor waterproofness and poor overall performance of existing flexible materials.

[0005] The present invention designs and develops a method for preparing a flexible conductive hydrophobic material. The purpose of the present invention is to solve the problem that liquid metal is evenly dispersed during the preparation process and is easy to agglomerate during use. At the same time, the plasma action only processes the surface of the fiber / yarn by a dozen nanometers, which will not affect the overall performance of the fiber / yarn while ensuring waterproofness.

[0006] The technical solution provided by the present invention is:

[0007] A method for preparing a flexible conductive hydrophobic material comprises the following steps:

[0008] Step 1: pre-treating and activating the flexible fabric by atmospheric pressure plasma;

[0009] Step 2: Brushing liquid metal on the surface of the activated flexible fabric;

[0010] Step 3: After coating polydimethylsiloxane on the flexible surface coated with liquid metal, cross-linking is performed to form a film to obtain the flexible conductive hydrophobic material.

[0011] Preferably, in step one, the plasma pretreatment process includes: the working gas is one or more of oxygen, hydrogen, carbon dioxide, and nitrogen, the processing power is 100 to 500 W, the processing time is 3 to 100 s, and the processing spacing is 1 to 3.5 mm.

[0012] Preferably, in the step 2, the brush coating thickness is controlled to be 0.1 to 4 mm.

[0013] Preferably, in step three, the cross-linking film forming process includes a plasma-induced cross-linking film forming process: polydimethylsiloxane with a viscosity of 1000 to 10000 cps is selected as a raw material, and after being scraped on the flexible surface of the brushed liquid metal, it is placed in a plasma discharge chamber to induce cross-linking film formation.

[0014] Preferably, the processing parameters for inducing the cross-linking film forming process in the plasma discharge chamber are: the plasma discharge device is a capacitive coupling and inductive coupling discharge, which can be divided into one of direct current, pulse, low frequency, and radio frequency plasma discharge according to the discharge frequency;

[0015] The reaction gas is argon, helium, oxygen, air or a mixture of the above; and

[0016] The power is 50-500W, the modulation pulse is 2%-100%, the processing time is 20-300s, and the processing interval is 1-12cm.

[0017] Preferably, in step three, the cross-linking film-forming process includes a chemical cross-linking agent cross-linking film-forming process: hydroxyl-terminated polydimethylsiloxane with a viscosity of 1000 to 4000 cps is selected as a raw material, tetraethyl orthosilicate is used as a cross-linking agent, and di-n-octyltin dilaurate is used as a catalyst. After being scraped and coated on the flexible surface of the brushed liquid metal, it is placed in an oven and heated to cross-link and form a film.

[0018] Preferably, in step three, the cross-linking film-forming process includes a chemical cross-linking agent cross-linking film-forming process: Dow Corning 184 is selected as the raw material, polydimethylsiloxane and the cross-linking agent are fully stirred and mixed, and then the mixture is scraped and applied to the flexible surface of the liquid metal, and then the mixture is placed in an oven to heat and cross-link to form a film.

[0019] Preferably, the cross-linking temperature is 60 to 150° C., and the cross-linking time is 30 to 600 min.

[0020] Preferably, the scraping thickness is between 0.5 and 5 mm.

[0021] A flexible conductive hydrophobic material is prepared using the flexible conductive hydrophobic material preparation method.

[0022] The beneficial effects of the present invention are:

[0023] 1. The preparation method of the flexible conductive hydrophobic material provided by the present invention uses atmospheric pressure plasma to activate and roughen the surface of the material, which is simple to operate and has good effect. After plasma surface activation, the liquid metal can be evenly dispersed on the surface of the material. At the same time, by using polydimethylsiloxane to coat the surface of the material, the problem of unstable conductive performance caused by the large internal stress and easy accumulation of liquid metal can be effectively solved;

[0024] 2. The roughness of the surface of the flexible conductive hydrophobic material after plasma treatment provided by the present invention is increased, which can appropriately increase the amount of liquid metal attached to the surface of the material, further increasing the conductive performance. Silicone polymer is attached to its surface, and induced to cross-link under the action of plasma or chemical cross-linking agent to form a coating, which can also give the yarn / fiber a certain hydrophobic function, further protecting the conductive stability of the material;

[0025] 3. The flexible conductive hydrophobic material provided by the present invention uses liquid metal to be evenly distributed on the surface of the material to make a flexible and conductive electrothermal material. The method of using plasma pretreatment and silicone polymer coating can ensure the conductive properties of the liquid metal while not affecting the extension of the liquid metal on the surface of the material, thereby ensuring the conductive properties of the flexible conductive material under deformation conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a schematic diagram of the surface temperature of the conductive fabric after power is applied in Example 1 of the present invention.

[0027] Figure 2 This is a graph showing how the surface temperature of the conductive fabric changes with time under different voltages at both ends in Example 1 of the present invention.

[0028] Figure 3 This is a temperature distribution diagram of the fabric surface when the voltage across both ends of Example 5 described in the present invention is 1.5V.

[0029] Figure 4 This is a graph showing the average temperature variation of the fabric surface under different voltages in Example 5 of the present invention.

[0030] Figure 5 This is a static water contact angle diagram of the surface of the flexible conductive fabric prepared in Example 8 of the present invention. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0032] The present invention provides a method for preparing a flexible conductive hydrophobic material, which specifically comprises the following steps:

[0033] Step 1: To solve the surface wetting problem of liquid metal, the fiber / yarn / fabric surface is pretreated by atmospheric pressure plasma using atmospheric pressure plasma method;

[0034] Among them, according to different materials, the working gas is one or more of oxygen, hydrogen, carbon dioxide, and nitrogen, the processing power is 100-500W, the processing time is 3-100s, the processing interval is 1-3.5mm, and active groups are introduced on its surface for surface activation. The etching effect can increase the surface roughness, based on which the liquid metal can be evenly distributed on the fiber / fabric surface;

[0035] Step 2: Select indium gallium alloy liquid metal as the raw material, and directly apply it on the surface of fiber / yarn / fabric cut into a certain shape by brushing, or use screen printing technology on the surface of the fabric to apply it on the surface of the fabric in a certain shape to form circuits with different structures;

[0036] The coating structure includes but is not limited to circular, U-shaped, string-shaped, mosquito coil-shaped, etc. To ensure conductivity, as a preferred embodiment, the coating thickness is controlled between 0.1 and 4 mm;

[0037] Step 3: cross-linking polysiloxane to form a film. In the present invention, plasma-induced cross-linking or chemical cross-linking agent cross-linking is used to form a film, which specifically includes the following process:

[0038] (1) The process of plasma-induced cross-linking film formation includes: selecting polydimethylsiloxane with a viscosity of 1000 to 10000 cps as a raw material, scraping it on the surface of a fiber / yarn / fabric cut into a certain shape with liquid metal adhered on the surface, and controlling the scraping thickness between 0.5 and 5 mm, and then placing it in a plasma discharge chamber, discharging under certain conditions, and inducing cross-linking film formation; wherein the processing parameters are: the plasma discharge device is a capacitive coupling and inductive coupling discharge, which can be divided into one of direct current, pulse, low frequency, and radio frequency plasma discharge according to the discharge frequency; the reaction gas is the first one or a mixture of several selected from argon, helium, oxygen, air, etc.; the power is 50 to 500 W; the modulation pulse is 2% to 100%; the processing time is 20 to 300 s; the processing interval is 1 to 12 cm;

[0039] (2) The process of cross-linking film formation using a chemical cross-linking agent includes:

[0040] ① Select hydroxyl-terminated polydimethylsiloxane with a viscosity of 1000-4000cps as raw material, ethyl orthosilicate as crosslinking agent, dioctyltin dilaurate as catalyst according to a certain mass ratio (M 聚二甲基硅氧烷 :M 正硅酸乙酯 :M 二月桂酸二正辛基锡 =100:5:1~100:10:2) after being fully stirred and mixed, the mixture is scraped and applied to the surface of the fiber / yarn / fabric cut into a certain shape with liquid metal adhered on the surface, and the scraping thickness is controlled between 0.5~5mm;

[0041] ② Select Dow Corning 184 as the raw material, and mix polydimethylsiloxane and crosslinking agent according to a certain mass ratio (M 聚二甲基硅氧烷 :M 交联剂 =10:1~10:5) after being fully stirred and mixed, the mixture is scraped and applied to the surface of the fiber / yarn / fabric cut into a certain shape with liquid metal adhered on the surface, and the scraping thickness is controlled between 0.5~5mm;

[0042] After the above-mentioned coating is applied to the surface of the fiber / yarn / fabric cut into a certain shape with liquid metal adhering to the surface, it is placed in an oven for heating and cross-linking to form a film, the cross-linking temperature is 60-150° C., and the cross-linking time is 30-600 min.

[0043] The present invention also provides a flexible conductive hydrophobic material, which is prepared by the method for preparing the flexible conductive hydrophobic material.

[0044] The present invention will be further described below in conjunction with specific embodiments.

[0045] Example 1

[0046] Polyester woven plain fabric was used as flexible fabric, with a cutting size of about 1cm×5cm, and surface activation was performed using atmospheric pressure plasma. The treatment process was as follows: the working gas was air, the treatment power was 300W, the treatment time was 50s, and the treatment spacing was 2.8mm. The liquid metal was evenly brushed on the surface of the surface-activated fabric at room temperature, and the brushing thickness was 4mm. Polydimethylsiloxane with a viscosity of 10000cps was selected as the raw material, and was scraped on the surface of the fabric adhered with liquid metal, and the scraping thickness was 5mm. It was then placed in a plasma discharge chamber. The treatment parameters were as follows: a low-voltage capacitively coupled discharge plasma device, the discharge form was radio frequency discharge, the reaction gas was argon, the power was 50W, the modulation frequency was 100%, the treatment time was 300s, and the treatment spacing was 1cm. The surface polydimethylsiloxane was induced to cross-link and form a film under the action of plasma, and a flexible conductive hydrophobic polyester fabric was made.

[0047] Example 2

[0048] Polyester woven plain fabric was used as flexible fabric, with a cutting size of about 1cm×10cm, and surface activation was performed using atmospheric pressure plasma. The treatment process was as follows: the working gas was air, the treatment power was 300W, the treatment time was 50s, and the treatment spacing was 2.8mm. The liquid metal was evenly brushed on the surface of the surface-activated fabric at room temperature, and the brushing thickness was 2mm. Polydimethylsiloxane with a viscosity of 5000cps was selected as the raw material, and was scraped on the surface of the fabric adhered with liquid metal, and the scraping thickness was 2mm. It was then placed in a plasma discharge chamber. The treatment parameters were as follows: a low-voltage capacitively coupled discharge plasma device, the discharge form was radio frequency discharge, the reaction gas was argon, the power was 200W, the modulation frequency was 75%, the treatment time was 200s, and the treatment spacing was 8cm. The surface polydimethylsiloxane was induced to cross-link and form a film under the action of plasma, and a flexible conductive hydrophobic polyester fabric was made.

[0049] Example 3

[0050] Polyester woven plain fabric was used as flexible fabric, with a cutting size of about 1cm×10cm, and surface activation was performed using atmospheric pressure plasma. The treatment process was as follows: the working gas was air, the treatment power was 300W, the treatment time was 50s, and the treatment spacing was 2.8mm. The liquid metal was evenly brushed on the surface of the surface-activated fabric at room temperature, and the brushing thickness was 0.1mm. Polydimethylsiloxane with a viscosity of 1000cps was selected as the raw material, and was scraped on the surface of the fabric adhered with liquid metal, and the scraping thickness was 0.5mm. It was then placed in a plasma discharge chamber. The treatment parameters were as follows: a low-voltage inductively coupled discharge plasma device, a pulse discharge, a reaction gas of helium, a power of 500W, a modulation frequency of 2%, a treatment time of 20s, and a treatment spacing of 12cm. The surface polydimethylsiloxane was induced to crosslink and form a film under the action of plasma, and a flexible conductive hydrophobic polyester fabric was made.

[0051] Example 4

[0052] High-density nylon woven plain fabric is used as flexible fabric, the cutting size is about 10cm×10cm, and atmospheric pressure plasma is used for surface activation. The treatment process is: the working gas is a mixture of hydrogen, carbon dioxide and nitrogen, the treatment power is 500W, the treatment time is 3s, and the treatment spacing is 1mm. Under room temperature conditions, an "S-type" mask is selected, and liquid metal is printed on the surface of the surface-activated fabric using screen printing technology. The thickness of the liquid metal is 4mm. Polydimethylsiloxane with a viscosity of 4000cps is selected as the raw material, and it is mixed with ethyl orthosilicate and dioctyltin dilaurate at a mass ratio of 50:5:1 and stirred evenly. The fabric surface adhered with liquid metal is evenly coated by scraping method, and the scraping thickness is about 5mm. It is cured at a temperature of 80℃ for 480min to form a flexible conductive hydrophobic nylon fabric.

[0053] Example 5

[0054] Polyester weft plain knitted fabric is used as flexible fabric, the cutting size is about 1cm×10cm, and the surface is activated under normal pressure plasma. The treatment process is: the working gas is a mixture of hydrogen, carbon dioxide and nitrogen, the treatment power is 100W, the treatment time is 100s, and the treatment spacing is 3.5mm. The liquid metal is evenly brushed on the surface of the surface activated fabric at room temperature, and the brushing thickness is 0.1mm. Polydimethylsiloxane with a viscosity of 1000cps is selected as the raw material, and it is mixed with ethyl orthosilicate and dioctyltin dilaurate in a mass ratio of 100:5:1 and stirred evenly. The scraping method is used to evenly coat the surface of the fabric adhered with liquid metal, and the scraping thickness is about 0.5mm. It is cured at a temperature of 120℃ for 30min to prepare a flexible conductive hydrophobic polyester fabric.

[0055] Example 6

[0056] High-density nylon woven plain fabric is used as flexible fabric, the cutting size is about 10cm×10cm, and atmospheric pressure plasma is used for surface activation. The treatment process is: the working gas is air, the treatment power is 500W, the treatment time is 3s, and the treatment spacing is 1mm. Under room temperature conditions, an "S-type" mask is selected, and the liquid metal is printed on the surface of the surface-activated fabric using screen printing technology. The thickness of the liquid metal is 4mm. Hydroxyl-terminated polydimethylsiloxane with a viscosity of 4000cps is selected as the raw material, and it is mixed with ethyl orthosilicate and di-n-octyltin dilaurate in a mass ratio of 50:5:1 and stirred evenly. The fabric surface adhered with liquid metal is evenly coated by scraping method, and the scraping thickness is about 5mm. It is cured at a temperature of 60°C for 600min to form a flexible conductive hydrophobic nylon fabric.

[0057] Example 7

[0058] High-density nylon woven plain fabric is used as flexible fabric, the cutting size is about 10cm×10cm, and atmospheric pressure plasma is used for surface activation. The treatment process is: the working gas is nitrogen-oxygen mixed gas, the treatment power is 400W, the treatment time is 20s, and the treatment spacing is 2.5mm. Under room temperature conditions, an "S-type" mask is selected, and the liquid metal is printed on the surface of the surface-activated fabric using screen printing technology. The thickness of the liquid metal is 2mm. Hydroxyl-terminated polydimethylsiloxane with a viscosity of 3000cps is selected as the raw material, and it is mixed with ethyl orthosilicate and di-n-octyltin dilaurate in a mass ratio of 75:5:1 and stirred evenly. The fabric surface adhered with liquid metal is evenly coated by scraping method, and the scraping thickness is about 3mm. It is cured at a temperature of 100℃ for 240min to form a flexible conductive hydrophobic nylon fabric.

[0059] Example 8

[0060] High-density nylon woven plain fabric is used as flexible fabric, the cutting size is about 1cm×10cm, and atmospheric pressure plasma is used for surface activation. The treatment process is: the working gas is air, the treatment power is 400W, the treatment time is 20s, and the treatment spacing is 2.5mm. Under room temperature conditions, the thickness of the liquid metal is 1.5mm, Dow Corning 184 is selected as the raw material, and it is mixed with the cross-linking agent at a mass ratio of 10:1 and stirred evenly. The scraping method is used to evenly coat the surface of the fabric adhered with liquid metal. The scraping thickness is about 3mm, and it is cured at a temperature of 120℃ for 60min to make a flexible conductive hydrophobic nylon fabric.

[0061] Example 9

[0062] High-density aramid woven plain fabric was used as the flexible fabric, the cutting size was about 10cm×10cm, and the surface was activated by atmospheric pressure plasma. The treatment process was: the working gas was air, the treatment power was 300W, the treatment time was 10s, and the treatment spacing was 2.3mm. Under room temperature, a "mosquito-repellent type" mask was selected, and the liquid metal was brushed on the surface of the surface-activated fabric using a brushing technique. The thickness of the liquid metal was 2mm. Dow Corning 184 was selected as the raw material, and it was mixed with the cross-linking agent at a mass ratio of 10:5 and stirred evenly. The scraping method was used to evenly coat the surface of the fabric adhered with liquid metal. The scraping thickness was about 2mm, and it was cured at a temperature of 150℃ for 30min to form a flexible conductive hydrophobic aramid fabric.

[0063] Test Case

[0064] Surface hydrophobicity test: The hydrophobicity of the material surface is judged by the size of the static water contact angle. The larger the contact angle, the better the hydrophobicity. Test method: Use OCA15EC contact angle meter, select deionized water as the test liquid, the drop volume is 5μL, the injection rate is 2μL / s, and each group of samples is tested 5 times and the average value is taken.

[0065] The conductivity test includes the resistance method and the electrothermal test. For the resistance test, use a multimeter to place the positive and negative electrodes of the test pen at both ends of the flexible conductive fabric, observe the multimeter reading, test each group of samples 5 to 8 times, and take the average value. For the electrothermal test, use a dolphin clip to clamp both ends of the fabric, use a DC power supply to adjust the voltage at both ends, and power on. Use a thermal infrared imager to test the change in surface temperature of the fabric after power on. Perform a voltage boost and temperature test every 10 seconds.

[0066] In Example 1, the static water contact angle of the fabric surface before and after treatment increased from ≤10° to 143°; in Example 5, the static water contact angle of the fabric surface before and after treatment increased from ≤10° to 132°; in Example 8, the static water contact angle of the fabric surface before and after treatment increased from ≤10° to 121°; the resistance at both ends of the fabric was about 1.9Ω.

[0067] like Figure 1 , Figure 2 As shown, in Example 1, the resistance at both ends of the fabric is about 0.5Ω; after different voltages are applied to both ends, the surface temperature increases with the increase of voltage, and at 0.8V, the temperature reaches 115.3℃, stays for 1min, and the temperature remains basically unchanged. After turning off the power, the temperature gradually decreases.

[0068] like Figure 3 , Figure 4As shown, in Example 5, the resistance at both ends of the fabric is about 0.2Ω; after different voltages are applied to both ends, the surface temperature increases with the increase of voltage, and at 0.5V, the temperature reaches 115.3℃, stays for 1min, and the temperature remains basically unchanged. After turning off the power, the temperature gradually decreases.

[0069] like Figure 5 As shown, in Example 8, the static water contact angle of the fabric surface before and after treatment increased from ≤10° to 121°; the electrical resistance at both ends of the fabric was about 1.9Ω.

[0070] It can be seen from the results of the above embodiments that the flexible conductive hydrophobic material and the flexible conductive fabric made by the preparation method provided by the invention have relatively stable conductive properties and good hydrophobicity after treatment, and the surface hydrophobicity of the flexible conductive fabric formed by plasma-induced cross-linking is slightly better than that formed by chemical cross-linking agent-induced cross-linking. It shows that the surface pretreatment of the material by atmospheric pressure plasma method can well solve the problem of uniform dispersion and poor conductive stability of liquid metal on the surface of the material. It is simple to operate, has good effect, and does not affect the overall performance of the material. The use of polydimethylsiloxane to coat the surface of the material can not only effectively solve the problem of unstable conductive performance caused by the large internal stress and easy accumulation of liquid metal, but also give the flexible conductive material a certain hydrophobic and waterproof function, further protecting the conductive stability of the material.

[0071] In the present invention, in order to solve the problem of uniform dispersion of liquid metal, a normal-pressure plasma method is used to perform normal-pressure plasma pretreatment on the surface of fiber / yarn / fabric, and active groups are introduced on its surface to perform surface activation. The etching effect can increase the surface roughness, based on which the liquid metal can be evenly distributed on the surface of the fiber / yarn / fabric; in order to solve the problem that liquid metal is easy to agglomerate during use, an organic silicon polymer is attached to its surface, and induced cross-linking to form a coating under the action of plasma or a chemical cross-linking agent, which can not only effectively prevent the agglomeration of liquid metal on the surface of the fiber / yarn but also give the yarn / fiber a certain waterproof function, further protecting the conductive stability of the material; the plasma pretreatment-attachment of silicon-containing polymer-induced cross-linking film-forming method can directly treat the surface of the fiber / yarn, and the plasma action only treats the surface of the fiber / yarn of more than a dozen nanometers, which will not affect the overall performance of the fiber / yarn.

[0072] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for preparing a flexible conductive hydrophobic material, characterized in that: The steps include: Step 1: pre-treating and activating the flexible fabric by atmospheric pressure plasma; Step 2: Brushing liquid metal on the surface of the activated flexible fabric; Step 3: After coating polydimethylsiloxane on the flexible surface coated with liquid metal, cross-linking is performed to form a film to obtain the flexible conductive hydrophobic material.

2. The method for preparing a flexible conductive hydrophobic material according to claim 1, characterized in that: In the step 1, the plasma pretreatment process includes: the working gas is one or more of oxygen, hydrogen, carbon dioxide, and nitrogen, the processing power is 100 to 500 W, the processing time is 3 to 100 s, and the processing spacing is 1 to 3.5 mm.

3. The method for preparing the flexible conductive hydrophobic material according to claim 1 or 2, characterized in that: In the step 2, the brush coating thickness is controlled to be 0.1 to 4 mm.

4. The method for preparing a flexible conductive hydrophobic material according to claim 1, characterized in that: In step three, the cross-linking film-forming process includes a plasma-induced cross-linking film-forming process: polydimethylsiloxane with a viscosity of 1000 to 10000 cps is selected as a raw material, and after being scraped on the flexible surface of the brushed liquid metal, it is placed in a plasma discharge chamber to induce cross-linking film formation.

5. The method for preparing a flexible conductive hydrophobic material according to claim 4, characterized in that: Processing parameters for inducing cross-linking film formation in a plasma discharge chamber: The plasma discharge device is a capacitively coupled or inductively coupled discharge, which can be divided into one of direct current, pulse, low frequency, and radio frequency plasma discharge according to the discharge frequency; The reaction gas is argon, helium, oxygen, air or a mixture of the above; and The power is 50-500W, the modulation pulse is 2%-100%, the processing time is 20-300s, and the processing interval is 1-12cm.

6. The method for preparing the flexible conductive hydrophobic material according to claim 1, characterized in that: In the step three, the cross-linking film-forming process includes a chemical cross-linking agent cross-linking film-forming process: selecting hydroxyl-terminated polydimethylsiloxane with a viscosity of 1000 to 4000 cps as a raw material, ethyl orthosilicate as a cross-linking agent, and di-n-octyltin dilaurate as a catalyst, after scraping and coating the flexible surface of the brushed liquid metal, placing it in an oven to heat and cross-link to form a film.

7. The method for preparing a flexible conductive hydrophobic material according to claim 1, characterized in that: In the step three, the cross-linking film-forming process includes a chemical cross-linking agent cross-linking film-forming process: Dow Corning 184 is selected as the raw material, polydimethylsiloxane and the cross-linking agent are fully stirred and mixed, and then scraped on the flexible surface of the brushed liquid metal, and then placed in an oven to heat and cross-link to form a film.

8. The method for preparing the flexible conductive hydrophobic material according to claim 6 or 7, characterized in that: The cross-linking temperature is 60-150°C, and the cross-linking time is 30-600min.

9. The method for preparing the flexible conductive hydrophobic material according to claim 4, 6 or 7, characterized in that: The scraping thickness is between 0.5 and 5 mm.

10. A flexible conductive hydrophobic material, characterized in that: The flexible conductive hydrophobic material is prepared using the preparation method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Conductive fabric and preparation method thereof

    CN107938369A

  • Preparation method of fabric loaded with high-entropy alloy nanoparticles on surface

    CN117188166A

  • Flexible conductive interconnection film based on liquid metal, conductive interface and flexible conductive connection method

    CN117219323A

  • Liquid metal flexible electrode and preparation method and application thereof

    CN117838134A

  • Conductive fiber based on liquid metal, preparation method of conductive fiber and wearable fabric

    CN118308873A

Cited By

  • Breathable metal composite textile and preparation method thereof

    CN122518843A