Method for preparing wood fiber paper-based material through foam molding

By adding non-ionic surfactant and paper reinforcement to the paper-based material for foam molding, covalent bonds and hydrogen bonds between fibers are formed, the problem of insufficient mechanical properties of paper-based materials is solved and the tensile strength is significantly improved and tear strength, and meet environmental protection requirements.

CN118880642APending Publication Date: 2024-11-01TIANJIN UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411023185.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The mechanical properties of existing paper-based materials prepared by foam molding need to be improved, and it is difficult to significantly improve their strength and tear resistance without affecting the uniformity and looseness of the paper.

Method used

In the method of preparing lignocellulosic paper-based materials for foam molding, nonionic surfactants and paper reinforcers, such as nanocellulose, sodium carboxymethylcellulose, and polyacrylamide, are added, and the reinforcement is made by blending ultrasound and mechanical stirring. The agent forms covalent bonds and hydrogen bonds with the fibers, forming a three-dimensional network structure to enhance the binding force between the fibers.

Benefits of technology

It effectively improves the tensile strength, uniformity and tear strength of paper-based materials, while maintaining the uniformity and looseness of the paper. The reinforcement and surfactants used are environmentally friendly and pollution-free, and meet modern environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880642A_ABST
    Figure CN118880642A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a wood fiber paper-based material through foam molding, and relates to the technical field of paper preparation. The method comprises the following steps: pulping a pulp board to obtain pulp, and then defibering; blending a paper reinforcing agent and a surfactant, and then adding into the defibered pulp for stirring and foaming; and carrying out papermaking on the treated foaming slurry to obtain the wood fiber paper-based material. The foam molding technology is applied to preparation of the paper-based material, the mechanical property of the paper-based material is improved by adding the paper reinforcing agent, the method is a case capable of achieving efficient production, saving energy consumption and saving industrial water, and the requirements of social development are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of paper preparation, and in particular relates to a method for preparing a wood fiber paper-based material by foam forming. Background Art

[0002] Foam forming technology is a papermaking technology that uses the principle of using surfactants in aqueous solution to produce a certain volume of foam through mechanical stirring, and uses foam instead of water as a carrier for plant fibers. This dispersion method not only improves the uniformity and quality of paper, but also significantly reduces the amount of water used and reduces energy consumption, thereby achieving the greening of the papermaking process. Foam forming technology was first proposed by Radvan in the 1970s. In recent years, with the increasing demand for sustainable materials and energy-saving technologies, the application of foam technology in the papermaking industry has once again attracted widespread attention from researchers and the industry. Foam technology not only has broad application prospects in the field of papermaking, but also shows its unique value in many fields such as building thermal regulation, non-woven material production, and wastewater treatment. For example, in the field of construction, foam technology can be used to manufacture high-performance insulation boards, which not only have good thermal insulation properties, but also have self-reinforcement characteristics, and can achieve high strength and light weight without the use of chemical adhesives. In the non-woven industry, foam laying technology can improve the dispersion of fibers, improve the uniformity and bulk of products, and reduce production costs. However, the mechanical properties of paper-based materials prepared using foam molding technology need to be improved. In order to solve this problem, we added paper enhancers and utilized their interaction with surfactants to better combine with the existing ones, so as to improve the mechanical properties of paper-based materials without affecting the uniformity and bulk of the paper. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing wood fiber paper-based materials by foam molding, which is simple to operate and economically feasible.

[0004] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0005] S1, beating the wood pulp board to obtain pulp, and then performing a decomposition treatment on the pulp;

[0006] S2, adding a paper strengthening agent and a surfactant to the slurry of S1 and stirring;

[0007] S3, papermaking the pulp treated in step S2 to obtain a wood fiber paper-based material.

[0008] Furthermore, in step S1, the wood pulp is one or more of bleached coniferous pulp, unbleached coniferous pulp, bleached broadleaf pulp, unbleached broadleaf pulp, bamboo pulp, straw pulp, and hemp pulp, the average length of the pulp is 1mm-3mm, and the beating degree is 15°SR-60°SR.

[0009] Furthermore, in step S2, the surfactant is a nonionic surfactant, and one or more of polyoxyethylene sorbitan fatty acid ester, fatty alcohol polyoxyethylene ether, Triton X-100, and alkylphenol polyoxyethylene ether are used.

[0010] Furthermore, in step S2, the paper strengthening agent is one or more of nanocellulose, sodium carboxymethyl cellulose, and polyacrylamide.

[0011] Furthermore, the dosage of the enhancer in step S2 is 0.1%-5%.

[0012] Furthermore, the amount of surfactant used in step S2 is 0.1%-5%.

[0013] Furthermore, in step S2, the paper strengthening agent and the surfactant are blended by ultrasonication for 10 minutes and stirred for 10-60 minutes.

[0014] Furthermore, in step S2, the slurry concentration is 0.1%-2%, the stirring speed of the stirrer is 400-2000r / min, and the stirring is performed for 5-15min.

[0015] A wood fiber paper-based material prepared by the above-mentioned preparation method.

[0016] The reinforcing agent and surfactant used in the present invention are both environmentally friendly and pollution-free reagents, and are environmentally friendly. They are also widely available and economically advantageous. The fiber paper-based material synthesized therefrom is biodegradable and meets the trend of modern environmental protection requirements.

[0017] The present invention utilizes the foaming principle of nonionic surfactants, and introduces air into the fiber-water system through mechanical stirring, so that the evenly distributed foam supports the dispersed fibers in the foam channel, which is also called the Plateau boundary. Nonionic surfactants exist in the aqueous solution in the form of neutral nonionic molecules or micelles, and will not dissociate into charged anions or cations, so they will not produce adsorption through electrostatic force. The only adsorption effect on the fiber is the van der Waals force, so the effect on the interaction between the fibers is very small. The surfactant is adsorbed on the fiber to improve the hydrophobicity of the fiber.

[0018] The present invention adds a paper reinforcing agent, utilizes the active groups in the reinforcing agent to generate chemical bonds such as covalent bonds and hydrogen bonds with fibers, and strengthens the bonding between fibers, thereby enhancing the mechanical properties of the paper-based material. The polymer reinforcing agent is used, and the reinforcing agent forms a three-dimensional network structure through a cross-linking reaction. This structure acts as an adhesive in the fiber-water-air system, and can better enhance the interaction between fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is the distribution diagram of foaming diameter of cationic polyacrylamide slurry;

[0020] Figure 2 is the distribution diagram of foaming diameter of nanocellulose pulp;

[0021] Figure 3 This is the distribution diagram of foaming diameter of slurry containing sodium carboxymethyl cellulose;

[0022] Figure 4 is the distribution diagram of the foaming diameter of the original slurry;

[0023] Figure 5 This is a schematic diagram of the process of Example 1. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with specific embodiments, but is not limited thereto.

[0025] Example 1

[0026] (1) Prepare enhancer solution: add 0.2 g of cationic polyacrylamide to 500 g of deionized water, heat in a 50° C. water bath, and add a rotor for magnetic stirring for 20 min.

[0027] (2) Preparation of raw materials containing enhancer and surfactant: Take 9 g of enhancer solution, add 0.3 g of fatty alcohol polyoxyethylene ether, stir evenly with a glass rod, put into a rotor for magnetic stirring, and stir for 20 min.

[0028] (3) Preparation of fiber-containing foam slurry: 1.8 g of absolute dry fiber was added to 400 g of water for decomposition at a decomposition speed of 3000 rpm for 15 min. Then, the prepared raw materials containing reinforcing agent and surfactant were added and stirred at a speed of 500 rpm for 10 min, and then at a speed of 1500 rpm for 10 min for foaming.

[0029] (4) Papermaking: Pour the prepared fiber-containing foam slurry into a forming funnel and filter to obtain a wet paper web. Press the wet paper web with a force of 5N and then place it in a flat dryer at a drying temperature of 95°C for 20 minutes to obtain a paper web with a basis weight of 100 g / m 2 Paper-based material.

[0030] It can be seen from Tables 1-4 that compared with the control example, the addition of cationic polyacrylamide can effectively improve the tensile strength, uniformity and tear strength of the paper-based material, but the bulk of the paper-based material is significantly reduced.

[0031] Example 2

[0032] (1) Prepare the enhancer solution: add 0.2 g of nanocellulose to 500 g of deionized water and add a rotor for magnetic stirring for 20 min.

[0033] (2) Preparation of raw materials containing enhancer and surfactant: Take 9 g of enhancer solution, add 0.3 g of fatty alcohol polyoxyethylene ether, stir evenly with a glass rod, put into a rotor for magnetic stirring, and stir for 20 min.

[0034] (3) Preparation of fiber-containing foam slurry: 1.8 g of absolute dry fiber was added to 400 g of water for decomposition at a decomposition speed of 3000 rpm for 15 min. Then, the prepared raw materials containing reinforcing agent and surfactant were added and stirred at a speed of 500 rpm for 10 min, and then at a speed of 1500 rpm for 10 min for foaming.

[0035] (4) Papermaking: Pour the prepared fiber-containing foam slurry into a forming funnel and filter to obtain a wet paper web. Press the wet paper web with a force of 5N and then place it in a flat dryer at a drying temperature of 95°C for 20 minutes to obtain a paper web with a basis weight of 100 g / m 2 Paper-based material.

[0036] It can be seen from Tables 1-4 that compared with the control example, the addition of nanocellulose can effectively improve the tensile strength, uniformity and tear strength of the paper-based material, but the bulk of the paper-based material is slightly reduced.

[0037] Example 3

[0038] (1) Prepare enhancer solution: add 0.2 g sodium carboxymethyl cellulose to 500 g deionized water, heat in a 50° C. water bath, and add a rotor for magnetic stirring for 20 min.

[0039] (2) Preparation of raw materials containing enhancer and surfactant: Take 9 g of enhancer solution, add 0.3 g of fatty alcohol polyoxyethylene ether, stir evenly with a glass rod, put into a rotor for magnetic stirring, and stir for 20 min.

[0040] (3) Preparation of fiber-containing foam slurry: 1.8 g of absolute dry fiber was added to 400 g of water for decomposition at a decomposition speed of 3000 rpm for 15 min. Then, the prepared raw materials containing reinforcing agent and surfactant were added and stirred at a speed of 500 rpm for 10 min, and then at a speed of 1500 rpm for 10 min for foaming.

[0041] (4) Papermaking: Pour the prepared fiber-containing foam slurry into a forming funnel and filter to obtain a wet paper web. Press the wet paper web with a force of 5N and then place it in a flat dryer at a drying temperature of 95°C for 20 minutes to obtain a paper web with a basis weight of 100 g / m 2 Paper-based material.

[0042] It can be seen from Tables 1-4 that compared with the control example, the addition of sodium carboxymethyl cellulose can effectively improve the tensile strength, uniformity and tear strength of the paper-based material, but has a certain negative impact on the bulk.

[0043] Comprehensive comparison of Examples 1, 2, and 3 shows that nanocellulose, polyacrylamide, and sodium carboxymethylcellulose can all improve the tensile strength of paper-based materials, among which sodium carboxymethylcellulose has the most obvious effect. The addition of reinforcing agents has a negative effect on the bulk of paper-based materials, among which nanocellulose has the least negative impact. Nanocellulose, polyacrylamide, and sodium carboxymethylcellulose can all improve the uniformity of paper, among which polyacrylamide has the best uniformity improvement, with a uniformity of 91. The addition of reinforcing agents significantly improves the tear strength of paper-based materials, among which sodium carboxymethylcellulose has the best improvement effect, which is 21.3% higher than the control example. Figure 1 , 2 From the comparison of Figures 3 and 4, it can be seen that after adding the paper enhancer, the size distribution of the foam is more uniform. The foam size of cationic polyacrylamide is concentrated between 400-500 microns, the foam size of nanocellulose is concentrated between 400-600 microns, and the foam size of sodium carboxymethyl cellulose is concentrated between 450-500 microns.

[0044] Comparative Example 1

[0045] (1) Prepare surfactant solution: add 0.3 g of fatty alcohol polyoxyethylene ether to 10 g of water, stir initially with a glass rod, and then ultrasonicate for 10 min.

[0046] (2) Preparation of fiber-containing foam slurry: 1.8 g of absolute dry fiber was added to 400 g of water for decomposition at a decomposition speed of 3000 rpm for 15 min. Then the prepared surfactant solution was added and stirred at a speed of 500 rpm for 10 min, and then at a speed of 1500 rpm for 10 min for foaming.

[0047] (3) Papermaking: Pour the prepared fiber-containing foam slurry into a forming funnel and filter to obtain a wet paper web. Press the wet paper web with a force of 5N and then place it in a flat dryer at a drying temperature of 95°C for 20 minutes to obtain a paper web with a basis weight of 100 g / m 2 Paper-based material.

[0048] It can be seen from Tables 1-4 that compared with the control example, after adding the reinforcing agent, various indicators of the paper-based material are improved, but the bulkiness is reduced.

[0049] Performance Testing

[0050] Table 1 Effect of different paper reinforcing agents on tensile strength

[0051]

[0052] Table 2 Effect of different paper reinforcing agents on bulk

[0053]

[0054] Table 3 Effect of different paper strengthening agents on uniformity

[0055]

[0056] Table 4 Effect of different paper reinforcing agents on tear index

[0057]

[0058] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

Claims

1. A method for preparing wood fiber paper-based materials by foam molding, characterized in that: Follow these steps: S1, beating a wood pulp board to obtain pulp, and then performing a decomposition treatment on the pulp; S2, adding a paper strengthening agent and a surfactant to the slurry of S1 and stirring; S3, papermaking the pulp treated in step S2 to obtain a wood fiber paper-based material.

2. The method for preparing wood fiber paper-based material by foam molding according to claim 1, characterized in that: In step S1, the wood pulp is one or more of bleached coniferous pulp, unbleached coniferous pulp, bleached broadleaf pulp, unbleached broadleaf pulp, bamboo pulp, straw pulp, and hemp pulp, the average length of the pulp is 1mm-3mm, and the beating degree is 15°SR-60°SR.

3. The method for preparing wood fiber paper-based material by foam molding according to claim 1, characterized in that: In the step S2, the surfactant is a nonionic surfactant, and one or more of polyoxyethylene sorbitan fatty acid ester, fatty alcohol polyoxyethylene ether, Triton X-100, and alkylphenol polyoxyethylene ether are used.

4. The method for preparing wood fiber paper-based material by foam molding according to claim 1, characterized in that: In step S2, the paper strengthening agent is one or more of nanocellulose, sodium carboxymethyl cellulose, polyacrylamide, and starch.

5. The method for preparing wood fiber paper-based material by foam molding according to claim 4, characterized in that: The amount of surfactant used in step S2 is 0.1%-5%.

6. The method for preparing wood fiber paper-based material by foam molding according to claim 3, characterized in that: The dosage of the enhancer in step S2 is 0.1%-5%.

7. The method for preparing wood fiber paper-based material by foam molding according to claim 1, characterized in that: In the step S2, the paper strengthening agent and the surfactant are blended by ultrasonication for 10 minutes and stirred for 10-60 minutes.

8. The method for preparing wood fiber paper-based material by foam molding according to claim 1, characterized in that: In step S2, the slurry concentration is 0.1%-2%, the stirring speed of the stirrer is 400-2000r / min, and the stirring is performed for 5-15min.

9. A wood fiber paper-based material prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Paper pulp foam material and preparation method thereof

    CN106832985A

  • Nano-cellulose-reinforced paper pulp foam material and preparation method thereof

    CN106835808A