Method for preparing mica paper through thermocompression bonding process
By modifying the combination of mica flakes and aramid fibers through hot pressing, the problem of insufficient mechanical strength and dielectric strength of mica paper in wet papermaking was solved, and high-performance preparation of mica paper was achieved.
Patent Information
- Application Number
- CN202411124408.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-01
AI Technical Summary
Existing wet papermaking technology has problems such as low mica retention, poor interfacial bonding, and poor fatigue resistance of aramid fibers when preparing aramid fiber reinforced mica paper, resulting in insufficient mechanical strength, dielectric strength, and long-term stability.
A hot-pressing process is used to modify mica flakes with a pretreatment liquid and mix them with aramid fiber chopped stock. The mixture is then combined with a polyimide film for surface treatment and hot-pressing to form a strong and tough composite structure.
It significantly improves the interlayer bonding strength, overall density, flexibility and electrical properties of mica paper, extends its service life and expands its application range.
Abstract
Description
Technical Field
[0001] The invention relates to a preparation technology of mica paper in paper insulating materials, in particular to a method for preparing mica paper through a hot pressing process. Background Art
[0002] Electrical insulation materials are important materials in modern motor equipment and are widely used in traction motors, high-voltage power generation and transmission equipment, electrical and electronic equipment, home appliances, new energy and other fields. Mica paper, as a widely used electrical insulation material, is a paper-based insulation material made by breaking mica flakes into fine mica flakes through thermochemical or hydraulic stripping, and then preparing it through modern papermaking wet papermaking. It is widely used in industry as an insulation material in cables and large electromechanical equipment. It has high electrical strength, low dielectric loss, high surface resistance and volume resistance. It also has excellent physical and chemical properties such as high insulation, corona resistance, acid and alkali resistance, radiation resistance, chemical stability, elasticity, high peelability, shear resistance and high tensile strength.
[0003] At present, the production of mica paper generally relies on wet papermaking technology. Although mica paper prepared from pure mica slurry shows excellent insulation performance and heat resistance, it still has certain defects in mechanical strength and wear resistance. In view of this, aramid fiber is often used as a reinforcing material in actual operation to complement the performance of mica paper. In the production process, aramid fiber slurry is mixed with mica for pulping. This is to build an effective internal reinforcement network through aramid fiber. When the mica paper encounters external force, the aramid fiber can bear part of the load and effectively disperse the stress, thereby avoiding the damage of the mica paper. At the same time, the structural stability of aramid fiber in high temperature environment ensures the stability of the performance of mica paper under high temperature conditions, significantly improves its mechanical strength, wear resistance, UV resistance and high temperature stability, not only effectively extends the service life of mica paper, but also significantly enhances its reliability and safety in various application environments. In addition, the introduction of aramid fiber also optimizes the processing performance of mica paper, making it easier to cut, fold and shape, so as to more flexibly meet the manufacturing needs of insulation parts of different shapes and sizes.
[0004] In the process of wet papermaking, the defects are:
[0005] 1. The loss of mica with smaller particle size leads to low mica retention rate, further reducing the distribution uniformity of mica in the two-dimensional plane, and reducing its insulation performance compared with pure mica paper. At the same time, due to the loss of mica with smaller particle size, large-particle mica sheets are stacked and arbitrarily built up, resulting in larger gaps and pores, which reduces the mechanical strength and seriously reduces the dielectric strength of aramid mica paper, limiting the improvement of its insulation performance.
[0006] Second, the interfacial bonding force between aramid fiber and mica is relatively poor, which makes the paper base material structure of wet-made aramid fiber mica paper relatively loose, thus seriously affecting its mechanical properties and dielectric properties, limiting the application of wet-made aramid fiber mica paper in fields requiring high strength and high dielectric properties.
[0007] 3. The fatigue resistance of aramid fiber is relatively poor. Long-term cyclic load will cause fatigue creep and strength loss of the fiber. This characteristic makes aramid fiber mica paper prone to performance degradation in an environment subjected to repeated stress or dynamic load.
[0008] In summary, it is necessary to make technical improvements to the many shortcomings of the above-mentioned wet papermaking technology in the preparation of aramid fiber reinforced mica paper, so as to further improve the comprehensive performance of mica paper, especially its mechanical strength, wear resistance, dielectric strength and long-term stability. Summary of the invention
[0009] The technical problem solved by the present invention is to provide a method for preparing mica paper by a hot pressing process, aiming to overcome the limitations of the existing wet papermaking technology, further improve the electrical properties, mechanical strength and comprehensive application performance of mica paper, so as to solve the shortcomings of the above-mentioned background technology.
[0010] The technical problem solved by the present invention is achieved by adopting the following technical solutions:
[0011] A method for preparing mica paper by a hot pressing process, specifically comprising the following steps:
[0012] S1 selects calcined mica clinker as raw material for pretreatment. During the pretreatment, the calcined mica clinker is placed in a container and a pretreatment liquid is added for soaking and modification treatment; the pretreatment liquid is an organic solvent, a surfactant and a small amount of a dispersant;
[0013] The organic solvent is ethanol, acetone or a mixture thereof; the surfactant is sodium dodecyl sulfate or sodium stearate; the dispersant is sodium polyacrylate or polyvinyl pyrrolidone; the mass ratio of the surfactant added is 1.0% to 3.0%, and the mass ratio of the dispersant added is 0.5% to 1.5%;
[0014] S2 hot-air drying the calcined mica clinker treated in step S1, mixing it with aramid fiber chopped material after drying, and then pulping to obtain mica slurry, using the mica slurry as raw material to prepare mica paper intermediate material by papermaking process;
[0015] The thickness of the mica paper in the middle is 1 / 3 to 2 / 5 of the thickness of the final mica paper to be formed;
[0016] S3 takes a polyimide film, and processes the surfaces of both sides of the polyimide film into a micro-nano rough surface by laser etching; at the same time, the rough surface of the mica paper intermediate material is subjected to surface grinding to obtain a rough surface;
[0017] S4 overlaps the rough surface of the mica paper intermediate material on the two side surfaces of the polyimide film after gluing, performs a hot pressing by roller pressing, trims the edges and cuts to a fixed length after the hot pressing is completed, overlaps the mica paper that has been cut to a fixed length and places it in a hot pressing mold to perform a second hot pressing treatment by molding; after the second hot pressing treatment, it is cooled to room temperature, and the finished mica paper is obtained after cutting, grinding and removing the burrs.
[0018] As a further limitation, in step S1, the calcined mica clinker uses natural muscovite and natural phlogopite as raw materials, which are washed and dried in sequence to obtain dry mica flakes, and then the dry mica flakes are calcined and then removed from impurities and size-screened to obtain.
[0019] As a further limitation, in step S1, when the calcined mica clinker is pretreated, a two-stage soaking treatment is adopted:
[0020] First, the pretreatment liquid is used for heat preservation and static soaking, and the heat preservation temperature is 50-70° C., and the soaking treatment is carried out for 12-24 hours, and then the calcined mica clinker is separated from the pretreatment liquid;
[0021] The separated calcined mica clinker is directly put into the new pretreatment liquid, the liquid-to-solid mass ratio is controlled to be 10:1-15:1, and it is fully stirred by a high-speed stirrer to further refine the mica flakes and undergo a secondary immersion treatment; the stirring speed of the high-speed stirrer is 1000-1500 rpm, and the stirring treatment time is 20-30 min.
[0022] As a further limitation, when hot air drying is performed in step S2, the temperature of the hot air circulation system is controlled at 120-150°C, and the processing time is 2-4 hours; the temperature should be evenly distributed in the hot air circulation system to reduce stress concentration caused by temperature gradient during the drying process.
[0023] As a further limitation, the aramid fiber chopped material as raw material has a monofilament length of 4 to 7 mm and a denier of 1 to 1.5D, and is pre-dispersed and treated with a silane coupling agent before being added to the pulping process to ensure its uniform distribution and effective bonding in the mica slurry.
[0024] As a further limitation, when pulping mica slurry, the mass of the corresponding aramid fiber chopped material added is 5% to 15% of the calcined mica clinker to ensure that the aramid fiber forms an effective reinforcement network in the mica paper, while maintaining an appropriate mica content to ensure its insulation performance.
[0025] As a further limitation, during the mica slurry slurrying, filler is also added to the mica slurry, and the filler is one or a combination of nano silicon dioxide and nano aluminum oxide, and the addition amount is 0.8-3.5% of the total mass of the mica slurry.
[0026] As a further limitation, in step S4, when the laminated composite structure of mica paper intermediate material-polyimide film-mica paper intermediate material is subjected to hot pressing;
[0027] The primary hot pressing parameters of the roller pressing method are a roller pressing temperature of 150-180°C and a roller pressing surface pressure of 2-4 MPa;
[0028] The secondary hot pressing parameters of the molding method are molding temperature of 200-250°C, molding pressure of 5-8MPa, and molding maintenance of 5-10min.
[0029] As a further limitation, during the secondary hot pressing process of the molding method, the thickness of the laminated mica paper is 8 to 20 mm. When the thickness of the laminated mica paper is insufficient, high-density flat plastic plates can be used as pads on the upper and lower surfaces of the mica paper to ensure uniform pressure distribution during the hot pressing process and avoid local overpressure or underpressure.
[0030] As a further limitation, during the secondary hot pressing process of the molding method, an inert gas can be used to protect the molding area.
[0031] Beneficial effect: The method for preparing mica paper by hot pressing technology of the present invention is to paper pretreated mica flakes and aramid fibers and then perform surface treatment with polyimide film respectively, and then overlap and directly hot press to form after treatment; this mica paper forming method can greatly enhance the interlayer bonding strength and overall density of mica paper, so as to overcome the performance defects of loose structure and poor interlayer bonding force in the preparation of aramid fiber mica paper in the traditional single wet papermaking process. Compared with the traditional wet papermaking mica paper, the mica paper prepared by this method has advantages in flexibility, strength and structural stability, and realizes performance improvement in electrical properties, tear resistance and peeling resistance, which provides a technical reference for improving the comprehensive performance of mica paper and expanding its application range. DETAILED DESCRIPTION
[0032] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0033] In the following embodiments, it will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as the meaning in the context of the prior art, and will not be interpreted with an idealized or overly formal meaning unless defined as herein.
[0034] A method for preparing mica paper by a hot pressing process, specifically comprising the following steps:
[0035] In this embodiment, the method realizes the preparation of mica paper by the following specific steps:
[0036] First, natural muscovite and natural phlogopite are selected as raw materials, and they are washed and dried in sequence to obtain dry mica sheets. The dry mica sheets are calcined and then cooled to room temperature in a furnace, and then impurities are removed and size-screened to obtain calcined mica clinker for preparing mica paper. The calcined mica clinker is pretreated with a pretreatment liquid, and the corresponding pretreatment liquid is prepared by the following method:
[0037] Ethanol and acetone are compounded in a mass ratio of 1:1 to obtain a base solvent, and then a surfactant, sodium dodecyl sulfate, and a dispersant, sodium polyacrylate, are added in proportion to the base solvent. Specifically, the mass ratio of the surfactant, sodium dodecyl sulfate, is 2.0%, and the mass ratio of the dispersant, sodium polyacrylate, is 1.0%. The mixture is stirred until the components are uniformly dissolved to form a transparent or translucent pretreatment liquid.
[0038] This pre-treatment solution is designed to effectively penetrate and modify mica flakes through its combination of chemical components, improve its dispersibility and wettability, and lay a good foundation for subsequent processes.
[0039] When using the pretreatment liquid to treat the calcined mica clinker, a two-stage immersion treatment process is adopted:
[0040] During the treatment, the calcined mica clinker is first soaked in a pretreatment liquid for insulation. During this process, it is only necessary to keep the pretreatment liquid completely immersed in the calcined mica clinker. The insulation temperature is controlled to be set at 65°C, and the soaking treatment is carried out for 24 hours to ensure that the pretreatment liquid fully penetrates and modifies the mica surface and enhances its bonding with subsequent materials. Subsequently, the soaking liquid is discharged and rinsed with clean water to remove excess pretreatment liquid residue. The rinsing time is controlled at 30 to 45 seconds, and the temperature is maintained at room temperature or slightly higher to avoid excessive dissolution or damage to the modified layer that has been formed.
[0041] Subsequently, the calcined mica clinker was filtered and drained from the pretreatment liquid to complete solid-liquid separation. After separation, the calcined mica clinker was directly put into the new pretreatment liquid for secondary immersion treatment, and the liquid-to-solid mass ratio was controlled to be 15: 1. During the secondary immersion treatment, high-speed stirring was performed, the stirring speed was controlled to be 1200 rpm, and the stirring setting time was 24 minutes.
[0042] The secondary soaking process has two functions:
[0043] On the one hand, it is used to optimize the modification effect of the pre-insulation static immersion on the calcined mica clinker, and further promote the organic solvent, surfactant and dispersant in the pretreatment liquid to penetrate evenly and deeply into the microstructure of the mica flakes.
[0044] On the other hand, high-speed mechanical stirring is used to break up the calcined mica clinker and suspend it in the pretreatment liquid, so as to achieve a hydraulic stripping effect similar to mechanical assistance, so that the mica flakes are peeled into smaller scales and the wettability and dispersibility between the mica scales are optimized.
[0045] Compared with the traditional technical solution of hydraulically stripping mica materials for direct modification, this secondary immersion treatment process not only significantly improves the refinement of mica flakes, but also enables the organic solvents, surfactants and dispersants in the pretreatment liquid to penetrate more evenly into the interior and surface of the mica flakes, enhancing the wettability and dispersibility between mica flakes, and greatly enhancing its surface activity and compatibility with subsequent added materials, so as to facilitate better combination with aramid fiber chopped materials in the subsequent pulping and papermaking process to form a stable mica slurry.
[0046] After the modification treatment is completed, the calcined mica clinker needs to be dried to maintain its modification effect. During the treatment, the pretreated mica flakes are first removed from the pretreatment liquid, filtered to remove excess liquid, and then placed in a hot air circulation system for drying. During the treatment, the temperature of the hot air circulation system is controlled at 120-150°C, and the treatment time is 2-4 hours. The temperature should be evenly distributed in the hot air circulation system. The specific operation method is to set multiple air outlets and evenly heat the drying area to reduce the stress concentration caused by the temperature gradient during the drying process, so as to ensure the quality of the calcined mica clinker after drying.
[0047] In the pulping and papermaking stage, the calcined mica clinker treated as above is mixed with aramid fiber chopped material and filler as raw materials for pulping. The corresponding aramid fiber chopped material as raw material is chopped meta-aramid fiber monofilament with a monofilament length of 4-7 mm and a fineness of 1-1.5D, and the chopped meta-aramid fiber monofilament has been pre-dispersed and treated with a silane coupling agent before the pulping process to ensure its uniform distribution in the mica slurry and its bonding performance with the mica material. The addition amount of aramid fiber chopped material is 7% of the mass of the calcined mica clinker; and the filler is a composition of nano-silicon dioxide and nano-alumina in a mass ratio of 1:1, and the addition amount of the filler is 2.4% of the mass of the calcined mica clinker.
[0048] During the pulping process, the aforementioned materials are mixed in proportion to prepare mica pulp, and the obtained mica pulp enters the pulp storage tank of the paper machine, and is diluted with water that meets the quality requirements into a slurry of a certain concentration (processed according to the requirements of the corresponding paper machine), and the slurry is pumped into the mesh of the paper machine for papermaking and molding. In this process, mica flakes are gradually deposited on the mesh surface to form a paper tire, and are dehydrated by vacuum filtration or pressurized dehydration to reduce the moisture content in the paper tire. The pressed mica paper enters the drying section for drying to further remove moisture and reach the required dryness; finally, the dried mica paper is rolled into a tube by a paper reel for subsequent processing and use. It should be noted that the mica paper obtained in this step is a mica paper intermediate material, and its thickness is 1 / 3 of the thickness of the final mica paper to be formed. Aramid fiber chopped material, with its excellent mechanical properties and chemical stability, forms a strong reinforcement network in the mica paper intermediate material, effectively improving the tensile strength and tear resistance of the mica paper intermediate material. The addition of nano-scale silica and alumina as structural fillers further refines the internal structure of the mica paper intermediate material, reduces the porosity, and thus improves the density and dielectric properties of the mica paper intermediate material.
[0049] Commercially available polyimide films that meet the thickness requirements and the aforementioned mica paper intermediate material are taken for surface treatment respectively. For the polyimide film, the surface of the polyimide film is bombarded with high-energy particles by laser etching to produce a micro-nanoscale rough surface on its surface. The treatment of the mica paper intermediate material is carried out on the rough side of the mica paper intermediate material, and the treatment method is to physically rub its surface to obtain a rough surface.
[0050] Next, the core link of the hot pressing process is to lay the surface-treated polyimide film and mica paper intermediate material flat, apply glue to the rough surface of the mica paper intermediate material, and then accurately overlap it on the surface of the polyimide film. The laminated materials are then subjected to a hot pressing treatment using a rolling device. The rolling temperature is set to 180°C and the pressure is controlled at 2.8MPa to ensure a good initial bond between the mica paper intermediate material and the polyimide film, while avoiding deformation or damage to the material due to excessive temperature and pressure.
[0051] After the hot pressing process is completed, the edges are trimmed immediately to remove excess, irregular, damaged and misplaced parts; after the trimming work is completed, the mica paper is cut to a fixed length according to the preset length specifications to ensure that each section of material meets the established length requirements.
[0052] Subsequently, the mica paper cut to length is stacked neatly and placed in a hot pressing mold of the same size to ensure that the thickness of the stacked mica paper is 15 to 16 mm, and then the whole is placed in a hot press for secondary hot pressing. During the secondary hot pressing stage, the temperature of the hot pressing mold needs to be further increased to 250°C, and the molding pressure is increased to 8MPa to promote molecular-level bonding between the polyimide film and the mica paper intermediate material to form a strong and tough composite structure. The hot pressing time at this stage is maintained at 5 to 10 minutes to further improve the density and stability of the material, and to ensure that the composite structure is fully cured and achieves the expected physical and electrical properties. The specific duration of the aforementioned hot pressing time is positively correlated with the thickness of the finished mica paper. In this embodiment, the selected hot pressing treatment duration is 8 minutes.
[0053] In addition, in another embodiment, in order to further optimize the performance of the product, an inert gas (such as nitrogen or argon) can be introduced during the secondary hot pressing process to prevent oxidation of the material at high temperature, while reducing the generation of pores and bubbles, and improving the compactness and dielectric properties of the product. In addition, when the thickness of the stacked mica paper is insufficient, a high-density flat plastic plate can be used as a cushion on the upper and lower surfaces of the mica paper stack with insufficient thickness to ensure uniform pressure distribution during the hot pressing process and avoid the occurrence of local overpressure or underpressure.
[0054] After the secondary hot pressing is completed, the material is cooled naturally to room temperature. During the cooling process, the cooling rate is controlled to avoid the internal stress of the mica paper caused by too fast or too slow cooling, which will affect the dimensional stability and mechanical properties of the product. After naturally cooling to room temperature, it is finely cut, polished and deburred to ensure that the final product meets the established quality standards and flatness requirements. The mica paper processed through the above process is the finished product and can be used or processed later.
[0055] The mica paper prepared by the method of this embodiment has a thickness range of 0.08-0.11 mm, a basis weight of 168-172, a dielectric strength of 18-22 KV / mm, a tensile strength (GB / T13022-91) of 64-68 MPa, and a heat loss (thermal shrinkage, GB / T13022-91) of 1.9-2.2%. Compared with the corresponding technical indicators of the commercially available 507 type mica paper of the same type (having similar thickness and basis weight), its dielectric strength is close, and the tensile strength performance is improved by 10-15%, and the heat loss performance is improved by 8-10%. At the same time, the mica paper prepared by the embodiment will not peel off and break at a maximum bending angle of 110°, and the number of surface damages when the surface is continuously scraped with a nylon brush is greater than 60 times.
[0056] Therefore, the solution of this embodiment not only overcomes many shortcomings of traditional wet papermaking technology in the process of preparing aramid fiber reinforced mica paper, but also can significantly improve the mechanical strength and long-term stability of mica paper while ensuring the electrical properties of mica paper, and provides a new idea and method for the preparation of high-performance insulating materials.
[0057] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing mica paper by a hot pressing process, characterized in that: The specific steps include the following: S1 selects calcined mica clinker as raw material for pretreatment. During the pretreatment, the calcined mica clinker is placed in a container and a pretreatment liquid is added for soaking and modification treatment; the pretreatment liquid is an organic solvent, a surfactant and a small amount of a dispersant; The organic solvent is ethanol, acetone or a mixture thereof; the surfactant is sodium dodecyl sulfate or sodium stearate; the dispersant is sodium polyacrylate or polyvinyl pyrrolidone; the mass ratio of the surfactant added is 1.0% to 3.0%, and the mass ratio of the dispersant added is 0.5% to 1.5%; S2 hot-air drying the calcined mica clinker treated in step S1, mixing it with aramid fiber chopped material after drying, and then pulping to obtain mica slurry, using the mica slurry as raw material to prepare mica paper intermediate material by papermaking process; The thickness of the mica paper in the middle is 1 / 3 to 2 / 5 of the thickness of the final mica paper to be formed; S3 takes a polyimide film, and processes the surfaces of both sides of the polyimide film into a micro-nano rough surface by laser etching; at the same time, the rough surface of the mica paper intermediate material is subjected to surface grinding to obtain a rough surface; S4 overlaps the rough surface of the mica paper intermediate material on the two side surfaces of the polyimide film after gluing, performs a hot pressing by roller pressing, trims the edges and cuts to a fixed length after the hot pressing is completed, overlaps the mica paper that has been cut to a fixed length and places it in a hot pressing mold to perform a second hot pressing treatment by molding; after the second hot pressing treatment, it is cooled to room temperature, and the finished mica paper is obtained after cutting, grinding and removing the burrs.
2. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: In step S1, the calcined mica clinker uses natural muscovite and natural phlogopite as raw materials, washes and dries in sequence to obtain dry mica flakes, and then calcines the dry mica flakes and removes impurities and sizes them to obtain.
3. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: In step S1, when pre-treating the calcined mica clinker, a two-stage soaking treatment is adopted: First, the pretreatment liquid is used for heat preservation and static soaking, and the heat preservation temperature is 50-70° C., and the soaking treatment is carried out for 12-24 hours, and then the calcined mica clinker is separated from the pretreatment liquid; The separated calcined mica clinker is directly put into the new pretreatment liquid, the liquid-to-solid mass ratio is controlled to be 10:1-15:1, and it is fully stirred by a high-speed stirrer to further refine the mica flakes and undergo a secondary immersion treatment; the stirring speed of the high-speed stirrer is 1000-1500 rpm, and the stirring treatment time is 20-30 min.
4. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: When the hot air drying process is performed in step S2, the temperature of the hot air circulation system is controlled at 120-150°C, and the process time is 2-4 hours.
5. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: The aramid fiber chopped material as raw material is a chopped meta-aramid fiber monofilament with a monofilament length of 4 to 7 mm and a fineness of 1 to 1.5D, which is pre-dispersed and treated with a silane coupling agent before being added into the pulping process.
6. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: When mica slurry is being slurried, the mass of the corresponding aramid fiber chopped material added is 5% to 15% of the calcined mica clinker.
7. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: When the mica slurry is being slurried, fillers are added to the mica slurry. The fillers are one or a combination of nano silicon dioxide and nano aluminum oxide, and the addition amount is 0.8-3.5% of the total mass of the mica slurry.
8. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: In step S4, when the laminated composite structure of mica paper intermediate material-polyimide film-mica paper intermediate material is subjected to hot pressing; The primary hot pressing parameters of the roller pressing method are a roller pressing temperature of 150-180°C and a roller pressing surface pressure of 2-4 MPa; The secondary hot pressing parameters of the molding method are molding temperature of 200-250°C, molding pressure of 5-8MPa, and molding maintenance of 5-10min.
9. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: During the secondary hot pressing process of the molding method, the thickness of the laminated mica paper is 8 to 20 mm. When the thickness of the laminated mica paper is insufficient, high-density flat plastic plates are used as pads on the upper and lower surfaces of the mica paper to compensate for the thickness.
10. The method for preparing mica paper by hot pressing process according to claim 1, characterized in that: During the secondary hot pressing process of the molding method, inert gas is used to protect the molding area.
Citation Information
Patent Citations
Mica paper production method
CN108505387A
High-wear-resistance mica paper adhesive tape and preparation method thereof
CN111471407A
Mica paper tape with high wear resistance and aging resistance and preparation method thereof
CN111472207A
Reinforcing treatment method of mica paper
CN116716754A