Asphalt construction joint quality control method

In the construction of asphalt pavement in coastal areas, two pavers are used to spread and compact the oblique joints with staggered distances, and lay a maintenance layer on the joints, the problem of quality control of asphalt pavement joints is solved. , improves the road's rut ​​resistance and durability and extends its service life.

CN118880696APending Publication Date: 2024-11-01CCCC SHEC FIRST HIGHWAY ENG
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411263122.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In coastal areas, the quality control of asphalt pavement joint construction is difficult to ensure, affecting the road's rut ​​resistance, durability and service life.

Method used

Two pavers are staggered 10-20m for diagonal joint paving, combined with rolling and compacting treatment, and laying a curing layer on the construction joints with high temperature steam for maintenance, ensuring the uniform distribution of asphalt mixture and high temperature stability .

Benefits of technology

Through this method, the quality of asphalt pavement joints is improved, the rut resistance and durability are enhanced, the service life of the road is extended, and the construction quality under different road conditions is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880696A_ABST
    Figure CN118880696A_ABST
Patent Text Reader

Abstract

The invention discloses an asphalt construction joint quality control method which comprises the following steps: S1, paving an asphalt mixture on the surface of a joint by using two pavers, and adopting an inclined joint as a longitudinal joint of paving layers of the two pavers to avoid seam marks; s2, carrying out rolling compaction treatment on the asphalt mixture; s3, a maintenance layer is laid on the upper surface of the construction joint, and the maintenance layer is dismantled after maintenance is completed, the SBS modified asphalt, the coarse aggregate and the fine aggregate with the mass ratio being 65: 20: 15 are mixed to obtain the asphalt mixture for construction operation, good joint quality guarantee is achieved, and the method can be widely applied to different road conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of asphalt construction joint quality control, and more specifically, to an asphalt construction joint quality control method. Background Art

[0002] Asphalt pavement joint construction is an important part of asphalt pavement construction. The quality of asphalt pavement joint construction directly affects the appearance, internal quality and smoothness of the road, and affects the use effect and service life of the road.

[0003] How to control the quality of asphalt construction joints in coastal areas is also crucial. Good quality control of asphalt joints can improve the rutting resistance of the asphalt surface layer, increase durability, increase anti-aging ability, and extend the service life of the road. Therefore, it is necessary to provide a quality control method for asphalt construction joints in coastal areas. Summary of the invention

[0004] In order to achieve these purposes and other advantages according to the present invention, a preferred embodiment of the present invention provides a method for controlling the quality of asphalt construction joints, comprising the following steps:

[0005] S1. Use two pavers to spread the asphalt mixture on the joint surface. The two pavers are staggered 10-20m in front and back. The longitudinal joints of the paving layers of the two pavers are inclined to avoid seam marks. During the paving process, check whether the loose paving thickness meets the requirements at any time. If it does not meet the requirements, it should be adjusted in time. The asphalt mixture uses a mixture of SBS modified asphalt, coarse aggregate and fine aggregate, and the mass ratio of the three is 65:20:15.

[0006] S2. Rolling and compacting the asphalt mixture, wherein the rolling and compacting process includes initial compaction, re-compacting and final compaction. During the rolling process, the initial compaction temperature is controlled to be not less than 150°C, and the final compaction temperature is controlled to be not less than 90°C. The length of the rolling section is controlled to be 20m to 30m for initial compaction, and 50m to 80m for re-compacting and final compaction;

[0007] S3. A curing layer is laid on the upper surface of the construction joint, wherein the curing layer includes a plurality of pipes and curing covers arranged in parallel to each other, and adjacent pipes are directly connected through a plurality of vertically arranged connecting pipes, and the pipes are connected to the steam equipment. Steam holes are provided at the bottom of the pipes and the connecting pipes, and a support rod is provided at the bottom of the pipes. Traveling wheels are installed at the bottom of the support rods. The curing cover covers the pipes inside to form a curing space between the construction joint and the curing cover. The high-temperature steam produced by the steam equipment is transported to the curing space through the pipes to maintain the joints, and the curing layer is removed after the curing is completed.

[0008] According to a preferred embodiment of the present invention, in S1, when two pavers are used for paving, two ironing plates with the same vibration frequency and amplitude are used to vibrate the paving layers of the two pavers to avoid uneven distribution of coarse and fine materials on the surface and under the paving layer due to uneven excitation intensity; the initial elevation angles of the ironing plates of the two pavers should be consistent; after the pavers are in place, the ironing plates should be preheated to not less than 100°C 0.5h to 1h in advance. The ironing plates of the pavers should be tightly spliced ​​without gaps.

[0009] According to a preferred embodiment of the present invention, in S1, the initial compaction degree of paving is ≥85%, and the initial compaction degrees of the two pavers should be consistent.

[0010] According to a preferred embodiment of the present invention, in said S2, before the asphalt mixture is compacted, no one is allowed to step on it, and after compaction, if local segregation of the asphalt mixture is found, the segregated part needs to be repaired.

[0011] According to a preferred embodiment of the present invention, in S2, during rolling, the roller wheel should face the paver and roll from the outside to the center, and roll from low to high on super-high sections, and keep the driving wheel rolling from low to high on the ramp.

[0012] According to a preferred embodiment of the present invention, in S2, in the initial compaction stage, two double-steel-wheel oscillating rollers use half-width span seam rolling, first static rolling for 1 time, and then vibrating rolling for 1 time, and the rolling speed is maintained at 2.5km / h. In the re-compacting stage, two rubber-wheel rollers use half-width span seam sleeve wheel cyclic rolling, 5 times each, and follow the initial compaction, and the rolling speed is maintained at 3.5km / h. In the final compaction stage, one double-steel-wheel vibrating roller performs static compaction for 2 times, and the rolling speed is maintained at 4km / h.

[0013] According to a preferred embodiment of the present invention, in S1, when two pavers are used in echelon paving to produce longitudinal joints, loose paving oblique joints are used and cross-joint rolling is performed once in the form of hot joints.

[0014] According to a preferred embodiment of the present invention, in S1, during the paving process, if a longitudinal cold joint is produced, it is necessary to use a pickaxe to scrape off the edges to leave stubble before the asphalt mixture is completely cooled, and during the initial rolling at a later time, 5 to 10 cm of the mixture is laid on the surface of the longitudinal cold joint and then compacted across the joint.

[0015] According to a preferred embodiment of the present invention, in S3, a temperature and humidity sensor is further provided at the bottom of the pipeline for detecting the temperature and humidity of the space.

[0016] The present invention includes at least the following beneficial effects: the present invention adopts an asphalt mixture obtained by mixing SBS modified asphalt, coarse aggregate and fine aggregate in a mass ratio of 65:20:15 for construction work, has good joint quality assurance, and can be widely used in different road conditions.

[0017] Other advantages, objectives and features of the present invention will be embodied in part through the following description, and in part will be understood by those skilled in the art through study and practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a schematic diagram of the structure of the curing layer in the present invention. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with the accompanying drawings so that those skilled in the art can implement the invention with reference to the description.

[0020] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art can think of other obvious variations. The basic principles of the present invention defined in the following description can be applied to other embodiments, variations, improvements, equivalents, and other technical solutions that do not deviate from the spirit and scope of the present invention.

[0021] Those skilled in the art should understand that, in the disclosure of the present invention, the orientation or position relationship indicated by the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc. are based on the orientation or position relationship shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.

[0022] It is to be understood that the term "one" should be understood as "at least one" or "one or more", that is, in one embodiment, the number of an element may be one, while in another embodiment, the number of the element may be multiple, and the term "one" should not be understood as a limitation on the quantity.

[0023] like Figure 1 As shown, a preferred embodiment of the present invention provides a method for controlling the quality of asphalt construction joints, comprising the following steps:

[0024] S1. Use two pavers to spread the asphalt mixture on the joint surface. The two pavers are staggered 10-20m in front and back. The longitudinal joints of the paving layers of the two pavers are inclined to avoid seam marks. During the paving process, check whether the loose paving thickness meets the requirements at any time. If it does not meet the requirements, it should be adjusted in time.

[0025] Asphalt mixture needs to be transported before S1. The transport vehicle must be well maintained, the compartment must be cleaned, and a thin layer of isolation agent or anti-sticking agent (diesel should not be used) should be applied to the bottom and side panels of the compartment, but no excess liquid should be accumulated at the bottom of the compartment. After each loading, the asphalt mixture must not exceed the compartment board. The asphalt mixture that sticks to the top of the compartment board during loading should be cleaned with a shovel in time to prevent it from falling into the paver and being paved on the road surface after cooling and unloading, affecting the quality of the project. After each unloading, the driver of the material truck should use a small shovel to clean the fine asphalt mixture on the rear gate while it is still hot on site to avoid the rear gate being difficult to close completely after cooling and hardening, causing the asphalt mixture to drip on the road and pollute the road surface. A car wash point should be set up at the main road entrance and exit of the asphalt pavement construction to reduce the pollution of the road surface by vehicles entering the site.

[0026] The transport capacity of asphalt mixture transport trucks should be more than the paving capacity. When paving begins, there should be no less than 5 transport trucks waiting to unload at the construction site. The transport capacity should match the production capacity and the paver. The transport truck should have a tarpaulin covering facility. During the transportation process until the unloading is completed, the tarpaulin should remain covered throughout the process and should not be removed in advance. The tarpaulin of the transport truck must be tied tightly at the four corners. It is strictly forbidden to tie only the front two ends of the vehicle to prevent the tarpaulin from floating when the vehicle is driving.

[0027] In this embodiment, in S1, the initial compaction degree of paving is ≥85%, and the initial compaction degrees of the two pavers should be consistent.

[0028] In this embodiment, in S1, when two pavers are used in echelon paving to produce longitudinal joints, loose paving oblique joints are used, and cross-joint rolling is performed once in the form of hot joints.

[0029] In this embodiment, in S1, if a longitudinal cold joint is produced during the paving process, it is necessary to use a pickaxe to scrape off the edges to leave stubble before the asphalt mixture is completely cooled, and during the initial rolling in the later stage, 5 to 10 cm of the mixture is laid on the surface of the longitudinal cold joint and then compacted across the joint.

[0030] S2. Rolling and compacting the asphalt mixture, wherein the rolling and compacting process includes initial compaction, re-compacting and final compaction. During the rolling process, the initial compaction temperature is controlled to be not less than 150°C, and the final compaction temperature is controlled to be not less than 90°C. The length of the rolling section is controlled to be 20m to 30m for initial compaction, and 50m to 80m for re-compacting and final compaction;

[0031] Before the asphalt mixture is compacted, no one is allowed to walk on it. If local segregation is found in the asphalt mixture after compaction, the segregated area needs to be repaired.

[0032] Continuous and stable paving is the most important measure to improve the smoothness of the road surface. The paver cannot stop to wait for materials, and the paver must work continuously and smoothly. It is strictly forbidden to arbitrarily pave quickly for a few minutes and then stop to wait for the next truck of materials. Eating during paving should be carried out in batches and alternately, and it is forbidden to stop paving to eat. Try to stop the machine once a day.

[0033] The rolling route and direction should not be changed suddenly; the roller should slow down when starting and stopping, and the brakes are not allowed. The roller should not turn back on the same cross section. Small vibrating flat machines can be used to roll the parts that cannot be rolled by the roller.

[0034] Obvious signs are set up at the initial, repeated and final compaction sections. Special posts and personnel are set up to manage and inspect the loose paving thickness, compaction sequence, roller combination, compaction times, compaction speed and compaction temperature. The surface layer should be compacted without leakage or over-compaction.

[0035] The roller should take measures to prevent the wheels from sticking, and a small amount of water can be sprayed. The water used should be clean water to avoid yellowing of the road surface caused by spraying water during rolling.

[0036] In this embodiment, in S2, in the initial compaction stage, two double-steel-wheel oscillating rollers use half-width span seam rolling, first static rolling for 1 time, and then vibrating rolling for 1 time, and the rolling speed is maintained at 2.5km / h. In the re-compacting stage, two rubber-wheel rollers use half-width span seam sleeve wheel cyclic rolling, 5 times each, and follow the initial compaction, and the rolling speed is maintained at 3.5km / h. In the final compaction stage, a double-steel-wheel vibrating roller performs static compaction 2 times, and the rolling speed is maintained at 4km / h.

[0037] In this embodiment, in S2, the roller wheels should face the paver during rolling, rolling from the outside to the center, rolling from low to high on super-high sections, and keeping the driving wheels rolling from low to high on ramps.

[0038] S3. Lay a curing layer on the upper surface of the construction joint, the curing layer includes a plurality of pipes 1 and curing covers 2 arranged in parallel to each other, adjacent pipes 1 are directly connected through a plurality of vertically arranged connecting pipes, the pipes are connected to the steam equipment, the bottoms of the pipes 1 and the connecting pipes are provided with steam holes, the bottom of the pipes is provided with support rods 3, the bottom of the support rods 3 is provided with walking wheels 4, the curing cover 2 covers the pipes inside, and a curing space is formed between the construction joint and the curing cover, and the high-temperature steam produced by the steam equipment is transported to the curing space through the pipe to maintain the joint, and the curing layer is removed after the maintenance is completed. In S3, a temperature and humidity sensor is also provided at the bottom of the pipe to detect the temperature and humidity of the space.

[0039] In this embodiment, the asphalt mixture is a mixture of SBS modified asphalt, coarse aggregate and fine aggregate, and the mass ratio of the three is 65:20:15. The coarse aggregate must be rolled by a large-scale complete set of impact crushers and specified dust removal and shaping processing technology. The rolled coarse aggregate is hard, clean, dry, non-weathered, free of impurities, and has a particle size close to a cube. It has a good particle shape and must not contain soil and dust. The fine aggregate uses machine-made sand (basalt or fresh hard limestone rolled) processed by special equipment, which should be clean, hard, dry, non-weathered, free of impurities or other harmful substances. The waste materials of the material yard cannot be used, and there is an appropriate particle gradation (0-2.36mm machine-made sand). Among them, SBS modified asphalt is a modified asphalt belonging to the elastic plastic type. Proper use can greatly improve the anti-rutting performance of the asphalt surface layer. Its effect is much better than that of ordinary asphalt. It can be maintained for a longer time in daily use. The durability and aging resistance are very good, which extends the service life of the highway.

[0040] In order to verify the water damage resistance of asphalt mixture, a water immersion Marshall test was carried out. The test results are shown in the table below.

[0041] Table 1 immersion Marshall stability test results

[0042]

[0043] 4) High temperature stability test: Rutting tests were carried out at 60±1℃ and 0.7±0.05MPa to test the high temperature stability of asphalt mixture. The test results of 60℃ dynamic stability and rutting specimen void ratio are shown in the table below.

[0044] Table 2 Rutting test results

[0045]

[0046]

[0047] According to a preferred embodiment of the present invention, in S1, when two pavers are used for paving, two ironing plates with the same vibration frequency and amplitude are used to vibrate the paving layers of the two pavers to avoid uneven distribution of coarse and fine materials on the surface and under the paving layer due to uneven excitation intensity; the initial elevation angles of the ironing plates of the two pavers should be consistent; after the pavers are in place, the ironing plates should be preheated to not less than 100°C 0.5h to 1h in advance. The ironing plates of the pavers should be tightly spliced ​​without gaps.

[0048] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes, and they can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the illustrations shown and described herein.

Claims

1. A method for controlling the quality of asphalt construction joints, characterized in that: The following steps are involved: S1. Use two pavers to spread the asphalt mixture on the joint surface. The two pavers are staggered 10-20m in front and back. The longitudinal joints of the paving layers of the two pavers are inclined to avoid seam marks. During the paving process, check whether the loose paving thickness meets the requirements at any time. If it does not meet the requirements, it should be adjusted in time. The asphalt mixture is a mixture of SBS modified asphalt, coarse aggregate and fine aggregate, and the mass ratio of the three is 65:20:

15. S2. Rolling and compacting the asphalt mixture, wherein the rolling and compacting process includes initial compaction, secondary compaction and final compaction. During the rolling process, the initial compaction temperature is controlled to be not less than 150°C and the final compaction temperature is controlled to be not less than 90°C; S3. A curing layer is laid on the upper surface of the construction joint, wherein the curing layer includes a plurality of pipes and curing covers arranged in parallel to each other, and adjacent pipes are directly connected through a plurality of vertically arranged connecting pipes, and the pipes are connected to the steam equipment. Steam holes are provided at the bottom of the pipes and the connecting pipes, and a support rod is provided at the bottom of the pipes. Traveling wheels are installed at the bottom of the support rods. The curing cover covers the pipes inside to form a curing space between the construction joint and the curing cover. The high-temperature steam produced by the steam equipment is transported to the curing space through the pipes to maintain the joints, and the curing layer is removed after the curing is completed.

2. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S1, when two pavers are used for paving, two ironing plates with the same vibration frequency and amplitude are used to vibrate the paving layers of the two pavers to avoid uneven distribution of coarse and fine materials on the surface and under the paving layer due to uneven vibration intensity; the initial elevation angles of the ironing plates of the two pavers are consistent; After the paver is in place, the screed plate should be preheated to no less than 100°C 0.5h to 1h in advance. The screed plate of the paver should be spliced ​​tightly without any gaps.

3. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S1, the initial compaction degree of paving is ≥85%, and the initial compaction degrees of the two pavers should be consistent.

4. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S2, before the asphalt mixture is compacted, no one is allowed to step on it, and after compaction, if local segregation of the asphalt mixture is found, the segregated part is repaired.

5. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S2, during rolling, the roller wheel faces the paver and rolls from the outside to the center. On super-high sections, the roller rolls from low to high. On ramps, the driving wheel is kept rolling from low to high.

6. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S2, in the initial compaction stage, two double-steel-wheel oscillating rollers use half-width span seam rolling, first static rolling once, then vibrating rolling once, and the rolling speed is maintained at 2.5km / h. In the re-compacting stage, two rubber-wheel rollers use half-width span seam sleeve wheel cyclic rolling, 5 times each, and follow the initial compaction, and the rolling speed is maintained at 3.5km / h. In the final compaction stage, a double-steel-wheel vibrating roller performs static compaction twice, and the rolling speed is maintained at 4km / h.

7. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S1, when two pavers are used in echelon paving to produce longitudinal joints, loose paving oblique joints are used, and cross-joint rolling is performed once in the form of hot joints.

8. The asphalt construction joint quality control method according to claim 1 is characterized in that: In S1, if longitudinal cold joints are produced during the paving process, it is necessary to use a pickaxe to scrape off the edges to leave stubble before the asphalt mixture is completely cooled, and during the initial rolling, 5 to 10 cm of mixture is laid on the surface of the longitudinal cold joints and then compacted across the joints.

9. The asphalt construction joint quality control method according to claim 1, characterized in that: In S3, a temperature and humidity sensor is also provided at the bottom of the pipeline for detecting the temperature and humidity of the space.

Citation Information

Patent Citations

  • Construction method of asphalt concrete pavement of skid pad

    CN104631267A

  • Method for lap jointing of longitudinal cold joints of asphalt concrete pavement

    CN107338696A

  • Sand grain type asphalt construction process for central dividing band

    CN112575652A

  • Integrated bridge pavement maintenance equipment

    CN115652829A