Preparation method and application of V2CTX-coated MoS2 composite material

Through the preparation and application of V2CTx@MoS2 composite material, the problem of insufficient sensitivity of ammonia sensors in the prior art in low concentration detection is solved, and high sensitivity detection and rapid response to ammonia are achieved, and the sensor has good reproducibility and stability.

CN118883644APending Publication Date: 2024-11-01ACADEMY OF MILITARY MEDICAL SCIENCES
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410864844.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing gas sensors based on pure V2CTx cannot achieve high sensitivity detection of ammonia under high noise and low response, and cannot effectively detect low concentrations of ammonia.

Method used

V2CTx@MoS2 composite material is used to synthesize V2CTx through molten salt synthesis method and molten salt etching method, V2CTx@MoS2 composite material is synthesized by in-situ polymerization method and hydrothermal method, and applied it to ammonia detection sensors, using MoS2 The high-meter-volume ratio structure and the multi-layer MXene structure of V2CTx form an n-n-type heterojunction to improve detection sensitivity.

Benefits of technology

High sensitivity detection for low-concentration ammonia is achieved, and the sensor has fast response recovery, good reproducibility and stability, with a detection limit of 0.129ppm, which significantly improves the gas-sensitive response value to ammonia.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118883644A_ABST
    Figure CN118883644A_ABST
Patent Text Reader

Abstract

According to the invention, a V2CTx-coated MoS2 nano composite material is prepared by combining a hydrothermal method with an in-situ polymerization method, and then the nano composite material is dispensed on a gold interdigital electrode to prepare the gas sensor. An ammonia sensitive test result shows that the V2CTx-coated MoS2 nano composite material has a relatively high gas sensitive response value to NH3 gas in a low concentration range at room temperature, and the nano composite material sensor keeps good sensing response capability and sensing stability and relatively low detection limit at room temperature. The V2CTx-coated MoS2 nano composite material provided by the invention can provide potential application prospects for ultra-sensitive and low-concentration detection of ammonia gas by a sensor taking the V2CTx-coated MoS2 nano composite material as a sensing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of preparation of gas sensing composite materials, and specifically relates to V2CT x @MoS2 composite material, preparation method and application thereof. Background Art

[0002] Ammonia (NH2) is a gas that is now ubiquitous in the atmosphere. Its main sources are direct deposition of nitrates and ammonium salts, bacterial nitrogen fixation and combustion, and the use of chemical industry and automobiles. However, NH3 is not only seriously harmful to the environment, causing pollution to water bodies, soil and atmosphere, but also endangering human health. Low concentrations of ammonia can quickly irritate the eyes and moist skin. Mild inhalation of ammonia poisoning manifests as rhinitis, pharyngitis, sore throat and hoarseness. Ammonia entering the trachea and bronchi can cause coughing and sputum. In severe cases, it can cause hemoptysis, pulmonary edema, and dyspnea. Inhalation of high concentrations of ammonia can directly affect the permeability of pulmonary capillaries and cause pulmonary edema, which can induce convulsions, convulsions, drowsiness and coma and other consciousness disorders. Therefore, it is very necessary to develop a high-performance ammonia sensor to detect NH2. At present, sensors used to detect ammonia (NH3) can be divided into optical sensors, surface acoustic wave sensors, electrochemical sensors, catalytic field effect sensors and chemical resistance sensors. In comparison, chemiresistor sensors convert the monitored changes in electrical properties into readable electrical signals. They have the advantages of fast response, high sensitivity, easy operation and economy, and a wide range of applications. Therefore, sensing materials have become an important part. As a new type of two-dimensional material, MXene not only has a high specific surface area and high conductivity similar to graphene, but also has outstanding advantages such as adjustable chemical composition, controllable minimum nanolayers, and modifiable surface functional groups. These advantages can make MXene materials exhibit excellent chemical reactivity. At room temperature, the MXene material - V2CTx shows certain gas-sensitive properties, and its ultra-high signal-to-noise ratio also gives it the potential to detect ultra-low concentrations of ammonia. However, gas sensors based on pure V2CTx are hindered by high noise and low response, and cannot achieve high-sensitivity detection of ammonia. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the above problems, the present invention provides V2CT x @MoS2 composite material and its preparation method and sensor preparation method and application, considering that, among various inorganic two-dimensional layered materials, the adjacent planes of MoS2 are held together by weak van der Waals interactions, and its high surface-to-volume ratio structural characteristics can provide ultra-high sensitivity for the detection of ammonia molecules. Therefore, V2CTx and MoS2 composite can achieve high-sensitivity detection of ammonia in a low concentration range.

[0005] (II) Technical solution

[0006] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0007] The present invention provides a V2CT x The preparation method of @MoS2 composite material comprises the following specific steps:

[0008] S1, using vanadium powder, aluminum powder, graphite powder and NaCl powder as raw materials, V2CTx was synthesized by molten salt synthesis method combined with molten salt etching method;

[0009] S2, using thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 24 ·4H2O was used as raw material to synthesize V2CTx@MoS2 composite materials by in-situ polymerization combined with hydrothermal method.

[0010] Furthermore, the step S1 includes:

[0011] S11, mixing vanadium powder, aluminum powder and graphite powder according to a molar ratio of 2:1.2:1, and adding the mixed materials and NaCl powder into a ball mill for thorough mixing to obtain a mixed powder;

[0012] S12, placing the mixed powder in a tube furnace for annealing to obtain an annealed sample;

[0013] S13, crushing the annealed sample and passing it through a molecular sieve to obtain V2AlC powder;

[0014] S14, immersing the V2AlC powder in HF etching solution, and after magnetic stirring, centrifuging the powder in the HF etching solution by a centrifuge, washing and drying, to obtain V2CT X powder.

[0015] Furthermore, the mass ratio of the ingredients to the NaCl powder is (0.4-1):1; the annealing temperature is 1000-1500°C, and the time is 2-8h; the pore size of the molecular sieve is 500 mesh; the temperature of the magnetic stirring is 80-120°C, and the time is 48-90h.

[0016] Furthermore, the V2CT X The powder is a multilayer MXene structure.

[0017] Furthermore, the step S2 comprises:

[0018] S21, thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 244H2O was prepared in a molar ratio of 3.5:1 and dissolved in deionized water. 30-60 mg of glucose was added and transferred to the lining of the reactor.

[0019] S22, adding the V2CTx powder into the inner lining of the reactor, and after magnetic stirring for 20 minutes, performing in-situ polymerization reaction and hydrothermal synthesis reaction;

[0020] S23, the reactor is naturally cooled to room temperature, the obtained product is centrifuged, washed and dried to obtain the V2CT X @MoS2 composite material.

[0021] Furthermore, the thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 24 The mass ratio of 4H2O to the V2CTx powder is (0.5-4):1; the temperature of the hydrothermal synthesis and in-situ polymerization is 150-220°C, and the time is 10-14h.

[0022] The present invention also provides a V2CT X @MoS2 composite material, the V2CT X @MoS2 composites include V2CT with multilayer MXene structures X and fill in the V2CT X The interlayer MoS2 nanoparticles and the V2CT X Combined with the MoS2 to form a nn-type heterojunction.

[0023] The present invention also provides a V2CT X @MoS2 composite material application, the V2CT X @MoS2 composite materials are used in the production of ammonia detection sensors.

[0024] Furthermore, the specific steps include: X @MoS2 composite material is dissolved in a solvent to obtain a V2CTX@MoS2 composite material solution; the V2CT X The V2CTx@MoS2 composite material solution is dripped onto the gold interdigital electrode and dried to obtain the V2CTx@MoS2 composite material sensor.

[0025] Furthermore, the solvent is water or an organic solvent; the V2CT X The concentration of the @MoS2 composite material solution is 5 mg / ml; the V2CTx@MoS2 composite material sensor is applied to ammonia detection.

[0026] (III) Beneficial effects

[0027] (1) V2CT provided by the present invention X @MoS2 composite sensor, due to V2CT X The synergistic effect with MoS2 results in higher sensitivity and faster response recovery for NH3 detection.

[0028] (2) V2CT provided by the present invention X @The preparation method of MoS2 composite material is simple, the yield is high, the product is easy to store, and has excellent stability.

[0029] (3) V2CT provided by the present invention X @The nn-type heterojunction of the MoS2 composite material acts as a signal amplifier and has a high gas-sensitive response value and a low detection limit for NH3 gas in a low concentration range at room temperature. The detection limit obtained according to the linear fitting curve is 0.129 ppm.

[0030] (4) V2CT provided by the present invention X @MoS2 composite material sensors showed good reproducibility and sensing stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 V2CT X @The synthesis process of MoS2 nanocomposite materials.

[0033] Figure 2 To synthesize V2CT by molten salt method combined with molten salt etching X XRD patterns of powders.

[0034] Figure 3 To synthesize V2CT by molten salt method combined with molten salt etching X SEM image of powder.

[0035] Figure 4 XRD patterns of V2C@MoS2 composite materials synthesized by in-situ polymerization combined with hydrothermal method with different masses of V2CTx added.

[0036] Figure 5 SEM and TEM images of V2C@MoS2-25 composite material, where (a) and (b) are SEM images, and (c) is a TEM image.

[0037] Figure 6 The response of the sensor prepared by V2C@MoS2 composite material synthesized by in-situ polymerization combined with hydrothermal method with the addition of different masses of V2CTx in the ammonia concentration range of 0.2 to 10 ppm.

[0038] Figure 7 V2CT at room temperature X @The resistance and response changes of the MoS2-25 sensor in the ammonia concentration range of 0.2 to 10 ppm, where (a) is the resistance change and (b) is the response change.

[0039] Figure 8 V2CT X @The standard curve between the ammonia response of the MoS2-25 sensor and the ammonia concentration.

[0040] Fig. 9 V2CT at room temperature x @Reproducibility test results of MoS2-25 sensor under different ammonia concentrations.

[0041] Fig.10 V2CT at room temperature x @MoS2-25 sensor stability test results under different ammonia concentrations.

[0042] Fig.11 V2CT x @Diagram of the ammonia gas sensing mechanism of MoS2 sensor. DETAILED DESCRIPTION

[0043] The reagents used in the present invention: vanadium powder (99.6wt%, 325 mesh) and aluminum powder (99.6wt%, 200 mesh) were purchased from Beijing Xingrongyuan Technology Co., Ltd., graphite powder (99wt%, 325 mesh) was purchased from Tianjin Proen Technology Co., Ltd., concentrated hydrochloric acid (36wt%) was purchased from Beijing Beihua Fine Chemicals Co., Ltd., sodium chloride (NaCl), sodium fluoride (NaF), anhydrous ethanol, thiourea (CH4N2S), ammonium molybdate tetrahydrate ({(NH4)6Mo7O 24 ·4H2O}) and glucose were purchased from Sinopharm Chemical Reagent Co., Ltd. All other chemicals and reagents were analytical reagents (AR) unless otherwise stated.

[0044] In order to better explain the present invention and facilitate understanding, the technical solution of the present invention is described in detail below through specific implementation methods in conjunction with the accompanying drawings.

[0045] The present invention adopts a molten salt method to synthesize V2AlC, and then etches V2AlC with an HF etching solution prepared by sodium fluoride and hydrochloric acid to obtain a V2CTx powder with a multilayer structure, which is then added to a solution with thiourea and ammonium molybdate tetrahydrate as raw materials to react to obtain a V2CTx@MoS2 composite material. The synthesis process is as follows: Figure 1 shown.

[0046] Example 1: Preparation of V2CTx

[0047] In this example, V2AlC powder was synthesized by molten salt method, and V2CT was synthesized by molten salt etching method. x powder.

[0048] (1) Vanadium powder (99.6 wt%), aluminum powder (99.6 wt%) and graphite powder (99 wt%) were weighed and mixed at a molar ratio of V:Al:C=2:1.2:1. The mixed powder was recorded as A. 500 mg of mixed powder A was taken, and then 500 mg of NaCl powder was weighed at a mass ratio of A:NaCl=1:1. The mixed powder A and NaCl powder were fully mixed in a ball mill for 12 h, placed in a tubular furnace, and annealed at 1500°C for 4 h. The annealed sample was crushed and passed through a molecular sieve (500 mesh) to obtain sample powder 1.

[0049] (2) 1 g of NaF was mixed with 20 ml of HCl (1 M) and 20 ml of deionized water in an ultrasonic bath for 15 min to obtain an HF etching solution. 1.46 g of sample powder 1 was immersed in the etching solution and magnetically stirred at 90°C for 72 h. The powder was separated from the etching solution by centrifugation and then washed alternately with deionized water and anhydrous ethanol for 4 times to remove possible residual ions and precursors. The powder was vacuum dried at 60°C for 12 h to obtain sample powder 2.

[0050] The sample powder 2 was characterized by XRD test, and the results are as follows Figure 2 As shown in the figure, the diffraction peaks at 2θ=7.3°, 14.5°, 18.2°, 35.5°, 41.2° and 50.1° correspond to the (002), (004), (100), (008), (111) and (211) planes of V2CTx, respectively, indicating that V2CTx was successfully synthesized by the molten salt method combined with the molten salt etching method. x Powder, and form a hexagonal crystal structure. x The powder was characterized by SEM test and the results are shown in Figure 3 As shown in the figure, V2CT xIt has a typical layered structure with a thickness of about 200 nm. The obvious gaps between the nanosheets indicate that the Al layer is completely etched, which is consistent with the XRD test results. This shows that the present invention has successfully synthesized nanosheet-shaped V2CT x .

[0051] Example 2: Preparation of V2C@MoS2 composite material

[0052] In this example, thiourea and ammonium molybdate tetrahydrate are used as raw materials, and different masses of V2CTx powder are added. An in-situ polymerization method combined with a hydrothermal method is adopted to synthesize a V2C@MoS2 composite material, and the effect of adding different masses of V2CTx on the response sensitivity of the synthesized V2CTx@MoS2 composite material to ammonia is analyzed.

[0053] (1) Weigh 48 mg of thiourea (CH4N2S) and 56 mg of ammonium molybdate tetrahydrate {(NH4)6Mo7O 24 ·H2O} was dissolved in 30 ml of deionized water, 50 mg of glucose was added and mixed, the above steps were repeated 4 times, and five identical solutions were transferred to five identical 50 ml reactor liners, and then 100 mg, 66.7 mg, 50 mg, 25 mg and 12.5 mg of the V2CTx powder synthesized in Example 1 were added to the five reactor liners, respectively, and magnetic stirring was carried out for 20 min.

[0054] (2) After the five reactors were reacted at 200°C for 12 h, they were naturally cooled to room temperature. The obtained products were centrifuged at 11000 rpm for 10 min, washed alternately with deionized water and anhydrous ethanol for 4 times, and black precipitates were obtained. They were vacuum dried at 60°C for 12 h to obtain the reaction products. 100 mg, 66.7 mg, 50 mg, 25 mg and 12.5 mg of V2CTx powder were added to obtain the products, which were labeled as V2CTx@MoS2-100, V2CTx@MoS2-66.7, V2CTx@MoS2-50, V2CTx@MoS2-25 and V2CTx@MoS2-12.5, respectively.

[0055] The products obtained above were characterized by XRD test, and the results are as follows Figure 4As shown in the figure, it can be seen that the diffraction peaks at 2θ=7.3°, 14.5°, 18.2°, 35.5°, 41.2° and 50.1° correspond to the (002), (004), (100), (008), (111) and (211) planes of V2CTx, respectively; the three characteristic diffraction peaks at 2θ=7.5°, 33.1° and 58.3° correspond to the (002), (100) and (110) planes of MoS2, respectively. From these obvious characteristic peaks, it can be seen that the composite materials obtained by the above preparation method contain V2CTx and MoS2, indicating that first, MoS2 is synthesized by in-situ polymerization of thiourea and ammonium molybdate tetrahydrate, and then V2CTx@MoS2 composite materials are hydrothermally synthesized with different masses of V2CTx powder. However, as the mass of V2CTx increases, the (002) diffraction peak of V2CTx at 2θ=7.3° gradually disappears, indicating that the interlayer spacing of V2CTx increases with the increase of V2CTx mass. When V2CTx is 25 mg (V2CTx@MoS2-25), the XRD image can clearly show all the obvious characteristic peaks of molybdenum disulfide and V2CTx, and the (002) diffraction peak of molybdenum disulfide and the (002) diffraction peak of V2CTx MXene are relatively strong, indicating that when V2CTx is 25 mg, the purity of V2CTx@MoS2-2 composite material is high. All the diffraction peaks in the XRD spectrum are very sharp, indicating that the prepared product has good crystallinity.

[0056] SEM and TEM characterization of V2CTx@MoS2-25 were performed, and the results are as follows Figure 5 As shown in the figure, it can be seen from the scanning electron microscope images of Figure a and Figure b that MoS2 nanosheets with typical nanoflower-like structures grow on the surface of the V2CTx substrate, and from the transmission electron microscope image of Figure c, it can be found that MoS2 is evenly distributed on V2CTx. The scanning electron microscope and transmission electron microscope images show that MoS2 nanoparticles grow on the surface of the V2CTx MXene nanosheet layer to form a nanohybrid V2CTx@MoS2 composite material.

[0057] Example 3: Preparation of V2C@MoS2 composite sensor

[0058] Weigh 5 mg of the V2CTx@MoS2 composite material obtained in step (2) and dissolve it in 1 ml of deionized water. Use a pipette to drop 20 μμl of the V2CTx@MoS2 composite solution onto the gold interdigital electrode and dry it in a drying oven at 60°C for 6 h to prepare a V2CTx@MoS2 composite sensor.

[0059] The products obtained by adding different masses of V2CTx were subjected to ammonia sensitivity test on the composite materials by CGSMT gas-sensitive material analysis and testing system, and the resistance change of the composite materials under different concentrations of ammonia and in the air was used to characterize its response to ammonia. The gas response (sensor sensitivity) was calculated by the following formula:

[0060] Response(%)=(Ra-Rg) / Rg×100%

[0061] Where Response represents the gas response, Ra and Rg represent the resistance of the sensor measured in dry air and target gas, respectively. The response time is defined as the time required for the sensor to reach 90% of the maximum response when exposed to the target gas. The recovery time is defined as the time required for the sensor's response to recover to 10% of the minimum response after the device is exposed to dry air. The test results are as follows Figure 6 As shown in the figure, it can be seen that from the horizontal point of view, under the exposure of 0.2-10ppm ammonia, the response values ​​of all sensors to ammonia increase with the increase of ammonia concentration, indicating that the above five groups of reaction products have a certain response to ammonia. However, from the vertical point of view, for the same ammonia concentration, the response of the sensor to ammonia first increases and then decreases, reaching the maximum (1ppm@9.39%) when the mass of V2CTx is 25mg. However, V2CTx@MoS2-25 has the best sensitivity response to ammonia detection. The possible reason is that the nn-type heterojunction formed between V2CTx and MoS2 at this mass ratio is high, which enhances the response of the composite material to ammonia, and this result is consistent with the above XRD results. The low response of V2CTx@MoS2-100 and V2CTx@MoS2-66.7 to ammonia may be due to the high content of V2CTx and the failure of MoS2 to grow uniformly on its surface. The low response of V2CTx@MoS2-50 to ammonia can be attributed to the fact that V2CTx and MoS2 are not well compounded. It can also be seen from its XRD spectrum that the diffraction peaks of V2CTx and MoS2 are not very obvious. The low response of V2CTx@MoS2-12.5 to ammonia is mainly due to the excess of MoS2, the low content of V2CTx, and the low response of MoS2 to ammonia.

[0062] Test Example 1:

[0063] Drawing of standard curve: The sensor made of composite material V2CTx@MoS2-25 was tested for multiple responses in NH3 concentration range of 0.2-10ppm. The test results are shown in Figure 7As shown, the error bars represent the relative standard deviation of five independent measurements. It can be seen that the response and ammonia concentration show the best linear relationship. The linear regression equation is Y = 8.76676 + 0.60985 * X, R2 = 0.99589, and the detection limit is 0.129ppm. The fitting curve shows that the response value (Y) and ammonia concentration (I) of both have a good linear relationship. It can also be found that the V2CTx@MoS2-25 composite sensor has a higher linear fitting coefficient and better sensitivity.

[0064] Test Example 2:

[0065] Reproducibility test: The sensor made of composite material V2CTx@MoS2-25 was tested for repeatability of 1, 5, and 8 ppm ammonia response at room temperature. The test results are as follows: Figure 8 As shown, after three cycles of switching between air and ammonia, the response of the sensor can be restored to the initial state, which indicates that the composite sensor has good repeatability and fast response recovery to ammonia.

[0066] Test Example 3

[0067] Stability test: Within two months, the sensor made of the composite material V2CTx@MoS2-25 was tested for ammonia response at ammonia concentrations of 1ppm, 3ppm and 5ppm. The test results are as follows: Fig. 9 As shown in Figure 2, the ammonia response of the sensor changed little within two months, which indicates that the sensor has good stability in response to ammonia. Fig.10 shown.

[0068] Mechanism analysis: The sensor made of V2CTx@MoS2 composite material can cause changes in the width of the depletion layer through the interaction between the oxygen adsorbed on the surface and ammonia, which can lead to changes in resistance, thereby affecting its response to ammonia. Specifically, when the sensor is exposed to ammonia, the captured electrons are released back to the conduction band of the V2CTx@MoS2 sensitive material, thereby reducing the width of the depletion layer and the resistance of the sensor. The resistance of the sensor changes exponentially with the barrier height of the heterojunction. In addition, Fig.11 The synergistic effect of V2CTxMXene and MoS2 binary nanomaterials is shown. The V2CTxMXene multilayer stacked nanolayer structure has the advantage of a large specific surface area, which can increase its contact sites with MoS2, provide a large number of adsorption sites for the reaction and adsorption of ammonia, and effectively improve the composite material's response to ammonia.

[0069] According to the experimental results, V2CTx and MoS2 showed n-type conduction to ammonia, respectively. After forming the composite material, they formed a nn-type heterojunction. When the heterojunction is formed, the difference in work function leads to the transfer of electrons until the Fermi level in the two materials reaches equilibrium. This process leads to the formation of a depletion layer at the interface between the two different n-type materials. When the sensor based on the V2CTx@MoS2 composite material is exposed to the air, oxygen molecules can be converted into chemically adsorbed oxygen ions (O2-) by capturing electrons on the surface of the sensitive material. As mentioned above, during this process, an electron depletion layer is formed on the surface of the V2CTx@MoS2 sensitive material, resulting in a high resistance of the sensitive material. The above process can be expressed by the following formula:

[0070] O2(gas)→O2(ads) (1)

[0071] O2(ads)+e-→O2 - (ads) (2)

[0072] In summary, the present invention synthesized a V2CTx@MoS2 nanocomposite material by combining an in-situ polymerization method with a hydrothermal method, and then the nanocomposite material was drop-coated on a gold interdigital electrode to make a gas sensor. The ammonia-sensitive test results show that the V2CTx@MoS2 composite material has a certain gas-sensitive response value to NH3 gas in a low concentration range at room temperature, especially the V2CTx@MoS2-25 composite material has a higher gas-sensitive response value. The nanocomposite sensor maintains good sensing response capability, sensing stability and a lower detection limit at room temperature. Therefore, it is shown that the sensor using the V2CTx@MoS2 nanocomposite material synthesized by the present invention as a sensing material can provide potential application prospects for ultra-sensitive, low-concentration detection of ammonia.

[0073] It should be noted that the above embodiments can be freely combined as needed. The above description is only the preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A V2CT X The preparation method of @MoS2 composite material is characterized in that: include: S1, using vanadium powder, aluminum powder, graphite powder and NaCl powder as raw materials, V2CTx was synthesized by molten salt synthesis method combined with molten salt etching method; S2, using thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 24 ·4H2O was used as raw material to synthesize V2CTx@MoS2 composite materials by in-situ polymerization combined with hydrothermal method.

2. The V2CT according to claim 1 X The preparation method of @MoS2 composite material is characterized in that: The S1 step comprises: S11, mixing vanadium powder, aluminum powder and graphite powder according to a molar ratio of 2:1.2:1, and adding the mixed ingredients and NaCl powder into a ball mill for thorough mixing to obtain a mixed powder; S12, placing the mixed powder in a tube furnace for annealing to obtain an annealed sample; S13, crushing the annealed sample and passing it through a molecular sieve to obtain V2AlC powder; S14, immersing the V2AlC powder in HF etching solution, and after magnetic stirring, centrifuging the powder in the HF etching solution by a centrifuge, washing and drying, to obtain V2CT X powder.

3. The V2CT according to claim 2 X The preparation method of @MoS2 composite material is characterized in that: The mass ratio of the ingredients to the NaCl powder is (0.4-1):1; the annealing temperature is 1000-1500°C, and the time is 2-8h; the pore size of the molecular sieve is 500 mesh; the temperature of the magnetic stirring is 80-120°C, and the time is 48-90h.

4. The V2CT according to claim 2 X The preparation method of @MoS2 composite material is characterized in that: The V2CT X The powder is a multilayer MXene structure.

5. The V2CT according to claim 1 X The preparation method of @MoS2 composite material is characterized in that: The step S2 comprises: S21, thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 24 4H2O was prepared in a molar ratio of 3.5:1 and dissolved in deionized water. 30-60 mg of glucose was added and transferred to the lining of the reactor. S22, adding the V2CTx powder into the inner lining of the reactor, and after magnetic stirring for 20 minutes, performing in-situ polymerization reaction and hydrothermal synthesis reaction; S23, the reactor is naturally cooled to room temperature, the obtained product is centrifuged, washed and dried to obtain the V2CT X @MoS2 composite material.

6. The V2CT according to claim 5 X The preparation method of @MoS2 composite material is characterized in that: The thiourea CH4N2S and ammonium molybdate tetrahydrate (NH4)6Mo7O 24 The mass ratio of 4H2O to the V2CTx powder is (0.5-4):1; the temperature of the hydrothermal synthesis and in-situ polymerization is 150-220°C, and the time is 10-14h.

7. A V2CT X @MoS2 composite material, characterized in that Prepared by the preparation method according to any one of claims 1 to 6; the V2CT X @MoS2 composites include V2CT with multilayer MXene structures X and fill in the V2CT X The interlayer MoS2 nanoparticles and the V2CT X Combined with the MoS2 to form a nn-type heterojunction.

8. A V2CT as claimed in claim 7 X The application of MoS2 composite material is characterized by: The V2CT X @MoS2 composite materials are used in the production of ammonia detection sensors.

9. V2CT according to claim 8 X The application of MoS2 composite material is characterized by: include: The V2CT X @MoS2 composite material is dissolved in a solvent to obtain a V2CTX@MoS2 composite material solution; the V2CT X The V2CTx@MoS2 composite material solution is dripped onto the gold interdigital electrode and dried to obtain the V2CTx@MoS2 composite material sensor.

10. The V2CT according to claim 8 X The application of MoS2 composite material is characterized by: The solvent is water or an organic solvent; the V2CT X The concentration of the @MoS2 composite material solution is 5 mg / ml; the V2CTx@MoS2 composite material sensor is applied to ammonia detection.

Citation Information

Cited By

  • EMC gas component prediction method based on V2C / V2O5 / SnO2 sensor and GRU-Attention