Nano Cu-coated C-OH-PAM composite material and nano Cu-coated C / carrier complex for removing algae, and preparation method and application of nano Cu-coated C-OH-PAM composite material and nano Cu-coated C / carrier complex
By preparing nano Cu@C-OH-PAM composite material and nano Cu@C/carrier composite, the problem of filamentous green algae reproduction in water bodies is solved, and efficient and low-cost algae removal is achieved, and the material stability is high. Meet environmental protection requirements.
Patent Information
- Application Number
- CN202411064971.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art methods for suppressing filamentous green algae in water bodies have problems of low efficiency, high cost and secondary pollution. Traditional physical, chemical and biological treatment methods are difficult to effectively solve the problem of algae reproduction in eutrophied water bodies.
NanoCu@C-OH-PAM composite and nanoCu@C/carrier composite were used to prepare nanoCu@C composite and nanoCu@C/carrier composite by activating nanoCu@C composite and dispersing them in polyacrylamide solution to optimize loading conditions , form high stability and efficient algae removal materials.
It has achieved efficient removal of filamentous green algae in water, the material has good dispersion and stability, significantly improved the removal effect, met the green environmental protection requirements, and reduced the material cost.
Smart Images

Figure CN118975553A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material preparation, and in particular to a nano Cu@C-OH-PAM composite material and a nano Cu@C / carrier complex for algae removal, a preparation method and application thereof. Background Art
[0002] Algae, especially filamentous green algae, multiply in eutrophic waters, which not only reduces the transparency of the water, but also causes the depletion of dissolved oxygen in the water, leading to the death of fish and other aquatic organisms. In addition, the outbreak of filamentous green algae will also produce a foul odor, which has a serious impact on the ornamental value and ecological function of the water.
[0003] At present, the methods for inhibiting filamentous green algae in water bodies mainly include physical, chemical and biological methods. Physical methods such as mechanical salvage and shading treatment can reduce the number of algae in the short term, but they are costly and only treat the symptoms. Chemical methods such as the use of algae inhibitors, although they are quick to take effect, are prone to secondary pollution and have potential negative impacts on aquatic ecosystems. Biological methods such as the introduction of algae-eating organisms, although more environmentally friendly, have unstable control effects and require long-term monitoring and management. Although these methods are effective to a certain extent, there are still problems such as high energy consumption, high cost, complex maintenance and potential secondary pollution, and further improvement and exploration of new treatment methods are urgently needed.
[0004] Chinese patent CN 117417043 A discloses a biodegradable algaecide and its preparation method and application. First, a flocculant material with a positive charge density is synthesized, and flocs are formed between algae particles by electrostatic neutralization and sedimentation. Unmanned equipment is used as a carrier to realize intelligent and precise application scenarios to solve practical application problems. The problem that traditional flocculants are difficult to degrade and easily cause secondary pollution in the process of water ecological restoration is solved. The proposed intelligent coagulation system avoids the insufficient coagulation caused by simple artificial spraying of flocculants on the surface of the water body, as well as the high labor cost and low intelligence of human ship operation, and realizes the full mixing of flocculants, thereby improving the coagulation and algae removal effect. However, there are problems such as complex synthesis process, high material cost, and complex maintenance.
[0005] Chinese patent CN 117772282A discloses a floating aerogel algaecide catalyst, a preparation method and a floating algaecide. The floating algaecide catalyst uses guar gum as a carrier matrix and is loaded with a single metal atom; the single metal atom includes one of a copper atom, an iron atom, a cobalt atom and a manganese atom. The single metal atom can catalyze the decomposition of persulfate in the floating algaecide to form a large number of active oxygen free radicals, which then attack the surface morphology and internal tissue structure of algae cells, resulting in the destruction of cell integrity and a significant decrease in cell activity, thereby achieving an algaecide effect. At the same time, the single metal atom can form a cross-linked network structure with guar gum through a coupling reaction to form an aerogel, so that the algaecide can stably float on the water surface, can efficiently remove algae and is conducive to later recycling and reuse. However, in practical applications, there are still potential problems such as the side effects of active oxygen free radicals and the degradation of guar gum.
[0006] Chinese patent CN 117502450 A discloses a method for preparing a slow-release algaecide and its application. The method is characterized in that a non-oxidant and an allelopathic agent are dissolved in an organic solvent, a natural substance is used as a carrier, and the agent is placed in an organic solution. After 24-72 hours, the adsorbed and loaded carrier is ventilated and dried or dried to obtain a slow-release algaecide. The slow-release algaecide prepared by the invention can remove algae in situ, solving the problems of high cost, short efficacy, low efficiency, transportation trouble, high environmental toxicity, and complicated use methods for eutrophic water treatment. In addition, the product prepared by the present invention has a variety of uses, can be directly sprinkled in water, can also be suspended in the light-transmitting layer of water or the position of algae, semi-floating on the water surface to remove surface algae, and is suitable for any water body and any position of the water body. However, there are problems such as large demand for raw materials and difficulty in obtaining them.
[0007] In summary, traditional physical, chemical and biological treatment methods have the problems of low efficiency, high cost and secondary pollution in removing algae. Copper reagents are the most commonly used agents for emergency treatment of algal blooms. Copper is one of the essential trace elements for organisms. Therefore, compared with other algaecides, the water environment and aquatic organisms are more tolerant of copper. With the development of nanotechnology, the application of nano-copper materials in the field of water environment has become increasingly widespread. Summary of the invention
[0008] In view of the above problems, the present invention provides a nano Cu@C-OH-PAM composite material and a nano Cu@C / carrier composite for algae removal. The nano Cu@C / carrier composite is prepared by activating a nano Cu@C composite material (CCCSNs) and dispersing it in a polyacrylamide solution, and the loading conditions are optimized to obtain the nano Cu@C / carrier composite. The nano Cu@C / carrier composite is green and environmentally friendly, can be used for the treatment of filamentous green algae in water bodies, and has high stability.
[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0010] On the one hand, the present invention provides a nano Cu@C-OH-PAM composite material, which is prepared by the following preparation method: nano Cu@C with a core-shell structure is activated to obtain nano Cu@C-OH, which is dispersed in a polyacrylamide solution to obtain a nano Cu@C-OH-PAM composite material; the particle size of the nano Cu@C-OH is 100-200nm.
[0011] Preferably, the particle size of the nano Cu@C is 45-65 nm, and more preferably, the particle size of the nano Cu@C is 50-60 nm.
[0012] Preferably, the nano Cu@C is CCCANs.
[0013] Preferably, the activating agents used in the activation are NaOH and H2O2.
[0014] Preferably, the preparation method comprises the following steps:
[0015] a: Activation: Mix nano Cu@C with a concentration of 100-130 mg / mL with NaOH solution and H2O2 solution, and stir for 50-70 min to obtain nano Cu@C-OH;
[0016] b: Dispersion: Nano Cu@C-OH was mixed with 0.03-0.08% polyacrylamide solution for 50-70 min and ultrasonicated for 1.5-3 h to obtain nano Cu@C-OH-PAM composite material.
[0017] Preferably, in step a, the concentration is 100-120 mg / mL; further preferably, in step a, the concentration is 100 mg / mL, 120 mg / mL.
[0018] Preferably, in step a, the mass fraction of the NaOH solution is 3-8%; further preferably, in step a, the mass fraction of the NaOH solution is 4-6%; more preferably, in step a, the mass fraction of the NaOH solution is 5%.
[0019] Preferably, in step a, the mass fraction of the H2O2 solution is 3-8%; preferably, in step a, the mass fraction of the H2O2 solution is 4-6%; further preferably, in step a, the mass fraction of the H2O2 solution is 5%.
[0020] Preferably, in step a, the NaOH solution is a NaOH aqueous solution;
[0021] Preferably, in step a, the H2O2 solution is a H2O2 aqueous solution;
[0022] Preferably, in step a, the mixing is ultrasonic, and the ultrasonic time is 20-40 min; more preferably, the ultrasonic time is 30 min.
[0023] Preferably, in step a, the stirring temperature is 45-50°C, and the rotation speed is 1900-2000r / min; further preferably, in step a, the stirring temperature is 50°C, and the rotation speed is 2000r / min.
[0024] Preferably, step a further comprises washing and drying steps;
[0025] The solvent used for washing is at least one of deionized water, purified water and distilled water; more preferably, the solvent used for washing is deionized water.
[0026] Preferably, the purpose of the washing is to wash away excess NaOH solution and stabilize the pH of the nano-Cu@C-OH.
[0027] Preferably, the drying temperature is 40-60°C and the drying time is 1.5-3h; more preferably, the drying temperature is 40-50°C and the drying time is 1.5-2h.
[0028] Preferably, in step b, the mass fraction of the polyacrylamide solution is 0.04-0.06%; further preferably, in step b, the mass fraction of the polyacrylamide solution is 0.05%.
[0029] Preferably, in step b, the mixing temperature is 45-55°C, and the rotation speed is 1800-2200 r / min; further preferably, in step b, the mixing temperature is 45-50°C, and the rotation speed is 1800-2000 r / min.
[0030] Preferably, in step b, the mixing is stirring;
[0031] Preferably, in step b, the temperature of the ultrasound is 45-55°C. Further preferably, in step b, the temperature of the ultrasound is 45-50°C.
[0032] On the other hand, the present invention provides the use of the nano Cu@C-OH-PAM composite material described above in the preparation of a nano Cu@C / carrier complex for algae removal.
[0033] On the one hand, the present invention provides a nano Cu@C / carrier complex for algae removal, comprising a nano Cu@C-OH-PAM composite material and a carrier; the carrier is selected from at least one of polyester fiber Acoman, polyurethane sponge, and polypropylene non-woven fabric.
[0034] Preferably, the carrier is polyester fiber acoman, polyurethane sponge or polypropylene non-woven fabric.
[0035] In another aspect, the present invention provides a method for preparing a nano Cu@C / carrier complex for algae removal, comprising the following steps:
[0036] S1: Carrier treatment: the carrier is mixed with a solvent and the pH is adjusted to 6.5-7.5 to obtain a pretreated carrier;
[0037] S2: Preparation of nano Cu@C-OH-PAM composites;
[0038] S3: Chemical coupling: premix the pretreated carrier with the solution of the coupling agent, then put it into 40-60 mg / L of the nano-Cu@C-OH-PAM composite material and mix for 3-5 hours to obtain a nano-Cu@C / carrier complex.
[0039] Preferably, in S1, the solvent is acetone.
[0040] Preferably, in S1, the carrier is cut into square pieces of 4-6 cm*4-6 cm or cubic pieces of 0.8-1.2 cm*0.8-1.2 cm*0.8-1.2 cm.
[0041] Preferably, in S3, the coupling agent is selected from at least one of KH560, CS171, and KH570; further preferably, in S3, the coupling agent is selected from KH560, CS171, or KH570.
[0042] Preferably, in S3, the premixing is performed to ensure that the carrier is always immersed in the coupling agent solution; and the premixing time is 20-50 minutes.
[0043] Preferably, in S3, the mixing is performed to ensure that the carrier is always immersed in the nano-Cu@C-OH-PAM suspension.
[0044] Preferably, in S3, the mixing time is 20-40 min;
[0045] Preferably, in S3, the mixing temperature is 45-55°C, and the rotation speed is 1800-2200 r / min; further preferably, in S3, the mixing temperature is 45-50°C, and the rotation speed is 1800-2000 r / min.
[0046] Preferably, S3 further comprises a drying step;
[0047] The drying temperature is 45-55°C and the time is 3-5h; more preferably, the drying temperature is 45-50°C and the time is 3-4h.
[0048] In another aspect, the present invention also provides the use of the nano Cu@C / carrier complex for algae removal in the preparation of a material for inhibiting or removing filamentous green algae in water.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] 1. Optimization of preparation conditions: The present invention optimizes parameters such as the concentration of different CCCSNs suspensions and the type of coupling agents by systematically screening reagents and preparation conditions, thereby ensuring the high stability and high algaecidal performance of the material.
[0051] 2. Green and environmentally friendly: The preparation method adopted by the present invention does not use toxic and harmful chemical reagents, meets the requirements of green chemistry, and is environmentally friendly.
[0052] 3. Highly efficient algaecide: The material combines the algaecidal properties of copper and the adsorption capacity of carbon, significantly improving the removal effect of filamentous green algae in water bodies.
[0053] 4. High stability: By optimizing the preparation conditions, the composite material obtained by the present invention has good dispersibility and stability in water, is not easy to aggregate and settle, and ensures a long-lasting algaecidal effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 XRD pattern of the nano Cu@C-OH-PAM material prepared in Example 1;
[0055] Figure 2 The SEM images of the nano Cu@C / carrier complex prepared in Example 1; wherein a1-a2 are nano Cu@C / PETAQU complexes, b1-b2 are nano Cu@C / PUSNG complexes, and c1-c2 are nano Cu@C / PPNWF complexes; wherein the test conditions are:
[0056] a1-c2 accelerating voltage (EHT) is 3.00KV; detector is SE2;
[0057] a1: Magnification (Mag) is 500 times; working distance (WD) is 3.4mm;
[0058] a2: Magnification (Mag) is 2000 times; working distance (WD) is 3.4mm;
[0059] b1: Magnification (Mag) is 1000 times; working distance (WD) is 8.1mm;
[0060] b2: Magnification (Mag) is 2000 times; working distance (WD) is 8.1mm;
[0061] c1: magnification (Mag) is 500 times; working distance (WD) is 6.4mm;
[0062] c2: Magnification (Mag) is 2000 times; working distance (WD) is 6.4mm;
[0063] Figure 3 The loading capacity and loading stability diagram of nano-Cu@C / PETAQUA complex at different nano-material suspension concentrations;
[0064] Figure 4 The loading capacity and loading stability diagram of nano-Cu@C / PUSNG composite at different nano-material suspension concentrations;
[0065] Figure 5 The loading capacity and loading stability diagram of nano-Cu@C / PPNWF composite at different nano-material suspension concentrations;
[0066] Figure 6 is the loading density of nano-Cu@C / PETAQUA complex at different nanomaterial suspension concentrations;
[0067] Figure 7 is the loading density of nano-Cu@C / PUSNG composite at different nano-material suspension concentrations;
[0068] Figure 8 is the loading density of nano-Cu@C / PPNWF composite at different nano-material suspension concentrations;
[0069] Fig. 9 is the loading amount of nano-Cu@C / PETAQUA complex under different coupling agent types;
[0070] Fig.10 is the loading amount of nano-Cu@C / PUSNG complex under different coupling agent types;
[0071] Fig.11 is the loading amount of nano-Cu@C / PPNWF complex under different coupling agent types;
[0072] Fig.12 is the loading density of nano-Cu@C / PETAQUA complex under different coupling agent types;
[0073] Fig.13 is the loading density of nano-Cu@C / PUSNG complex under different coupling agent types;
[0074] Fig.14 is the loading density of nano-Cu@C / PPNWF complex under different coupling agent types. DETAILED DESCRIPTION
[0075] In order to make the technical means, creative features, purpose and effect of the present invention easy to understand, the present invention is further explained below in conjunction with specific embodiments, but the following embodiments are only preferred embodiments of the present invention, not all. Based on the embodiments in the implementation mode, other embodiments obtained by those skilled in the art without making creative work all belong to the protection scope of the present invention. It is worth noting that the raw materials used in the present invention are all common commercial products, and their sources are not specifically limited. The technology and scientific terms used in the embodiments have the meanings commonly understood by those of ordinary skill in the art to which the present invention belongs.
[0076] Example 1
[0077] S1: Cut polyester fiber Acoman (PETAQUA), polyurethane sponge (PUSNG) and polypropylene nonwoven fabric (PPNWF) into 5cm*5cm square pieces, 1cm*1cm*1cm cubic pieces and 5cm*5cm square pieces respectively. Place the cut pieces in acetone until they are completely immersed, and then treat them in an ultrasonic cleaner for 30 minutes. After that, adjust the pH value of the rinse solution to neutral. Finally, dry the pieces in an oven at 80℃ for 3h.
[0078] S2. Activation of nanoparticles: In order to improve the surface activity of nanomaterials, NaOH and H2O2 were used to introduce surface hydroxyl groups. An appropriate amount of 100 mg / L of nano Cu@C composite material (CCCSNs) was placed in a beaker containing 5% NaOH aqueous solution and 5% H2O2 aqueous solution, and ultrasonically treated for 30 minutes at room temperature to form a uniform suspension. Then, the suspension was placed in a constant temperature magnetic stirrer and stirred for 60 minutes at 50°C and 2000r / min. After taking it out, it was washed with deionized water until the pH value of the washing liquid was stable. Finally, the washed nanomaterial was placed in an oven at 50°C and dried for 2 hours to obtain an activated nano Cu@C composite material (nano Cu@C-OH).
[0079] S3, dispersion: Take an appropriate amount of nano Cu@C-OH and put it into a beaker containing 0.05% polyacrylamide (PAM) solution, and stir it with constant temperature magnetic stirring at 50°C and 2000r / min for 30min until a uniform suspension is obtained. Then, place the beaker in an ultrasonic instrument and ultrasonically treat it at 50°C for 2h to consolidate the dispersion effect of the suspension. Finally, a uniformly dispersed and stable suspension (nano Cu@C-OH-PAM composite material) is obtained.
[0080] S4: Chemical coupling: The cleaned and dried PETAQUA pieces, PUSNG pieces and PPNWF pieces are placed in a coupling agent solution (KH560) with a volume ratio of 1.0%, and slowly stirred for 30 minutes to ensure that the carrier is always immersed in the coupling agent solution during the stirring process. After the stirring is completed, the carrier is removed and the excess coupling agent solution is absorbed with absorbent paper. Then, these carriers are placed in a 50mg / L nano Cu@C-OH-PAM composite material and stirred at a constant temperature of 50°C and 2000r / min for 4h to ensure that the carrier is always immersed in the suspension. After the stirring is completed, the carrier is removed and placed in an oven at 50°C for 4h to dry, and the corresponding nano Cu@C / carrier complex can be obtained. Depending on the carrier, they are nano Cu@C / PETAQUA complex, nano Cu@C / PUSNG complex, and nano Cu@C / PPNWF complex.
[0081] Example 2
[0082] Compared with Example 1, only the coupling agent was replaced by CS171 from KH560, and the rest of the operations were the same as those in Example 1.
[0083] Example 3
[0084] Compared with Example 1, only the coupling agent was replaced by KH570 from KH560, and the rest of the operations were the same as those in Example 1.
[0085] Example 4
[0086] Compared with Example 1, only the concentration of the Cu@C nanocomposite material (CCCSNs) was replaced from 100 mg / L to 120 mg / L, and the remaining operations were the same as those in Example 1.
[0087] Comparative Example 1
[0088] Compared with Example 1, only the concentration of Cu@C composite material (CCCSNs) was changed to 40 mg / L, 60 mg / L, and 80 mg / L, and the rest of the operations were the same as in Example 1.
[0089] Comparative Example 2
[0090] Compared with Example 1, only the types of coupling agent solutions were changed to KH550, CS201, CS401, MMA and physical etching, and the other operations were the same as those in Example 1.
[0091] Test Example 1
[0092] 1. X-ray diffraction (XRD) phase analysis was performed on the nano Cu@C-OH-PAM material prepared in Example 1. The results are as follows: Figure 1 And as shown in Table 1.
[0093] Table 1. XRD peak interplanar spacing of nano Cu@C-OH-PAM composites
[0094]
[0095] Figure 1 Table 1 and Table 1 present the X-ray diffraction (XRD) phase analysis results of the nano Cu@C-OH-PAM composite material. In the XRD spectrum, the nanoparticles dispersed by PAM present the strongest diffraction peak at 2θ=43.297°, which is determined to be the Cu(111) crystal plane; at the same time, the second strongest diffraction peaks can be observed at 2θ=50.433° and 2θ=36.025°, corresponding to the Cu(200) crystal plane and the C(401) crystal plane, respectively. In addition, the spectrum also shows a bun-shaped diffraction peak near 2θ=21.004°, which is confirmed to be the amorphous carbon (202) crystal plane, and a diffraction peak of sp2 carbon crystal (001) at 2θ=26.522°. No other crystalline substances have been found so far. The distribution of these interplanar spacings is consistent with the carbon shell copper core structure of the nanoparticles, indicating that the dispersion process has little effect on the phase and structure of the particles.
[0096] 2. The nano Cu@C / PETAQUA composite, nano Cu@C / PUSNG composite, and nano Cu@C / PPNWF composite prepared in Example 1 were characterized by scanning electron microscopy (SEM). Figure 2 As shown, a1-a2 are nano-Cu@C / PETAQU composites, b1-b2 are nano-Cu@C / PUSNG composites, and c1-c2 are nano-Cu@C / PPNWF composites;
[0097] It can be seen that the surface of the carrier treated with the coupling agent has a coating, which is unevenly distributed and has different thickness and size. Figure 2 The structures of the three carriers can be clearly seen in the figure. Both PETAQUA and PPNWF have irregular three-dimensional network structures, while PUSNG has a porous block structure. In terms of compactness, the structure of PUSNG is more compact, followed by the fiber structure of PPNWF, and the fiber structure of PETAQUA is the loosest. Figure 2It can be seen that compared with PETAQUA and PPNWF, the surface of PUSNG is rougher, which is conducive to the loading of nanoparticles on its surface, and the volume of block aggregates is much larger than that of the other two carriers. CCCSNs no longer exist as single particles on the carrier, but aggregate to form aggregates through coupling to "adhere" to the surface of the carrier, and it is difficult to see the single particle morphology.
[0098] 3. By Figure 3-5 As shown in Table 2, the load of the three carriers before disturbance increases with the increase of the concentration of CCCSNs suspension. PETAQUA reaches a maximum load of 0.046g at a concentration of 100mg / L, and the load decreases after exceeding this concentration. The reason is that after the concentration of nanomaterials exceeds the saturated load, the number of free nanoparticles increases, causing the "self-agglomeration" phenomenon and reducing the load. PUSNG and PPNWF reach a maximum load of 0.070g and 0.085g respectively at a concentration of 120mg / L. After disturbance, the three carriers all show good load stability, and the load basically increases with the increase of concentration. The load of PETAQUA and PUSNG begins to decrease when the concentration exceeds 100mg / L, and the load of PPNWF is the largest at a concentration of 120mg / L, which is 0.0578g. Combined with the load stability in Table 2, the maximum stability of the three carriers appears at 100mg / L, and almost all are greater than 70%.
[0099] Table 2. Loading stability under different nanomaterial suspension concentration conditions (%)
[0100] Carrier 40mg / L 60mg / L 80mg / L 100mg / L 120mg / L PETAQUA 68 74 65 76 73 PUSNG 70 58 59 71 58 PPNWF 71 60 68 78 77
[0101] 4. Load density determines the efficiency of nanomaterials in the carrier "microenvironment". The greater the load density, the more nanomaterials per unit volume and the higher the efficiency. However, if the load density is too large, the nanoparticles will occupy each other's adsorption points, which will reduce the efficiency. Figure 6-8 As shown in Table 3, the maximum loading densities of the three complexes are concentrated in the 100 mg / L and 120 mg / L experimental groups. The maximum loading densities of PETAQUA before and after disturbance are both in the 100 mg / L experimental group, which are 0.0091 g / cm 3 and 0.0068g / cm 3 The loss rate is about 25%; the maximum pre-disturbance load density of PUSNG in the 120 mg / L experimental group is 0.0690 g / cm 3 The loss rate is about 44%, and the maximum load density after disturbance is 0.0420 g / cm in the 100 mg / L experimental group. 3 , the loss rate is about 29%; the maximum load density of PPNWF before and after disturbance is 0.0150g / cm 3and 0.0120g / cm 3 , the loss rate is about 24%. PUSNG has the highest loading density and the highest loss rate under the same conditions; PPNWF has the lowest loss rate. Combining the loading capacity and stability experiments, the optimal CCCSNs concentration of PETAQUA and PUSNG is 100 mg / L, and the optimal CCCSNs concentration of PPNWF is 120 mg / L.
[0102] Table 3. Loss rate (%) under different nanomaterial suspension concentration conditions
[0103] Carrier 40mg / L 60mg / L 80mg / L 100mg / L 120mg / L PETAQUA 32 22 38 25 26 PUSNG 23 43 41 29 44 PPNWF 31 40 32 22 24
[0104] 5. By Figure 9-11 As shown in Table 4, the three carriers have different adaptability to different coupling agents. PETAQUA has the largest load before disturbance when there is no coupling agent. The experimental group using silane coupling agent KH570 is the optimal group for PETAQUA load after disturbance, which is 0.0339g and the stability is 74%; the KH560 group has the highest load stability, which is 86%. PUSNG has higher adaptability to titanate coupling agents than other types, among which CS171 has the best coupling effect, with a load and stability of 0.08g and 81% before disturbance, respectively, making it the optimal coupling agent for nano-Cu@C / PUSNG complexes. PPNWF has better adaptability to silane coupling agents than titanates, among which the KH570 group has the largest load and stability, which are 0.07g and 78%, respectively, making it the optimal coupling agent for nano-Cu@C / PPNWF complexes. In general, except for PETAQUA, the loading capacity of CCCSNs on the carrier after adding coupling agent was higher than that of the group without coupling agent, and the loading stability was greater than that of the group without coupling agent. The loading rate of the experimental group with the maximum loading capacity exceeded 50%, indicating that the type of coupling agent is one of the important factors affecting the loading effect of nanomaterials.
[0105] Table 4. Loading stability under different coupling agent types (%)
[0106]
[0107] 6. By Figure 12-14 As shown in Table 5, PETAQUA and PPNWF have the highest loading density in the silane coupling agent experimental group. The maximum pre-disturbance loading density of PETAQUA is in the physical etching group, reaching 0.011 g / cm 3 , loss rate 46%; the maximum load density after disturbance is KH560 group, reaching 0.0058g / cm 3 , loss rate 15%. The maximum load density of PUSNG before and after disturbance is 0.076g / cm for CS171 group. 3 and 0.062g / cm 3, loss rate 19%. The maximum load density of PPNWF before and after disturbance is 0.014g / cm 3 and 0.011 g / cm 3 , loss rate 23%. Combining the results of loading capacity and loading stability experiments, the optimal coupling agent for PUSNG is CS171, and the optimal coupling agent for PPNWF is KH570. Although the addition of KH560 to PETAQUA reduces the initial loading capacity, it improves the loading stability by 21%. Therefore, considering the comprehensive engineering application and ecological safety, KH560 is selected as the optimal coupling agent for nano-Cu@C / PETAQUA complex.
[0108] Table 5. Loss rate (%) under different nanomaterial suspension concentration conditions
[0109]
[0110] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions of the technical solution of the present invention by ordinary technicians in this field do not deviate from the essence and scope of the technical solution of the present invention.
Claims
1. A nano Cu@C-OH-PAM composite material, characterized in that: The nano Cu@C with a core-shell structure is prepared by the following preparation method: the nano Cu@C-OH is obtained by activating the nano Cu@C-OH with a core-shell structure, and the nano Cu@C-OH-PAM composite material is obtained by dispersing the nano Cu@C-OH in a polyacrylamide solution; the particle size of the nano Cu@C-OH is 100-200nm.
2. The nano Cu@C-OH-PAM composite material according to claim 1, characterized in that: The activating agents used in the activation are NaOH and H2O2.
3. The nano Cu@C-OH-PAM composite material according to claim 1, characterized in that: The preparation method comprises the following steps: a: Activation: Mix nano Cu@C with a concentration of 100-130 mg / mL with NaOH solution and H2O2 solution, and stir for 50-70 min to obtain nano Cu@C-OH; b: Dispersion: Nano Cu@C-OH was mixed with 0.03-0.08% polyacrylamide solution for 50-70 min and ultrasonicated for 1.5-3 h to obtain nano Cu@C-OH-PAM composite material.
4. The nano Cu@C-OH-PAM composite material according to claim 3, characterized in that: In step a, the concentration is 100-120 mg / mL; In step a, the mass fraction of the NaOH solution is 3-8%; In step a, the mass fraction of the H2O2 solution is 3-8%; In step a, the mixing is ultrasonic, and the ultrasonic time is 20-40 minutes; In step a, the stirring temperature is 45-50° C. and the rotation speed is 1900-2000 r / min.
5. The nano Cu@C-OH-PAM composite material according to claim 3, characterized in that: In step b, the mass fraction of the polyacrylamide solution is 0.04-0.06%; In step b, the mixing temperature is 45-55° C. and the rotation speed is 1800-2200 r / min; In step b, the temperature of the ultrasound is 45-55°C.
6. Use of the nano Cu@C-OH-PAM composite material according to any one of claims 1 to 5 in preparing a nano Cu@C / carrier complex for algae removal.
7. A nano Cu@C / carrier complex for algae removal, characterized in that: The invention comprises the nano Cu@C-OH-PAM composite material according to any one of claims 1 to 5 and a carrier; the carrier is selected from at least one of polyester fiber Acoman, polyurethane sponge and polypropylene non-woven fabric.
8. The method for preparing the nano Cu@C / carrier complex for algae removal according to claim 7, characterized in that: The following steps are involved: S1: Carrier treatment: the carrier is mixed with a solvent and the pH is adjusted to 6.5-7.5 to obtain a pretreated carrier; S2: Preparation of nano Cu@C-OH-PAM composites; S3: Chemical coupling: premix the pretreated carrier with the solution of the coupling agent, then put it into 40-60 mg / L of the nano-Cu@C-OH-PAM composite material and mix for 3-5 hours to obtain a nano-Cu@C / carrier complex.
9. The preparation method according to claim 8, characterized in that: In S3, the coupling agent is selected from at least one of KH560, CS171, and KH570; In S3, the premixing time is 20-50 min; In S3, the mixing time is 20-40 minutes; the mixing temperature is 45-55° C., and the rotation speed is 1800-2200 r / min.
10. Use of the nano Cu@C / carrier complex for algae removal according to claim 7 in preparing a material for inhibiting or removing filamentous green algae in water.
Citation Information
Cited By
Method for efficiently removing algae based on trace copper ion activated calcium peroxide
CN120441127A
Method for efficiently removing algae based on activation of calcium peroxide by trace copper ions