TiO2 nano jungle sensing chip modified by self-driven assembled strong interconnection hybrid layer, preparation and application
The TiO2 nano jungle sensing chip modified by self-driven assembled strong interconnect hybrid layer uses a high-conductivity pitch titanium dioxide nanotube array and spherical polypyrrole and molybdenum oxide hybrid nanoparticles to solve the existing NO2 gas sensor in low The limitations of concentration detection accuracy and response speed enable high sensitivity detection at room temperature and are suitable for industrial and clinical medical applications.
Patent Information
- Application Number
- CN202410900388.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing NO2 gas sensors have limitations in low concentration detection accuracy and response speed, and most of them need to operate at high temperatures, increasing energy consumption and limiting their applicability to specific environments.
TiO2 nano jungle sensing chip modified with a self-driven assembly, highly interconnected hybrid layer, optimizes the gas diffusion path and improves response through the combination of high-conductivity pitch titanium dioxide nanotube array and spherical polypyrrole and molybdenum oxide hybrid nanoparticles. speed and high sensitivity detection at room temperature.
It realizes high-precision and rapid response detection of NO2, reduces detection temperature, improves operating stability and sensitivity, and is suitable for industrial emission monitoring and clinical medical applications.
Smart Images

Figure CN118883646A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of gas sensing technology, and in particular to a TiO2 nano-jungle sensing chip modified with a strongly interconnected hybrid layer assembled by self-driven assembly, and its preparation and application. Background Art
[0002] With the rapid development of industrial technology, air quality issues have become a focus of great concern in the scientific community. Nitrogen dioxide (NO2), as a harmful gas, is not only the main source of photochemical smog, acid rain and ozone, but also causes permanent damage to the human respiratory system when its concentration exceeds 1ppm, and may increase the risk of asthma, chronic obstructive pulmonary disease (COPD) and cardiovascular disease. In addition, NO2 can also be used as an exhaled breath marker for patients with lung tissue infections and gastrointestinal disorders, and its concentration is usually in the ppb order of magnitude. Therefore, the development of an efficient NO2 gas sensor to achieve ultra-high sensitivity room temperature detection of NO2 has great scientific significance and application value for environmental monitoring and clinical medicine.
[0003] Currently, NO2 is mainly detected by gas chromatography (mass spectrometry), laser spectroscopy and gas sensors. Gas chromatography and laser spectroscopy are generally not suitable for daily environments due to their high cost, complex operation and large equipment. In contrast, gas sensors are widely used in flammable and explosive environments, breath analysis and environmental monitoring due to their small size, low cost and easy operation. However, gas sensors on the market have limitations in the accuracy and response speed of low-concentration (ppb level) detection, and most of them need to operate at high temperatures to ensure sensitivity and selectivity, which increases energy consumption and limits their applicability in specific environments.
[0004] The gas sensing detection mechanism of metal oxide semiconductor nanomaterials is mainly based on the surface chemical reaction between the target gas and the oxygen molecules adsorbed on the surface of the material. Due to their unique physical and chemical sensitivity in gas adsorption and reactivity, they are able to provide highly sensitive and fast-response sensing solutions that accurately reflect environmental changes. Among them, titanium dioxide has attracted widespread attention due to its non-toxicity, high chemical stability, excellent electron transport and photoelectric conversion properties. Many titanium dioxide nanostructures with large specific surface areas have been used to enhance gas sensing performance. These structures can increase the number of surface active sites and are very sensitive to changes in the external atmospheric environment. However, there are still some problems with the unmodified spaced titanium dioxide nanotubes when used for gas detection, such as: slow response and recovery; poor selectivity for gas, making it difficult to accurately identify the target gas in a variety of gas environments; and high detection temperature.
[0005] Based on the above content, it is an urgent problem to prepare a spacing-type titanium dioxide nanotube sensor chip that is conducive to the diffusion of NO2 gas and to precisely control its structure and surface properties to improve the response recovery speed, reduce the operating temperature and improve the sensitivity. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a TiO2 nano-jungle sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven assembly, preparation and application. The chip uses specific materials and designs to achieve high-precision and fast response detection of NO2 at room temperature, overcoming the problems of low sensitivity, high operational stability and poor stability of existing gas-sensitive chips, and is suitable for industrial emission monitoring and clinical medical applications.
[0007] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven means, which is a composite material of a highly conductive spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is a spherical polypyrrole and molybdenum oxide hybrid nanoparticle.
[0008] The nanotube array is a titanium dioxide nanotube grown on a substrate with a spacing, the diameter of the titanium dioxide nanotube is 240-260nm, the length is 3-5μm, and the spacing between the titanium dioxide nanotubes is 300-400nm. The spacing of the high-conductivity spacing titanium dioxide nanotube array is used to optimize the gas diffusion path, reduce the detection time, and improve the response speed.
[0009] The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defects, the conductivity of nanotubes is as high as 10 3 ~10 4 Ω.
[0010] The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
[0011] A method for preparing a TiO2 nano-jungle sensor chip comprises the following steps:
[0012] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0013] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.01 to 0.08, and the mass fraction of NH4F in the mixed solution is 0.2 to 1.5%, and a constant voltage of 30 to 80 V is applied for a duration of 20 to 60 min;
[0014] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining at 400-500° C. for 1-4 hours to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0015] Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array:
[0016] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.1 to 1 mol / L, a constant voltage of -5 to -1 V is applied, and the duration is 1.5 to 5 min to obtain a Ti nanotube forest array. 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects;
[0017] Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array;
[0018] Step 3: preparing an electrolyte containing polypyrrole and molybdenum salt:
[0019] Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0020] Step 3.2, adding 0.001-0.06 mmol / L of polypyrrole and 0.0002-0.01 mmol / L of molybdenum salt to the mixed solution A, and stirring until the solution is uniform;
[0021] Step 4: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0022] Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry;
[0023] Step 4.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
[0024] In the step 3.1, the volume ratio of sulfuric acid to deionized water is 0.01-0.1%, and the concentration of sodium sulfate is 0.05-1 mmol / L.
[0025] In the step 3.2, the molybdenum salt is ammonium molybdate, sodium molybdate or potassium molybdate.
[0026] In the step 3.2, the polypyrrole is distilled and has a transparent color.
[0027] In the step 4.1, the voltage range of the cyclic voltammetry is -2.5-+2.5 V, the scan rate is 30-240 mV / s, and the number of scans is 2-30 times.
[0028] An application of a TiO2 nano-jungle sensor chip, the TiO2 nano-jungle sensor chip is used for NO2 detection, has high sensitivity, a detection temperature of 15-30°C, a detection limit as low as 0-10ppb, and is used for respiratory gas detection and environmental quality detection.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. The method of the present invention is easy to operate, highly controllable and time-saving;
[0031] 2. The present invention uses a large-pitch titanium dioxide nano-forest array as a support and electron collector for the NO2 sensor chip, providing sufficient paths and more reaction sites for the NO2 gas flow;
[0032] 3. The present invention uses strongly interconnected polypyrrole and molybdenum oxide hybrid nanoparticles to promote the transport of carriers, increase the number of electrons participating in the sensing reaction, and ultimately achieve high-sensitivity detection of NO2 at room temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a physical picture of the sensor chip prepared in Example 1;
[0034] Figure 2 This is a scanning electron microscope (SEM) photograph of the titanium dioxide nanotube composite material prepared in Example 1;
[0035] Figure 3 is the X-ray diffraction (XRD) pattern of the titanium dioxide nanotube composite material prepared in Example 1;
[0036] Figure 4 is the infrared spectrum (FT-IR) of the titanium dioxide nanotube composite material prepared in Example 1;
[0037] Figure 5(a)-Figure 5(e) is the X-ray photoelectron spectrum (XPS) of the titanium dioxide nanotube composite material prepared in Example 1;
[0038] Figure 6 The dynamic response curve of the sensor chip in Example 1 for detecting NO2 in the ppb range;
[0039] Figure 7 This is a calculation diagram of the detection limit of NO2 of the sensor chip in Example 1. DETAILED DESCRIPTION
[0040] Example 1
[0041] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving is a composite material of a highly conductive spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0042] The nanotube array is a titanium dioxide nanotube grown on a substrate with a spacing, the diameter of the titanium dioxide nanotube is 240-260nm, the length is 3-5μm, and the spacing between the titanium dioxide nanotubes is 300-400nm. The spacing of the high-conductivity spacing titanium dioxide nanotube array is used to optimize the gas diffusion path, reduce the detection time, and improve the response speed.
[0043] The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defect, the conductivity of the nanotube is 4×10 4 Ω.
[0044] The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
[0045] The method for preparing the TiO2 nano-jungle sensor chip comprises the following steps:
[0046] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0047] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.03, the mass fraction of NH4F in the mixed solution is 1%, and a constant voltage of 60V is applied for 30min;
[0048] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining it at 450° C. for 2 h to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0049] Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array:
[0050] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.2 mol / L, a constant voltage of -2 V is applied for 2 min, and the Ti-containing 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects;
[0051] Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array;
[0052] Step 3: preparing an electrolyte containing polypyrrole and molybdenum salt:
[0053] Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0054] Step 3.2, add 0.006 mmol / L of polypyrrole and 0.00042 mmol / L of molybdenum salt to the mixed solution A, and stir until the solution is uniform;
[0055] Step 4: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0056] Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry;
[0057] Step 4.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
[0058] In the step 3.1, the volume ratio of sulfuric acid to deionized water is 0.09%, and the concentration of sodium sulfate is 0.05-0.5 mmol / L.
[0059] In the step 3.2, the molybdenum salt is ammonium molybdate.
[0060] In the step 3.2, the polypyrrole is distilled and has a transparent color.
[0061] In the step 4.1, the voltage range of the cyclic voltammetry is -1.5-+2V, the scan rate is 180mV / s, and the number of scans is 8 times.
[0062] The TiO2 nano-jungle sensor chip is used for NO2 detection, has high sensitivity, a detection temperature of 25°C, a detection limit of 0.15ppb, and is used for respiratory gas detection and environmental quality detection.
[0063] The titanium dioxide nanotube composite material sensor chip obtained in Example 1 is Figure 1 The results are shown in Figure 2, and the results are characterized by scanning electron microscopy (SEM), X-ray diffraction (XRD), infrared spectroscopy (FT-IR) and X-ray photoelectron spectroscopy (XPS). Figure 2 , Figure 3 , Figure 4 , Figure 5(a), Figure 5(b), Figure 5(c), Figure 5(d), and Figure 5(e). Figure 2 It can be seen from the figure that the diameter of the titanium dioxide nanotubes is 240-260nm, and the spacing between the tubes is 300-400nm, which provides space for the subsequent modification of nanoparticles. In addition, it can be clearly seen from the electron microscope photos that the spherical nanoparticles have been successfully modified to the inner and outer sides of the titanium dioxide nanotube wall and the top of the tube. Figure 3 It can be seen that the (101), (103), (004), (112), (200), (105), (211), (204), (220) and (301) crystal planes of the anatase phase indicate that the titanium dioxide prepared is anatase phase. It can also be found in the figure that polypyrrole and molybdenum oxide are both amorphous structures. Furthermore, it can be obtained from infrared spectroscopy (FT-IR) ( Figure 4 ), 729cm -1 The characteristic peaks at 1050, 1457 and 1558 cm are attributed to the vibration peaks of O-Mo-O; -1 The characteristic peaks at are attributed to the stretching vibrations of CH, CN and C=C in the pyrrole ring. All the characteristic peaks indicate that polypyrrole and molybdenum oxide nanoparticles are successfully modified onto titanium dioxide nanotubes. In addition, as shown in Figure 5, Ti, O, Mo, N and C elements are present in the titanium dioxide nanocomposite material, indicating that polypyrrole and molybdenum oxide are connected by molybdenum-nitrogen bonds.
[0064] The NO2 sensing performance of the sensor chip based on titanium dioxide nanotube composite material was tested. The results are as follows Figure 6 and Figure 7 As shown. Figure 6 The obtained sensor chip shows a sensitive response to trace amounts of NO2 at the ppb level (1-1000 ppb). Figure 7 It can be seen that the response of the sensor chip to NO2 is positively correlated with the concentration, with a good linear relationship and a minimum detection limit of 0.15 ppb.
[0065] Example 2
[0066] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving is a composite material of a highly conductive spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0067] The nanotube array is a titanium dioxide nanotube grown on a substrate with a spacing, the diameter of the titanium dioxide nanotube is 240-260nm, the length is 3-5μm, and the spacing between the titanium dioxide nanotubes is 300-400nm. The spacing of the high-conductivity spacing titanium dioxide nanotube array is used to optimize the gas diffusion path, reduce the detection time, and improve the response speed.
[0068] The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defect, the conductivity of the nanotube is 8×10 3 Ω.
[0069] The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
[0070] The method for preparing the TiO2 nano-jungle sensor chip comprises the following steps:
[0071] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0072] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.05, and the mass fraction of NH4F in the mixed solution is 1.2%, and a constant voltage of 60V is applied for 20min;
[0073] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining it at 400° C. for 1.5 h to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0074] Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array:
[0075] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.1 mol / L, a constant voltage of -3 V is applied for 1 min, and the Ti-containing 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects;
[0076] Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array;
[0077] Step 3, preparing an electrolyte containing polypyrrole and molybdenum salt;
[0078] Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0079] Step 3.2, add 0.012 mmol / L of polypyrrole and 0.00084 mmol / L of molybdenum salt to the mixed solution A, and stir until the solution is uniform;
[0080] Step 4: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0081] Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry;
[0082] Step 4.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
[0083] In the step 3.1, the volume ratio of sulfuric acid to deionized water is 0.05%, and the concentration of sodium sulfate is 0.1 mmol / L.
[0084] In the step 3.2, the molybdenum salt is sodium molybdate.
[0085] In the step 3.2, the polypyrrole is distilled and has a transparent color.
[0086] In the step 4.1, the voltage range of the cyclic voltammetry is -2–+2.5 V, the scan rate is 120 mV / s, and the number of scans is 5 times.
[0087] The TiO2 nano-jungle sensor chip is used for NO2 detection, has high sensitivity, a detection temperature of 20°C, a detection limit of 4ppb, and is used for respiratory gas detection and environmental quality detection.
[0088] Example 3
[0089] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving is a composite material of a highly conductive spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0090] The nanotube array is a titanium dioxide nanotube grown on a substrate with a spacing, the diameter of the titanium dioxide nanotube is 240-260nm, the length is 3-5μm, and the spacing between the titanium dioxide nanotubes is 300-400nm. The spacing of the high-conductivity spacing titanium dioxide nanotube array is used to optimize the gas diffusion path, reduce the detection time, and improve the response speed.
[0091] The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defect, the conductivity of the nanotube is 2×10 4 Ω.
[0092] The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
[0093] The method for preparing the TiO2 nano-jungle sensor chip comprises the following steps:
[0094] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0095] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.04, the mass fraction of NH4F in the mixed solution is 0.6%, and a constant voltage of 55V is applied for 40min;
[0096] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining it at 480° C. for 1 h to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0097] Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array:
[0098] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.2 mol / L, a constant voltage of -5 V is applied for 3 min, and the Ti-containing 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects;
[0099] Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array;
[0100] Step 3: preparing an electrolyte containing polypyrrole and molybdenum salt:
[0101] Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0102] Step 3.2: Add 0.03 mmol / L of polypyrrole and 0.0042 mmol / L of molybdenum salt to the mixed solution A, and stir until the solution is uniform.
[0103] Step 4: Preparation of self-driven assembly of polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0104] Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry;
[0105] Step 4.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
[0106] In step 3.1, the volume ratio of sulfuric acid to deionized water is 0.02%, and the concentration of sodium sulfate is 0.5 mmol / L.
[0107] In the step 3.2, the molybdenum salt is potassium molybdate.
[0108] In the step 3.2, the polypyrrole is distilled and has a transparent color.
[0109] In the step 4.1, the voltage range of the cyclic voltammetry is -1.8-+1.8 V, the scan rate is 260 mV / s, and the number of scans is 10 times.
[0110] The TiO2 nano-jungle sensor chip is used for NO2 detection, has high sensitivity, a detection temperature of 22°C, a detection limit of 6ppb, and is used for respiratory gas detection and environmental quality detection.
[0111] Comparative Example 1
[0112] A TiO2 nano-forest sensor chip is a high-conductivity spacing type titanium dioxide nano-forest array, and the high-conductivity spacing type titanium dioxide nano-forest array is a nanotube array.
[0113] The nanotube array is titanium dioxide nanotubes grown on a substrate with intervals, the diameter of the titanium dioxide nanotubes is 240-260nm, the length is 3-5μm, and the intervals between the titanium dioxide nanotubes are 300-400nm.
[0114] The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defect, the conductivity of the nanotube is 4×10 4 Ω.
[0115] The method for preparing the TiO2 nano-jungle sensor chip comprises the following steps:
[0116] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0117] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.03, the mass fraction of NH4F in the mixed solution is 1%, and a constant voltage of 60V is applied for 30min;
[0118] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining it at 450° C. for 2 h to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0119] Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array:
[0120] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.2 mol / L, a constant voltage of -2 V is applied for 2 min, and the Ti-containing 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects;
[0121] Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array;
[0122] The TiO2 nano-jungle sensor chip is used for NO2 detection, but has low sensitivity, a detection temperature of 25°C, and a detection limit of up to 5ppm, which cannot meet the requirements of breath detection and environmental quality detection. If ppb-level (10ppb) NO2 detection is to be achieved, the sensor chip requires a detection temperature of up to 200°C.
[0123] Comparative Example 2
[0124] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving is a composite material of a spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0125] The nanotube array is titanium dioxide nanotubes grown on a substrate with intervals, the diameter of the titanium dioxide nanotubes is 240-260nm, the length is 3-5μm, and the intervals between the titanium dioxide nanotubes are 300-400nm.
[0126] The titanium in the nanotube array exists in the form of tetravalent titanium, without Ti 3+ (O vacancy) defect, the conductivity of the nanotube is 7×10 7 Ω.
[0127] The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
[0128] The method for preparing the TiO2 nano-jungle sensor chip comprises the following steps:
[0129] Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays:
[0130] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.03, the mass fraction of NH4F in the mixed solution is 1%, and a constant voltage of 60V is applied for 30min;
[0131] Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining it at 450° C. for 2 h to transform it into a spaced anatase phase titanium dioxide nanotube array;
[0132] Step 2: preparing an electrolyte containing polypyrrole and molybdenum salt:
[0133] Step 2.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0134] Step 2.2: Add 0.006 mmol / L of polypyrrole and 0.00042 mmol / L of molybdenum salt to the mixed solution A, and stir until the solution is uniform.
[0135] Step 3: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0136] Step 3.1, using the electrolyte prepared in step 2, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry;
[0137] Step 3.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
[0138] In the step 2.1, the volume ratio of sulfuric acid to deionized water is 0.09%, and the concentration of sodium sulfate is 0.5 mmol / L.
[0139] In the step 2.2, the molybdenum salt is ammonium molybdate.
[0140] In the step 2.2, the polypyrrole is distilled and has a transparent color.
[0141] In the step 3.1, the voltage range of the cyclic voltammetry is -1.5-+2V, the scan rate is 180mV / s, and the number of scans is 8 times.
[0142] The TiO2 nano-jungle sensor chip is used for NO2 detection, but has low sensitivity, a detection temperature of 25°C, and a detection limit of up to 2ppm, which cannot meet the requirements of breath detection and environmental quality detection. If ppb-level (10ppb) NO2 detection is to be achieved, the sensor chip requires a detection temperature of up to 150°C.
[0143] Comparative Example 3
[0144] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving is a composite material of a spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0145] A TiO2 nano-forest sensor chip modified by a strongly interconnected hybrid layer assembled by self-driven driving, characterized in that the sensor chip is a composite material of a highly conductive spacing-type titanium dioxide nano-forest array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-forest array is a nanotube array, and the strongly interconnected hybrid layer is spherical polypyrrole and molybdenum oxide hybrid nanoparticles.
[0146] The spacing type high-conductivity titanium dioxide nanotube array is titanium dioxide nanotubes with spacing grown on a substrate. The diameter of the titanium dioxide nanotubes is 240-260nm, the length is 3-5μm, and the spacing between the tubes is 300-400nm.
[0147] The titanium in the spacing type high conductive titanium dioxide nanotube array exists in the form of trivalent titanium and tetravalent titanium to form Ti 3+ (O vacancy) defect, the conductivity of the tube is as high as 10 3 ~10 4 Ω.
[0148] The polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the polypyrrole and molybdenum oxide to spontaneously assemble into composite nanoparticles. The polypyrrole and molybdenum oxide nanoparticles are evenly distributed on the inner side, outer side and top of the tube wall of the titanium dioxide nanotube.
[0149] The method for preparing the sensor chip comprises the following steps:
[0150] Step 1: Preparation of spaced titanium dioxide nanotube arrays:
[0151] Step 1.1, preparing a spaced titanium dioxide nanotube array by an anodic oxidation method, using a pure titanium sheet as an anode and a platinum sheet as a cathode, and the electrolyte used is a mixed solution of NH4F, deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.03, the mass fraction of NH4F in the mixed solution is 1%, and a constant voltage of 60V is applied for 30min;
[0152] Step 1.2: After the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet is cleaned and blown dry, it is calcined at 450° C. for 2 h to transform it into a spaced anatase phase titanium dioxide nanotube array.
[0153] Step 2: Preparation of high conductivity spaced titanium dioxide nanotube arrays:
[0154] Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube array, using a three-electrode device, the spaced titanium dioxide nanotube array as the working electrode, the platinum sheet as the counter electrode, the silver / silver chloride electrode as the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.2 mol / L, applying a constant voltage of -2 V, the duration is 2 min, and obtaining a Ti-containing 3+ Highly conductive spacing-type TiO2 nanotube arrays with (O vacancy) defects;
[0155] Step 2.2: Clean and dry the prepared high-conductivity spaced titanium dioxide nanotube array.
[0156] Step 3: preparing an electrolyte containing polypyrrole and molybdenum salt:
[0157] Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A;
[0158] Step 3.2: Add 0.1 mmol / L of polypyrrole and 0.1 mmol / L of molybdenum salt to the mixed solution A, and stir vigorously until the solution is uniform.
[0159] Step 4: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays:
[0160] Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-drivenly assembled onto the titanium dioxide nanotube array by cyclic voltammetry;
[0161] Step 4.2: Clean and dry the titanium dioxide nanotube array modified with polypyrrole and molybdenum oxide nanoparticles.
[0162] In step 3.1, the volume ratio of sulfuric acid to deionized water in the electrolyte is 0.09%, and the concentration of sodium sulfate is 0.5 mmol / L.
[0163] In the step 3.2, the molybdenum salt includes ammonium molybdate.
[0164] In the step 3.2, the polypyrrole is distilled and has a transparent color.
[0165] In the step 4.1, the voltage range of the cyclic voltammetry is -2.5-+2.5 V, the scan rate is 5 mV / s, and the number of scans is 50 times.
[0166] The sensor chip is used for NO2 detection, but has low sensitivity, a detection temperature of 25°C, and a detection limit of up to 10ppm, which cannot meet the requirements of breath detection and environmental quality detection. If ppb level (10ppb) NO2 detection is to be achieved, the sensor chip requires a detection temperature of up to 220°C.
[0167] The following are the detection limits of the TiO2 nano-jungle sensor chips obtained in various embodiments and comparative examples.
[0168] Example 1: 0.15 ppb; Example 2: 4 ppb; Example 3: 6 ppb; Comparative Example 1: 5 ppm; Comparative Example 2: 2 ppm; Comparative Example 3: 10 ppm.
[0169] It is easy for those skilled in the art to understand that, under the premise of no conflict, the above-mentioned preferred solutions can be freely combined and superimposed.
[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A strongly interconnected hybrid layer modified TiO via self-driven assembly 2 Nano jungle sensor chip, It is characterized in that The TiO 2 The nano-jungle sensor chip is a composite material of a highly conductive spacing-type titanium dioxide nano-jungle array modified by a strongly interconnected hybrid layer; the highly conductive spacing-type titanium dioxide nano-jungle array is a nanotube array, and the strongly interconnected hybrid layer is a spherical polypyrrole and molybdenum oxide hybrid nanoparticle.
2. A TiO2 modified by a self-driven assembly of a strongly interconnected hybrid layer according to claim 1 2 Nano jungle sensor chip, It is characterized in that The nanotube array is titanium dioxide nanotubes grown on a substrate with intervals, the diameter of the titanium dioxide nanotubes is 240-260nm, the length is 3-5μm, and the intervals between the titanium dioxide nanotubes are 300-400nm.
3. A TiO2 modified by a strongly interconnected hybrid layer assembled by self-driven assembly according to claim 1 2 Nano jungle sensor chip, It is characterized in that The titanium in the nanotube array exists in the form of trivalent titanium and tetravalent titanium, forming Ti 3+ (O vacancy) defects, the conductivity of nanotubes is as high as 10 3 ~10 4 Ω.
4. A TiO2 modified by a strongly interconnected hybrid layer assembled by self-driven assembly according to claim 1 2 Nano jungle sensor chip, It is characterized in that The spherical polypyrrole and molybdenum oxide form a molybdenum-nitrogen covalent bond to achieve strong interconnection. The self-driven assembly is that the molybdenum-nitrogen covalent bond guides the spherical polypyrrole and molybdenum oxide to spontaneously assemble into hybrid nanoparticles. The spherical polypyrrole and molybdenum oxide hybrid nanoparticles are evenly distributed on the inner side, outer side and top of the titanium dioxide nanotube wall.
5. A TiO according to any one of claims 1 to 4 2 Preparation method of nano jungle sensor chip, It is characterized in that The following steps are involved: Step 1: Preparation of spaced anatase phase titanium dioxide nanotube arrays: Step 1.1: Prepare the spaced titanium dioxide nanotube array by anodic oxidation, with pure titanium sheet as anode, platinum sheet as cathode, and NH 4 F, a mixed solution of deionized water and triethylene glycol, wherein the volume ratio of water to triethylene glycol is 0.01 to 0.08, and the NH 4 The mass fraction of F in the mixed solution is 0.2-1.5%, and a constant voltage of 30-80 V is applied for a duration of 20-60 min; Step 1.2, after cleaning and drying the spaced amorphous titanium dioxide nanotube array generated on the pure titanium sheet, calcining at 400-500° C. for 1-4 hours to transform it into a spaced anatase phase titanium dioxide nanotube array; Step 2: Preparation of high conductivity spacing type titanium dioxide nanotube forest array: Step 2.1, using electrochemical reduction method to prepare high conductivity spaced titanium dioxide nanotube forest array; using a three-electrode device, the spaced anatase phase titanium dioxide nanotube array is the working electrode, the platinum sheet is the counter electrode, the silver / silver chloride electrode is the reference electrode, the electrolyte used is a mixed solution of sodium sulfate and deionized water, wherein the sulfate concentration is 0.1 to 1 mol / L, a constant voltage of -5 to -1 V is applied, and the duration is 1.5 to 5 min to obtain a Ti nanotube forest array. 3+ Highly conductive spacing-type TiO2 nanotube forest arrays with (O vacancy) defects; Step 2.2, washing and drying the prepared high-conductivity spacing titanium dioxide nanotube forest array; Step 3: preparing an electrolyte containing polypyrrole and molybdenum salt: Step 3.1, uniformly mixing sodium sulfate, sulfuric acid and deionized water to obtain a mixed solution A; Step 3.2, adding 0.001-0.06 mmol / L of polypyrrole and 0.0002-0.01 mmol / L of molybdenum salt to the mixed solution A, and stirring until the solution is uniform; Step 4: Preparation of self-driven assembled polypyrrole and molybdenum oxide nanoparticle-modified titanium dioxide nanotube arrays: Step 4.1, using the electrolyte prepared in step 3, spherical polypyrrole and molybdenum oxide nanoparticles are self-driven assembled into a high-conductivity spacing-type titanium dioxide nanotube forest array by cyclic voltammetry; Step 4.2: Clean and dry the high-conductivity spaced titanium dioxide nanotube forest array modified with polypyrrole and molybdenum oxide nanoparticles.
6. The preparation method according to claim 5, It is characterized in that In the step 3.1, the volume ratio of sulfuric acid to deionized water is 0.01-0.1%, and the concentration of sodium sulfate is 0.05-1 mmol / L.
7. The preparation method according to claim 5, It is characterized in that In the step 3.2, the molybdenum salt is ammonium molybdate, sodium molybdate or potassium molybdate.
8. The preparation method according to claim 5, It is characterized in that In the step 3.2, the polypyrrole is distilled and has a transparent color.
9. The preparation method according to claim 5, It is characterized in that In the step 4.1, the voltage range of the cyclic voltammetry is -2.5-+2.5 V, the scan rate is 30-240 mV / s, and the number of scans is 2-30 times.
10. A TiO according to any one of claims 1 to 4 2 Nano jungle sensor chip or TiO prepared by any preparation method described in claim 5-9 2 Application of Nano-Jungle Sensor Chip, It is characterized in that The TiO 2 Nanojungle sensor chip for NO 2 Detection, with high sensitivity, detection temperature of 15-30℃, detection limit as low as 0-10ppb, used for respiratory gas detection and environmental quality detection.
Citation Information
Patent Citations
Method for preparing composite material of polypyrrole granules and titanium dioxide nanotube array
CN101955665A
Room temperature formaldehyde gas sensor based on titanium dioxide nanotube array
CN102062750A
Molybdenum-nitrogen co-doped flower-shaped carbon nanosphere / sulfur composite material, preparation method thereof and application in positive electrode of lithium-sulfur battery
CN110797514A
Preparation method of nitrogen-doped titanium dioxide nanotube loaded with molybdenum disulfide and nitrogen-doped titanium dioxide nanotube loaded with molybdenum disulfide
CN111383849A
Method of fabricating gas sensor nanoarray including metal oxide nanowire pattern
KR1020140103816A