Metal organic framework material ZIF composite membrane as well as preparation method and application thereof

By adopting a composite structure of porous support film layer, polypyrrole layer and ZIF layer in the ZIF film, the problem of insufficient strength and density in the hydrogen/carbon dioxide separation is solved, and efficient hydrogen/carbon dioxide separation performance is achieved , and reduces production costs.

CN118892747AActive Publication Date: 2024-11-05CHINA PETROLEUM & CHEMICAL CORP +1

Patent Information

Application Number
CN202310497923.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-05
Publication Date
2024-11-05
Estimated Expiration
2043-05-05

AI Technical Summary

Technical Problem

The existing ZIF membranes have problems such as poor strength, poor density continuity, and further improvement in permeability in hydrogen/carbon dioxide separation, and the existing preparation methods are complex and are not suitable for large-scale production.

Method used

Using a composite membrane structure of porous support membrane layer, polypyrrole layer and ZIF layer, the porous support membrane is modified by polypyrrole polymer, which enriches metal ions, and forms a ZIF composite membrane of metal organic frame material in the ZIF precursor solution to simplify The preparation process and improves the density and permeability of the membrane.

Benefits of technology

The prepared ZIF composite film has excellent strength, density and permeability, which significantly improves the separation performance of hydrogen/carbon dioxide, reduces the preparation cost, and is simple and easy to control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a metal organic framework material ZIF composite membrane as well as a preparation method and application thereof. The ZIF composite membrane sequentially comprises a porous support membrane layer, a polypyrrole layer and a ZIF layer. According to the preparation method, the porous support membrane is modified by adopting the polypyrrole polymer, so that the interface bonding property between the ZIF crystal and the porous support membrane is improved, and the compact and continuous ZIF composite membrane is obtained; in addition, the pyrrole monomer is low in price, so that the preparation cost is remarkably reduced. The metal organic framework ZIF composite membrane provided by the invention has better separation performance when being used in a hydrogen / carbon dioxide separation system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to membrane separation materials, and in particular to metal organic framework materials, and specifically to a metal organic framework material ZIF composite membrane and a preparation method and application thereof. Background Art

[0002] Typically, hydrogen is produced through the reforming or gasification of traditional fossil fuels, while carbon dioxide as a byproduct is captured and utilized or stored. Separating hydrogen from carbon dioxide and achieving efficient purification of hydrogen are key steps to improve the economic competitiveness of this technology and promote the promotion and use of hydrogen energy. Compared with traditional separation technologies such as adsorption and crystallization, membrane separation technology has the advantages of low energy consumption, high efficiency, and easy operation. It is considered to be one of the most promising technologies in the 21st century. The key to developing membrane separation technology to purify hydrogen lies in the development of high-performance membrane materials, increasing hydrogen flux, reducing membrane area and system costs, and at the same time improving selectivity and product purity.

[0003] According to the solution-diffusion model, the gas permeation rate P A Represented as P A =S A ×D A , where S A is the gas solubility coefficient, D A is the gas diffusion coefficient. Gas selectivity (P A / P B ) is the ratio of the two gas permeation rates, i.e., the solubility selectivity (S A / S B ) and diffusion selectivity (D A / D B ). In terms of solubility coefficient, the critical temperature of carbon dioxide is 304K, and the critical temperature of hydrogen is 33K. Carbon dioxide is easier to compress than hydrogen, and the solubility coefficient of carbon dioxide in the membrane material is higher than that of hydrogen. In terms of diffusion coefficient, the molecular dynamics diameter of hydrogen is 0.289nm, and the molecular dynamics diameter of carbon dioxide is 0.33nm. The diffusion coefficient of hydrogen in the membrane material is higher than that of carbon dioxide. Therefore, the free volume or pore size of the membrane material should be as close as possible to the range of 0.289-0.33nm to improve the molecular sieving ability and maximize the diffusion selectivity of hydrogen and carbon dioxide.

[0004] Metal-organic framework materials are a type of organic-inorganic hybrid porous materials with a periodic skeleton structure formed by self-assembly of inorganic metal centers and organic ligands. Metal-organic framework materials have regular pore structures, controllable pore sizes, high porosity and high specific surface area, as well as excellent chemical and thermodynamic stability, and show great development potential and broad application prospects in the fields of separation, catalysis, and sensing. Traditional polymer separation membranes have disordered segment network structures, and the gas separation process is limited by the dissolution-diffusion model, resulting in mutual constraints between permeability and selectivity, that is, separation membranes with high permeability often have low selectivity, and vice versa. Metal-organic framework material separation membranes have regular porous channels and are expected to break through the upper limit of the separation performance of traditional polymer membranes. Therefore, the preparation and application of metal-organic framework material separation membranes have become a research hotspot in the field of membrane separation. Among them, the crystal structure of the metal-organic framework material ZIF-8 has a window structure with a size of 0.34nm and a cavity structure with a size of 1.16nm. The window size is close to the molecular dynamics diameter of hydrogen and carbon dioxide. Therefore, the molecular sieving effect of the ZIF-8 membrane is expected to achieve the separation of hydrogen / carbon dioxide.

[0005] In recent years, taking ZIF-8 as an example, researchers have done a lot of work on the preparation method of ZIF-8 membrane. At present, the more mainstream methods include: 1. Secondary solvent thermal synthesis method (CN 107349805A), that is, generating ZIF-8 seed particles on a filter paper support layer through a solvent thermal synthesis reaction, and then performing a second solvent thermal synthesis reaction to promote the growth of the seed to form a dense and continuous ZIF-8 membrane. However, this method separates the nucleation and growth steps of the seed, resulting in a complex operation process, inability to accurately control the thickness of the membrane layer, and difficulty in large-scale production. 2. Spraying preparation method (CN 114733368A), that is, spraying the ZIF-8 precursor solution onto a porous support layer treated at high temperature to obtain a crystallized support, which is then placed under high temperature and closed conditions to prepare the ZIF-8 membrane by a sol-gel method. Although this method is suitable for preparing ZIF-8 membranes on inorganic porous supports under high temperature conditions, it is not suitable for preparing ZIF-8 membranes on organic polymer support layers with poor thermal stability. In addition, the high temperature reaction leads to high production energy consumption and high cost, which is not conducive to industrial scale-up production.

[0006] However, the ZIF membrane disclosed in the prior art still has problems such as poor strength, poor density and continuity, and the need to further improve permeability. Summary of the invention

[0007] In order to overcome the problems existing in the prior art, the present invention provides a metal organic framework material ZIF composite membrane and a preparation method and application thereof, wherein the ZIF-8 composite membrane prepared by the method has excellent strength, compactness and permeability, and the preparation method is simple and easy to control. The metal organic framework ZIF composite membrane provided by the present invention is used in a hydrogen / carbon dioxide separation system to have good separation performance.

[0008] The first aspect of the present invention provides a metal organic framework material ZIF composite membrane, which comprises a porous support membrane layer, a polypyrrole layer and a ZIF layer in sequence.

[0009] In the present invention, the thickness of the porous support membrane layer is 1-3000 μm, preferably 10-2000 μm; and / or the thickness of the polypyrrole layer is 50-500 nm, preferably 100-200 nm; and / or the thickness of the ZIF layer is 0.3-5 μm, preferably 0.5-3 μm.

[0010] In the present invention, the material of the porous support membrane layer is selected from at least one of polypropylene, polysulfone, polyethersulfone, aluminum oxide and silicon oxide; and / or the material of the polypyrrole layer is selected from polypyrrole and / or polypyrrole derivatives.

[0011] The second aspect of the present invention provides a method for preparing a metal organic framework material ZIF composite membrane, which is preferably used to prepare the metal organic framework material ZIF composite membrane described in the first aspect of the present invention, comprising: (1) modifying a layer of polypyrrole polymer on the surface of a porous support membrane to obtain a modified porous support membrane; (2) enriching metal ions on the surface of the modified porous support membrane to obtain a metal ion-rich porous support membrane; (3) immersing the metal ion-rich porous support membrane in a ZIF precursor solution, and obtaining the metal organic framework material ZIF composite membrane after treatment.

[0012] In the present invention, the shape of the porous support membrane is selected from at least one of flat plate, tubular, and hollow fiber membrane, and / or the material of the porous support membrane is selected from at least one of polypropylene, polysulfone, polyethersulfone, alumina, and silica.

[0013] In the present invention, step (1) comprises: (1.1) placing the porous support membrane in a solution containing pyrrole monomers, (1.2) adding an initiator solution to the solution, and (1.3) obtaining the modified porous support membrane through reaction and post-treatment.

[0014] In the present invention, the pyrrole monomer is selected from at least one of pyrrole and / or its derivatives; and / or the initiator is selected from at least one of ammonium persulfate and ferric chloride; preferably, the molar ratio of the pyrrole monomer to the initiator is 1:(0.5-3), preferably 1:(1-2).

[0015] In the present invention, the reaction in step (1.3) is carried out at 20-40° C. for 1-4 hours; and / or the post-treatment in step (1.3) comprises: washing once or multiple times with water, acid solution, and alkaline solution in sequence, and then drying.

[0016] In the present invention, step (2) comprises: (2.1) placing the modified porous support membrane in an aqueous solution containing metal ions, (2.2) heating treatment, and (2.3) post-treatment to obtain the porous support membrane rich in metal ions.

[0017] In the present invention, the metal ion is selected from at least one of transition metal ions, preferably at least one of zinc ions, cobalt ions and optionally nickel ions.

[0018] In the present invention, the temperature of the heating treatment in step (2.2) is 40-100°C, preferably 50-80°C, and more preferably 60-70°C; and / or, the time of the heating treatment in step (2.2) is 0.5-5h, preferably 1-3h, and more preferably 1.5-2h; and / or, the post-treatment in step (2.3) includes: cooling to room temperature, taking out from the solution, washing with water once or more, leaving at room temperature for 5-40h, and drying.

[0019] In the present invention, the ZIF precursor solution in step (3) contains metal ions, ligands and water; preferably, the metal ions are selected from at least one of transition metal ions, preferably from at least one of zinc ions, cobalt ions and optional nickel ions; preferably, the ligands are selected from at least one of imidazole ligands, preferably, the imidazole ligands are selected from imidazole and / or its derivatives; preferably, in the ZIF precursor solution, the molar ratio of the metal ions to the ligands is 1:(1-80), preferably 1:(30-75); the molar ratio of the metal ions to water is 1:(1000-8000), preferably 1:(1000-3000).

[0020] In the present invention, the treatment in step (3) includes reaction and post-treatment; preferably, the reaction temperature is 20 to 40° C.; and / or, the post-treatment includes water washing, placing, and drying.

[0021] The third aspect of the present invention provides the use of the metal organic framework material ZIF composite membrane described in the first aspect of the present invention or the metal organic framework material ZIF composite membrane obtained by the preparation method described in the second aspect of the present invention in gas separation, especially in the separation of hydrogen and carbon dioxide.

[0022] The endpoints and any values ​​of the scope disclosed in the present invention are not limited to the precise scope or value, and these scopes or values ​​should be understood to include values ​​close to these scopes or values. For numerical ranges, the endpoint values ​​of each scope, the endpoint values ​​of each scope and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be regarded as specifically disclosed in this article.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The present invention uses polypyrrole polymers to modify the porous support membrane, which is more conducive to improving the interface bonding between the ZIF crystal and the porous support membrane, and obtaining a denser and more continuous ZIF composite membrane; in addition, the pyrrole monomer is low in price, which significantly reduces the preparation cost;

[0025] (2) The ZIF composite membrane provided by the present invention has excellent compactness and continuity, and has good separation performance in the separation of hydrogen and carbon dioxide;

[0026] (3) The preparation method provided by the present invention is simple and easy to control, and the prepared ZIF composite membrane has high quality and good strength. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a SEM image of the surface of the ZIF-8 composite membrane prepared in Example 1 of the present invention;

[0028] Figure 2 This is the XRD diffraction spectrum of the ZIF-8 composite film prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] The following detailed description of the present invention will make the features and advantages of the present invention more clear and explicit.

[0030] One of the purposes of the present invention is to provide a metal organic framework material ZIF composite membrane, which comprises a porous support membrane layer, a polypyrrole layer and a ZIF layer in sequence.

[0031] In a preferred embodiment, the thickness of the porous support membrane layer is 1 to 3000 μm, preferably 10 to 2000 μm, for example, 1 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 60 μm, 80 μm, 100 μm, 500 μm, 1000 μm, 1500 μm, 2000 μm, 2500 μm or 3000 μm.

[0032] In a further preferred embodiment, the material of the porous support membrane layer is selected from at least one of polypropylene, polysulfone, polyethersulfone, aluminum oxide and silicon oxide.

[0033] In a preferred embodiment, the thickness of the polypyrrole layer is 50 to 500 nm, preferably 100 to 200 nm, for example 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm.

[0034] In a further preferred embodiment, the material of the polypyrrole layer is selected from polypyrrole and / or polypyrrole derivatives.

[0035] In a preferred embodiment, the thickness of the ZIF layer is 0.3-5 μm, preferably 0.5-3 μm, more preferably 1-2 μm, for example 0.3 μm, 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm.

[0036] In a further preferred embodiment, the ZIF is ZIF-8.

[0037] The second object of the present invention is to provide a method for preparing a metal organic framework material ZIF composite membrane, comprising: (1) modifying a layer of polypyrrole polymer on the surface of a porous support membrane to obtain a modified porous support membrane; (2) enriching metal ions on the surface of the modified porous support membrane to obtain a metal ion-rich porous support membrane; (3) immersing the metal ion-rich porous support membrane in a ZIF precursor solution to obtain the metal organic framework material ZIF composite membrane after treatment.

[0038] In a preferred embodiment, the shape of the porous support membrane is selected from at least one of flat plate, tubular, and hollow fiber membrane, and / or the material of the porous support membrane is selected from at least one of polypropylene, polysulfone, polyethersulfone, alumina, and silica.

[0039] In a preferred embodiment, step (1) comprises: (1.1) placing the porous support membrane in a solution containing a pyrrole monomer, (1.2) adding an initiator solution to the solution, and (1.3) obtaining the modified porous support membrane through reaction and optional post-treatment.

[0040] In a further preferred embodiment, the pyrrole monomer is selected from at least one of pyrrole and / or its derivatives; and / or the initiator is selected from at least one of ammonium persulfate and ferric chloride.

[0041] Preferably, the initiator solution is slowly added to the solution containing pyrrole monomers. More preferably, the solution containing pyrrole monomers is an aqueous solution, and the initiator solution is an aqueous solution.

[0042] In a further preferred embodiment, the molar ratio of the pyrrole monomer to the initiator is 1:(0.5-3), preferably 1:(1-2), for example 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5 or 1:3.

[0043] Among them, the inventors found through a large number of experiments that the effect of using pyrrole monomers is better than other monomers (such as aniline), for example: the polypyrrole layer is more tightly combined with the porous support membrane, and the mechanical strength of the polypyrrole layer is better than that of the polyaniline layer, so that the obtained ZIF membrane has better mechanical strength, and it is easier to promote the nucleation and growth of ZIF particles on the support layer to obtain a denser, more continuous, more permeable and more selective ZIF membrane. In addition, pyrrole monomers are low in price, which significantly reduces the preparation cost of metal organic framework material separation membranes and improves the economic competitiveness of membrane gas separation (such as hydrogen separation) purification.

[0044] In a preferred embodiment, the reaction in step (1.3) is carried out at 20-40° C. (eg room temperature) for 1-4 h (preferably 2-3 h).

[0045] In a preferred embodiment, the concentration of the pyrrole monomer in the solution containing the pyrrole monomer is 0.01-1 mol / L, preferably 0.05-0.5 mol / L, more preferably 0.1-0.3 mol / L (e.g. 0.15-0.25 mol / L), specifically 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L or 0.3 mol / L.

[0046] In a preferred embodiment, the post-treatment in step (1.3) includes: rinsing one or more times with water (to remove precipitates attached to the membrane surface), acid solution (to remove unreacted residues on the membrane surface), and alkaline solution (to deprotonate the polypyrrole layer), and then drying.

[0047] The function of water washing is to remove the precipitates attached to the membrane surface, the function of acid solution washing is to remove the unreacted residues on the membrane surface, and the function of alkaline solution washing is to deprotonate the polypyrrole layer.

[0048] In a further preferred embodiment, the acid solution is selected from a hydrochloric acid aqueous solution and an acetic acid aqueous solution; and / or the alkaline solution is selected from at least one of an ammonia aqueous solution and a sodium hydroxide aqueous solution.

[0049] In a further preferred embodiment, the concentration of the acid in the acid solution is 0.01-0.2 mol / L, preferably 0.05-0.15 mol / L; and / or the concentration of the alkali in the alkali solution is 0.05-0.2 mol / L, preferably 0.1-0.15 mol / L.

[0050] In a preferred embodiment, the thickness of the polypyrrole polymer in step (1) is 50 to 500 nm, preferably 100 to 200 nm.

[0051] Among them, if the thickness is too small, the mechanical strength is insufficient, and if the thickness is too large, gas penetration is blocked and the gas penetration rate is reduced.

[0052] In a preferred embodiment, step (2) comprises: (2.1) placing the modified porous support membrane in the aqueous solution containing metal ions, (2.2) heating treatment, and (2.3) post-treatment to obtain the porous support membrane rich in metal ions.

[0053] Through this process, metal ions can be enriched on the modified porous support membrane.

[0054] In a further preferred embodiment, the metal ion is selected from at least one of transition metal ions, preferably at least one of zinc ions, cobalt ions and optionally nickel ions.

[0055] In a further preferred embodiment, the concentration of metal ions in the aqueous solution containing metal ions is 0.005-0.335 mol / L, preferably 0.03-0.1 mol / L, for example, 0.005 mol / L, 0.05 mol / L, 0.08 mol / L, 0.1 mol / L, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L or 0.335 mol / L.

[0056] In a preferred embodiment, the temperature of the heating treatment in step (2.2) is 40-100°C, preferably 50-80°C, more preferably 60-70°C; and / or the time of the heating treatment in step (2.2) is 0.5-5h, preferably 1-3h, more preferably 1.5-2h.

[0057] In a preferred embodiment, the post-treatment in step (2.3) includes: cooling to room temperature, taking out from the solution, washing with water once or multiple times, leaving at room temperature for 5 to 40 hours, and drying.

[0058] In a preferred embodiment, the ZIF precursor solution in step (3) contains metal ions, ligands and water.

[0059] In a further preferred embodiment, the metal ion is selected from at least one transition metal ion, preferably at least one of zinc ion, cobalt ion (preferably zinc ion) and optional nickel ion, and more preferably the same as the metal ion in step (2).

[0060] In a further preferred embodiment, the ligand is selected from at least one of the imidazole ligands. Preferably, the imidazole ligand is selected from imidazole and / or its derivatives, for example, at least one selected from 2-methylimidazole, benzimidazole, 2-formylimidazole (preferably 2-methylimidazole).

[0061] In a further preferred embodiment, in the ZIF precursor solution, the molar ratio of the metal ion to the ligand is 1:(1-80), preferably 1:(30-75); the molar ratio of the metal ion to water is 1:(1000-8000), preferably 1:(1000-3000).

[0062] For example, in the ZIF precursor solution, the molar ratio of the metal ion to the ligand is 1:1, 1:5, 1:10, 1:20, 1:30, 1:40, 1:50, 1:55, 1:60, 1:70 or 1:80, and the molar ratio of the metal ion to water is 1:1000, 1:1500, 1:2000, 1:3000, 1:4000, 1:5000, 1:6000, 1:6200, 1:6400, 1:6600, 1:6800, 1:7000 or 1:8000.

[0063] When preparing the ZIF precursor solution, it is preferably prepared in a clear state, for example, by strong stirring or ultrasound until it is clear.

[0064] In a preferred embodiment, the treatment in step (3) includes reaction and optional post-treatment.

[0065] In a further preferred embodiment, the reaction temperature is 20-40°C (e.g., room temperature), the reaction time is 10-48h, preferably 18-24h; and / or, the post-treatment includes washing, placing (preferably 5-40h), and drying. The inventor unexpectedly discovered during the experiment that ZIF can be synthesized under room temperature conditions, which does not require heating, has milder reaction conditions, lower energy consumption, and thus lower costs.

[0066] Wherein, during the reaction, crystal growth is performed to form ZIF particles.

[0067] In a preferred embodiment, the thickness of the ZIF layer on the metal organic framework material ZIF composite membrane is 0.3-5 μm, preferably 0.5-3 μm, more preferably 1-2 μm. In addition, in the present invention, the thickness of the polypyrrole layer is about 50-500 nm, preferably 100-200 nm; the thickness of the porous support membrane layer is 1-3000 μm, preferably 10-40 μm.

[0068] In the present invention, a layer of polypyrrole polymer is first coated on a porous support membrane, a layer of metal ions is then enriched, and finally a ZIF composite membrane is formed in situ. The membrane material prepared by the method of the present invention not only has excellent strength (for example, not easy to peel off), but also has a good gas separation effect (for example, separation of hydrogen and carbon dioxide).

[0069] The third object of the present invention is to provide an application of the metal organic framework material ZIF composite membrane described in the first object of the present invention or the metal organic framework material ZIF composite membrane obtained by the preparation method described in the second object of the present invention in gas separation, especially in the separation of hydrogen and carbon dioxide.

[0070] In a preferred embodiment, when the metal organic framework material ZIF composite membrane is used for hydrogen / carbon dioxide separation, at a temperature of 35°C, the hydrogen permeation rate is about 11600-22300 Barrer, preferably 15000-20000 Barrer, and the hydrogen / carbon dioxide permeation selectivity is 5.0-8.0, preferably 6.0-7.0.

[0071] In the present invention, the gas separation evaluation is as follows: the prepared metal organic framework material ZIF composite membrane is sealed in a gas separation membrane pool, and the hydrogen / carbon dioxide separation performance of the metal organic framework material ZIF composite membrane is investigated by constant volume pressure method. Gas is introduced from the feed side to the upstream of the membrane pool by a gas cylinder; the temperature of the upstream and downstream of the membrane pool is controlled by a constant temperature box; the downstream of the membrane pool is evacuated by a vacuum pump; and the pressure sensor records the gas pressure downstream of the membrane pool in real time. The evaluation indicators of the gas separation performance of the metal organic framework material ZIF composite membrane are hydrogen permeation rate, carbon dioxide permeation rate, and hydrogen / carbon dioxide permeation selectivity.

[0072] The gas permeability is determined by the following formula:

[0073]

[0074] The gas permeation selectivity is determined by the following formula:

[0075]

[0076] Where P is the gas permeability (Barrer, 1Barrer = 1×10-10 cm 3 (STP)cm / cm 2 s cmHg), V is the volume of the cavity downstream of the membrane (cm 3 ), L is the thickness of the membrane (cm), A is the effective membrane area (cm 2 ), T is the test temperature (K), and p2 is the inlet pressure upstream of the membrane (psia). Theoretically, it is hoped that the hydrogen permeability is high and the carbon dioxide permeability is low, pursuing high gas permeation selectivity.

[0077] Example

[0078] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.

[0079] It should also be noted that the various specific technical features described in the following specific embodiments can be combined in any suitable manner without contradiction. To avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0080] In addition, the various embodiments of the present invention may be arbitrarily combined as long as they do not violate the concept of the present invention. The technical solutions thus formed belong to part of the original disclosure of this specification and also fall within the protection scope of the present invention.

[0081] The raw materials used in the examples and comparative examples, if not specifically limited, are all disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation method disclosed in the prior art. Among them, the porous polypropylene support membrane was purchased from Celgard, USA, the porous polyethersulfone support membrane was purchased from Sterlitech, USA, and the porous alumina support membrane was purchased from Guizhou Morui New Materials Technology Co., Ltd.

[0082] [Example 1] Synthesis of metal organic framework material ZIF-8 composite film

[0083] Dissolve 0.67g of pyrrole in 50mL of deionized water and stir to mix evenly. Put the cleaned and dried porous polypropylene support membrane into the above-mentioned aqueous solution of pyrrole. Then dissolve 2.85g of ammonium persulfate in 50mL of deionized water and stir to mix evenly. Slowly pour the ammonium persulfate aqueous solution into the pyrrole aqueous solution and react at room temperature for 2h. After the reaction is completed, take out the polypyrrole-modified polypropylene support membrane, rinse it several times with deionized water, 0.1mol / L hydrochloric acid aqueous solution, and 0.1mol / L ammonia aqueous solution in turn, dry it at room temperature for 24h for standby use, and obtain a polypyrrole-modified porous polypropylene support layer.

[0084] 1.0 g of zinc nitrate hexahydrate was dissolved in 50 mL of deionized water, stirred and mixed evenly, and poured into a reactor, and the prepared polypyrrole-modified porous polypropylene support layer was placed in the reactor, and heated at 60° C. for 2 h; after heating, it was cooled to room temperature, taken out and rinsed with deionized water several times, and then placed at room temperature for 24 h and dried to obtain a zinc ion-rich polypyrrole / porous polypropylene membrane;

[0085] Dissolve 0.11g zinc nitrate hexahydrate and 2.20g 2-methylimidazole in 20mL deionized water, stir vigorously or ultrasonically until clear, and prepare a synthetic ZIF-8 precursor solution; place the zinc ion-rich polypyrrole / porous polypropylene membrane prepared above vertically in a reactor, pour the ZIF-8 precursor solution, and react at room temperature for 24h; after the reaction, take out the zinc ion-rich polypyrrole / porous polypropylene membrane, rinse it with deionized water several times, then place it at room temperature for 24h, and dry it to obtain the metal organic framework material ZIF-8 composite membrane. Among them, the thickness of the porous polypropylene support layer is 25μm, the thickness of the polypyrrole layer is 200nm, and the thickness of the ZIF-8 layer is 1.1μm.

[0086] [Example 2] Synthesis of metal organic framework material ZIF-8 composite film

[0087] Dissolve 0.60g of pyrrole in 50mL of deionized water and stir to mix evenly. Put the cleaned and dried porous polypropylene support membrane into the above-mentioned aqueous solution of pyrrole. Then dissolve 4.56g of ammonium persulfate in 50mL of deionized water and stir to mix evenly. Slowly pour the ammonium persulfate aqueous solution into the pyrrole aqueous solution and react at room temperature for 1h. After the reaction is completed, take out the polypyrrole-modified polypropylene support membrane, rinse it several times with deionized water, 0.2mol / L hydrochloric acid aqueous solution, and 0.15mol / L ammonia aqueous solution in turn, dry it at room temperature for 18h for standby use, and obtain a polypyrrole-modified porous polypropylene support layer.

[0088] 0.5 g of zinc nitrate hexahydrate was dissolved in 50 mL of deionized water, stirred and mixed evenly, and poured into a reactor. The prepared polypyrrole-modified porous polypropylene support layer was placed in the reactor and heated at 80° C. for 1 h. After heating was completed and cooled to room temperature, the support layer was taken out and rinsed with deionized water several times, and then placed at room temperature for 24 h and dried to obtain a zinc ion-rich polypyrrole / porous polypropylene membrane.

[0089] Dissolve 0.22g zinc nitrate hexahydrate and 1.50g 2-methylimidazole in 30mL deionized water, stir vigorously or ultrasonically until clear, and prepare a synthetic ZIF-8 precursor solution; place the zinc ion-rich polypyrrole / porous polypropylene membrane prepared above vertically in a reactor, pour the ZIF-8 precursor solution, and react at room temperature for 15h; after the reaction, take out the zinc ion-rich polypyrrole / porous polypropylene membrane, rinse it with deionized water several times, then place it at room temperature for 24h, and dry it to obtain the metal organic framework material ZIF-8 composite membrane. Among them, the thickness of the porous polypropylene support layer is 30μm, the thickness of the polypyrrole layer is 150nm, and the thickness of the ZIF-8 layer is 1.4μm.

[0090] [Example 3] Synthesis of metal organic framework material ZIF-8 composite film

[0091] Dissolve 0.55g of pyrrole in 50mL of deionized water and stir to mix evenly. Put the cleaned and dried porous polypropylene support membrane into the above-mentioned aqueous solution of pyrrole. Then dissolve 1.62g of ferric chloride in 50mL of deionized water and stir to mix evenly. Slowly pour the ammonium persulfate aqueous solution into the pyrrole aqueous solution and react at room temperature for 2h. After the reaction is completed, take out the polypyrrole-modified polypropylene support membrane, rinse it several times with deionized water, 0.15mol / L hydrochloric acid aqueous solution, and 0.15mol / L ammonia aqueous solution in turn, dry it at room temperature for 24h for standby use, and obtain a polypyrrole-modified porous polypropylene support layer.

[0092] 0.8 g of zinc nitrate hexahydrate was dissolved in 50 mL of deionized water, stirred and mixed evenly, and poured into a reactor, and the prepared polypyrrole-modified porous polypropylene support layer was placed in the reactor, and heated at 60° C. for 2 h; after heating, it was cooled to room temperature, taken out and rinsed with deionized water several times, and then placed at room temperature for 24 h and dried to obtain a zinc ion-rich polypyrrole / porous polypropylene membrane;

[0093] Dissolve 0.20g zinc nitrate hexahydrate and 1.80g 2-methylimidazole in 20mL deionized water, stir vigorously or ultrasonically until clear, and prepare a synthetic ZIF-8 precursor solution; place the zinc ion-rich polypyrrole / porous polypropylene membrane prepared above vertically in a reactor, pour the ZIF-8 precursor solution, and react at room temperature for 24h; after the reaction, take out the zinc ion-rich polypyrrole / porous polypropylene membrane, rinse it with deionized water several times, then place it at room temperature for 24h, and dry it to obtain the metal organic framework material ZIF-8 composite membrane. Among them, the thickness of the porous polypropylene support layer is 20μm, the thickness of the polypyrrole layer is 110nm, and the thickness of the ZIF-8 layer is 2.1μm.

[0094] [Example 4] Synthesis of metal organic framework material ZIF-8 composite film

[0095] Dissolve 0.75g of pyrrole in 50mL of deionized water and stir to mix evenly. Put the cleaned and dried porous polyethersulfone support membrane into the above-mentioned aqueous solution of pyrrole. Then dissolve 2.43g of ferric chloride in 50mL of deionized water and stir to mix evenly. Slowly pour the ammonium persulfate aqueous solution into the pyrrole aqueous solution and react at room temperature for 2h. After the reaction is completed, the polypyrrole-modified polyethersulfone support membrane is taken out, rinsed several times with deionized water, 0.15mol / L hydrochloric acid aqueous solution, and 0.20mol / L ammonia aqueous solution in turn, and dried at room temperature for 24h for standby use to obtain a polypyrrole-modified porous polyethersulfone support layer.

[0096] 1.0 g of zinc nitrate hexahydrate was dissolved in 50 mL of deionized water, stirred and mixed evenly, and poured into a reactor, and the prepared polypyrrole-modified porous polyethersulfone support layer was placed in the reactor, and heated at 60° C. for 2 h; after heating, it was cooled to room temperature, taken out and rinsed with deionized water several times, and then placed at room temperature for 24 h and dried to obtain a zinc ion-rich polypyrrole / porous polyethersulfone membrane;

[0097] Dissolve 0.20g zinc nitrate hexahydrate and 1.80g 2-methylimidazole in 20mL deionized water, stir vigorously or ultrasonically until clear, and prepare a synthetic ZIF-8 precursor solution; place the zinc ion-rich polypyrrole / porous polyethersulfone membrane prepared above vertically in a reactor, pour the ZIF-8 precursor solution, and react at room temperature for 24h; after the reaction, take out the zinc ion-rich polypyrrole / porous polyethersulfone membrane, rinse it with deionized water several times, then place it at room temperature for 24h, and dry it to obtain the metal organic framework material ZIF-8 composite membrane. Among them, the thickness of the porous polyethersulfone support layer is 25μm, the thickness of the polypyrrole layer is 300nm, and the thickness of the ZIF-8 layer is 1.8μm.

[0098] [Example 5] Synthesis of metal organic framework material ZIF-8 composite film

[0099] Dissolve 0.67g of pyrrole in 50mL of deionized water and stir to mix evenly. Put the cleaned and dried porous alumina support membrane into the above-mentioned pyrrole aqueous solution. Then dissolve 3.55g of ammonium persulfate in 50mL of deionized water and stir to mix evenly. Slowly pour the ammonium persulfate aqueous solution into the pyrrole aqueous solution and react at room temperature for 2h. After the reaction is completed, take out the polypyrrole-modified alumina support membrane, rinse it several times with deionized water, 0.1mol / L hydrochloric acid aqueous solution, and 0.1mol / L ammonia aqueous solution in turn, dry it at room temperature for 24h for standby use, and obtain a polypyrrole-modified porous alumina support layer.

[0100] 0.7 g of zinc nitrate hexahydrate was dissolved in 50 mL of deionized water, stirred and mixed evenly, and poured into a reactor, and the prepared polypyrrole-modified porous alumina support layer was placed in the reactor, and heated at 60° C. for 2 h; after heating, it was cooled to room temperature, taken out and rinsed with deionized water several times, and then placed at room temperature for 24 h and dried to obtain a zinc ion-rich polypyrrole / porous alumina membrane;

[0101] Dissolve 0.15g zinc nitrate hexahydrate and 1.60g 2-methylimidazole in 20mL deionized water, stir vigorously or ultrasonically until clear, and prepare a synthetic ZIF-8 precursor solution; place the zinc ion-rich polypyrrole / porous alumina membrane prepared above vertically in a reactor, pour the ZIF-8 precursor solution into it, and react at room temperature for 24h; after the reaction, take out the zinc ion-rich polypyrrole / porous alumina membrane, rinse it with deionized water several times, then place it at room temperature for 24h, and dry it to obtain the metal organic framework material ZIF-8 composite membrane. Among them, the thickness of the porous alumina support layer is 1500μm, the thickness of the polypyrrole layer is 130nm, and the thickness of the ZIF-8 layer is 2.3μm.

[0102] [Comparative Example 1]

[0103] The process of Example 1 was repeated, except that aniline was used in an equal molar amount to replace pyrrole, and other conditions remained unchanged.

[0104] [Comparative Example 2]

[0105] The process of Example 1 was repeated, except that the obtained polypyrrole-modified porous polypropylene support layer was not subjected to zinc-enrichment treatment, but the ZIF membrane was grown directly thereon, while other conditions remained unchanged.

[0106] [Experimental Example 1] SEM characterization of membrane

[0107] The microstructure of the metal organic framework material ZIF-8 film obtained in Example 1 was characterized by FESEM (JEOL JSM-7610F (Hitachi High-Technologies, Tokyo, Japan). Figure 1 As shown. Figure 1 It can be seen that the ZIF-8 membrane is dense and continuous without obvious defects.

[0108] [Experimental Example 2] XRD characterization of the film

[0109] XRD (D / max-UltimaIII (Rigaku Corporation, Japan)) was used to characterize the microstructure of the metal organic framework material ZIF-8 composite film obtained in Example 1. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the ZIF-8 composite membrane contains the characteristic peaks of polypropylene and the characteristic peaks of ZIF-8 particles, indicating that a high-crystallinity ZIF-8 membrane was successfully prepared on the polypropylene support layer.

[0110] [Experimental Example 3] Characterization of membrane strength

[0111] Laboratory filter paper was used to rub the surface of the polyaniline / polypropylene film (before zinc enrichment) prepared in Comparative Example 1 and the surface of the polypyrrole / polypropylene film (before zinc enrichment) prepared in Example 1. The results showed that the polyaniline layer fell off significantly, while the polypyrrole layer remained intact and did not fall off, indicating that the interface between the polypyrrole layer and the polypropylene was more tightly bonded, and the mechanical strength of the polypyrrole layer was higher than that of the polyaniline layer.

[0112] Laboratory filter paper was used to rub the surface of the zinc ion-rich polyaniline / polypropylene film prepared in Comparative Example 1 and the surface of the zinc ion-rich polypyrrole / polypropylene film prepared in Example 1. The results showed that the zinc ion-rich polyaniline layer fell off significantly, while the zinc ion-rich polypyrrole layer remained intact and did not fall off, indicating that the zinc ion-rich polypyrrole layer was more tightly bonded to the interface of the polypropylene, and the mechanical strength of the zinc ion-rich polypyrrole layer was higher than that of the polyaniline layer.

[0113] [Experimental Example 4] Membrane separation evaluation

[0114] The method for evaluating the hydrogen / carbon dioxide separation performance of the metal organic framework material ZIF-8 composite membrane is shown in the aforementioned content of the present invention. The prepared metal organic framework material ZIF-8 composite membrane is sealed in a gas separation membrane pool, and the hydrogen / carbon dioxide separation performance of the metal organic framework material ZIF-8 composite membrane is investigated by constant volume pressure method. Gas is introduced from the feed direction upstream of the membrane pool by a gas cylinder; a thermostat controls the temperature upstream and downstream of the membrane pool; a vacuum pump is used to evacuate the downstream of the membrane pool; and a pressure sensor records the gas pressure downstream of the membrane pool in real time. The evaluation indicators of the gas separation performance of the metal organic framework material ZIF-8 composite membrane are hydrogen permeation rate, carbon dioxide permeation rate, and hydrogen / carbon dioxide permeation selectivity.

[0115] The gas permeability is determined by the following formula:

[0116]

[0117] The gas permeation selectivity is determined by the following formula:

[0118]

[0119] Where P is the gas permeability (Barrer, 1Barrer = 1×10 -10 cm 3 (STP)cm / cm 2 s cmHg), V is the volume of the cavity downstream of the membrane (cm 3 ), L is the thickness of the membrane (cm), A is the effective membrane area (cm 2 ), T is the test temperature (K), and p2 is the inlet pressure upstream of the membrane (psia).

[0120] Table 1: Separation performance of the metal organic framework material ZIF-8 composite membrane synthesized in the above examples and comparative examples at 35°C

[0121] Hydrogen permeation rate (Barrer) Hydrogen / carbon dioxide separation factor (α) Example 1 18200 7.2 Example 2 22300 5.4 Example 3 19050 5.8 Example 4 18500 6.5 Example 5 20100 6.8 Comparative Example 1 13800 5.3 Comparative Example 2 42000 1.5

[0122] As shown in Table 1, Examples 1-5 all obtained dense and continuous ZIF-8 composite membranes, which can be used to separate H 2 / CO 2 , the permeation rate of hydrogen ranges from 18000 to 22300 Barrer, and the separation factor of hydrogen / carbon dioxide is about 5.0 to 7.0. The difference between the permeation rate and the separation factor in Examples 1-5 is mainly attributed to the thickness of the ZIF-8 film and the influence of the preparation conditions on the crystallinity of the ZIF-8 film. The thinner the thickness of the ZIF-8 layer, the higher the permeation rate of hydrogen. The higher the crystallinity of the ZIF-8 layer and the fewer the membrane defects, the higher the selectivity of hydrogen / carbon dioxide.

[0123] In Comparative Example 1, since the gas permeation rate of polyaniline is relatively low, the hydrogen permeation rate of the obtained ZIF-8 composite membrane is lower than that of Examples 1-5.

[0124] In Comparative Example 2, since the obtained polypyrrole-modified porous polypropylene support layer was not subjected to zinc-enrichment treatment, a dense and continuous ZIF composite membrane could not be formed, a large number of defects were generated, and a low hydrogen / carbon dioxide permeation selectivity was exhibited.

[0125] The present invention has been described in detail above in conjunction with specific implementations and exemplary examples, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, a variety of equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.

Claims

1. A metal organic framework material ZIF composite membrane, comprising a porous support membrane layer, a polypyrrole layer and a ZIF layer in sequence.

2. The metal organic framework material ZIF composite film according to claim 1, It is characterized in that The thickness of the porous support membrane layer is 1 to 3000 μm, preferably 10 to 2000 μm; and / or, The thickness of the polypyrrole layer is 50 to 500 nm, preferably 100 to 200 nm; and / or, The thickness of the ZIF layer is 0.3-5 μm, preferably 0.5-3 μm.

3. The metal organic framework material ZIF composite film according to claim 1 or 2, It is characterized in that The material of the porous support membrane layer is selected from at least one of polypropylene, polysulfone, polyethersulfone, aluminum oxide and silicon oxide; and / or, The material of the polypyrrole layer is selected from polypyrrole and / or polypyrrole derivatives.

4. A method for preparing a metal organic framework material ZIF composite film, preferably used for preparing the metal organic framework material ZIF composite film according to any one of claims 1 to 3, include: (1) modifying a layer of polypyrrole polymer on the surface of the porous support membrane to obtain a modified porous support membrane; (2) enriching metal ions on the surface of the modified porous support membrane to obtain a metal ion-rich porous support membrane; (3) immersing the metal ion-rich porous support membrane in a ZIF precursor solution to obtain the metal organic framework material ZIF composite membrane after treatment.

5. The preparation method according to claim 4, It is characterized in that The shape of the porous support membrane is selected from at least one of flat plate, tubular, and hollow fiber membranes, and / or the material of the porous support membrane is selected from at least one of polypropylene, polysulfone, polyethersulfone, alumina, and silicon oxide.

6. The preparation method according to claim 4, It is characterized in that Step (1) comprises: (1.1) placing the porous support membrane in a solution containing a pyrrole monomer, (1.2) adding an initiator solution to the solution, and (1.3) reacting to obtain the modified porous support membrane; Preferably, the pyrrole monomer is selected from at least one of pyrrole and / or its derivatives; and / or, the initiator is selected from at least one of ammonium persulfate and ferric chloride; Preferably, the molar ratio of the pyrrole monomer to the initiator is 1:(0.5-3), preferably 1:(1-2).

7. The preparation method according to claim 4, It is characterized in that Step (2) comprises: (2.1) placing the modified porous support membrane in an aqueous solution containing metal ions, (2.2) heating treatment, and (2.3) post-treatment to obtain the porous support membrane rich in metal ions; Preferably, the metal ion is selected from at least one of transition metal ions, preferably at least one of zinc ions, cobalt ions and optionally nickel ions.

8. The preparation method according to claim 7, It is characterized in that The temperature of the heating treatment in step (2.2) is 40-100°C, preferably 50-80°C, more preferably 60-70°C; and / or, The heating time in step (2.2) is 0.5 to 5 hours, preferably 1 to 3 hours, more preferably 1.5 to 2 hours; and / or, The post-treatment in step (2.3) includes: cooling to room temperature, taking out from the solution, washing with water once or multiple times, leaving at room temperature for 5 to 40 hours, and drying.

9. The preparation method according to any one of claims 4 to 8, It is characterized in that The ZIF precursor solution in step (3) contains metal ions, ligands and water; Preferably, the metal ion is selected from at least one of transition metal ions, preferably at least one of zinc ions, cobalt ions and optionally nickel ions; Preferably, the ligand is selected from at least one of imidazole ligands, preferably, the imidazole ligand is selected from imidazole and / or its derivatives; Preferably, in the ZIF precursor solution, the molar ratio of the metal ion to the ligand is 1:(1-80), preferably 1:(30-75); the molar ratio of the metal ion to water is 1:(1000-8000), preferably 1:(1000-3000).

10. The preparation method according to claim 9, It is characterized in that The treatment in step (3) includes a reaction; preferably, the reaction temperature is 20 to 40°C.

11. Use of the metal organic framework material ZIF composite membrane according to any one of claims 1 to 3 or the metal organic framework material ZIF composite membrane obtained by the preparation method according to any one of claims 4 to 10 in gas separation, especially in separation of hydrogen and carbon dioxide.

Citation Information

Patent Citations

  • Ammonized hollow fiber membrane substrate and application of ammonized hollow fiber membrane substrate to preparation of metal-organic framework membrane

    CN104785129A

  • Synthetic method of metal organic skeleton membrane

    CN104959044A

  • Preparation method of highly-anti-fouling polyvinylidene fluoride (PVDF) porous base composite ultrafiltration membrane material

    CN110280150A

  • In-situ controllable synthesis method of MOF membrane

    CN111249918A

Cited By

  • Metal organic framework material composite membrane as well as preparation method and application thereof

    CN119633770A

  • Metal organic framework material composite membrane, and preparation method therefor and use thereof