Preparation method of high-conductivity graphene copper composite material

By plating copper on graphene-clad copper foil and hot-pressing, the problem of poor interfacial bonding between graphene and copper is solved, and a graphene copper composite material with high conductivity is achieved, with good process controllability and suitable for scale Chemical production.

CN118910548AActive Publication Date: 2024-11-08UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202411037292.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-08
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The poor interfacial bonding between graphene and copper leads to a decrease in material strength and weak interface adhesion, which affects the mechanical and electrical properties of the composite material, making it difficult to achieve uniform dispersion of graphene in metal matrix.

Method used

Magneto-controlled sputtering, electroplating or thermal evaporation technology is used to plate copper on the surface of graphene-clad copper foil, and hot-pressing is carried out through stacked hot pressing to form a highly conductive graphene copper composite material to improve graphene and copper Interface integration.

Benefits of technology

The high conductivity of graphene copper composite material has been achieved, the material density is close to full density, good interface bonding, significantly improved conductivity, and strong controllability of the process, which is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118910548A_ABST
    Figure CN118910548A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-conductivity graphene copper composite material, relates to the technical field of composite material preparation, and aims to solve the problem that the interface structure of graphene copper is regulated and controlled to improve the problem of weak interface adhesive force of the graphene copper. The method comprises the following steps: S1, putting a copper foil coated with graphene into a magnetron sputtering chamber; s2, taking a pure copper target material as a copper source, performing magnetron sputtering treatment on the graphene-coated copper foil, and sputtering a layer of copper on the surface of the graphene-coated copper foil to prepare the graphene-coated copper foil subjected to copper plating treatment; and S3, placing multiple layers of graphene coated copper foils subjected to copper plating treatment prepared in the step S2 into a hot pressing chamber, setting proper hot pressing temperature and pressure intensity, and performing hot pressing forming on the graphene coated copper foils subjected to copper plating treatment by utilizing a lamination hot pressing method to obtain the high-conductivity graphene copper composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material preparation, and in particular to a method for preparing a highly conductive graphene copper composite material. Background Art

[0002] Pure metals have long been considered to have the lowest conductivity at room temperature. Since the first official record of copper's conductivity about 100 years ago, a large number of studies on highly refined copper metal have only improved the conductivity by about 3%. The widely used International Annealed Copper Standard (IACS) records the conductivity of pure copper at room temperature as 5.8×10 7 S / m, among metals, only silver has a better electrical conductivity than copper (about 108% IACS), but its cost is too high, so copper-based materials have always been used as the main conductive material.

[0003] In order to improve the conductivity of copper-based materials, the method of preparing high-purity copper by increasing purity, reducing grain boundaries and reducing defects has gradually approached the physical limit, the cost has increased significantly, and the technical requirements have become more and more stringent; and the addition of other alloy materials (such as tin, rare earth elements, etc.) also often has the phenomenon of decreased conductivity due to process instability or copper-based lattice distortion, which has certain limitations. The use of metallic copper and new materials to prepare ultra-high conductive copper-based composite materials has attracted extensive research.

[0004] Graphene is an allotrope of carbon atoms and a two-dimensional crystalline material. It is the basic single-layer SP of a two-dimensional lattice component. 2 Hybrid (two-dimensional honeycomb structure) carbon atoms. In 2004, British scientists successfully prepared graphene sheets for the first time. The carbon atoms inside the graphene sheets are bonded by σ bonds with extremely high bonding strength, and each carbon atom can provide an unbonded free electron. This unique structure awakens its high strength and good conductivity. Its strength is as high as 130GPa, and the carrier mobility is 15000cm 2 / (Vs), both of which are the highest among currently known materials. In addition, graphene also has a high surface area and thermal conductivity, as well as unique properties such as molecular, quantum, and tunneling effects. Due to its special two-dimensional structure and excellent performance, graphene still has good advantages in improving the mechanical properties of materials and maintaining the high electrical and thermal conductivity of copper, making it an excellent reinforcement material for copper-based composites. Graphene-enhanced copper-based materials have been widely used in the automotive and aerospace industries.

[0005] However, the wettability between graphene and copper is very poor, resulting in poor interface bonding and reduced material strength. In the preparation process of composite materials, the structure of graphene is often destroyed, and the excellent performance of graphene is strongly dependent on the complete structure. The performance of the graphene composite material obtained is often far from the theoretical value. In addition, the lack of adhesion at the graphene-copper interface and other problems lead to weak interface adhesion, and the mechanical and electrical properties of the metal matrix are reduced due to elastic incompatibility. The uniform dispersion of graphene in the entire metal matrix is ​​a key issue in the preparation of composite materials. Therefore, regulating the interface structure of graphene-copper and improving the problem of weak adhesion at the graphene-copper interface are key issues in improving the performance of graphene-copper composite materials, which is of great significance to the research of composite materials. Summary of the invention

[0006] The present invention provides a method for preparing a highly conductive graphene copper composite material, which comprises the following steps: S1: placing the graphene-coated copper foil into the magnetron sputtering chamber; S2: Using a pure copper target as a copper source, magnetron sputtering is performed on the graphene-coated copper foil, and a layer of copper is sputtered on the surface of the graphene-coated copper foil to produce a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene copper composite material.

[0007] The present invention is further configured as follows: in step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

[0008] The present invention is further configured as follows: in step S2, the thickness of the magnetron sputtered copper is 1-1000 nm, and the magnetron sputtering time is 0.5-60 min; the magnetron sputtering chamber is subjected to vacuum treatment, and the vacuum degree is 2.0×10 -3 Pa-1.0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

[0009] The present invention is further configured as follows: in step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0010] The present invention also proposes a preparation scheme for a highly conductive graphene copper composite material, which is characterized by comprising the following steps: S1: placing the graphene-coated copper foil into an electroplating tank and adding electroplating solution; S2: electroplating the graphene-coated copper foil in step S1 by an electroplating process, depositing a layer of copper on the surface of the graphene-coated copper foil by electroplating to prepare a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

[0011] The present invention is further configured as follows: in step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

[0012] The present invention is further configured as follows: the anode of the electroplating process in step S2 is a pure copper plate, and the cathode is a titanium plate; the current density of the electroplating process in step S2 is 1-50A / dm 2 The electroplating time is 0.5-30min; the copper plating thickness is 1-1000nm, and the electroplating temperature in step S2 is 25-70°C; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

[0013] The present invention is further configured as follows: in step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0014] The present invention also proposes a preparation scheme for a highly conductive graphene copper composite material, which is characterized by comprising the following steps: S1: placing the graphene-coated copper foil into a thermal evaporation chamber; S2: using copper particles or copper wires as copper sources, performing a vapor deposition treatment on the graphene-coated copper foil, vapor-depositing a layer of copper on the surface of the graphene-coated copper foil, and preparing a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

[0015] The present invention is further configured as follows: in step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

[0016] The present invention is further configured as follows: the thickness of the copper layer deposited in step S2 is 1-1000 nm, and the deposition time is 0.5-50 min; the hot evaporation chamber is subjected to vacuum treatment, and the vacuum degree is 1.0×10 -3 Pa-1.0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

[0017] The present invention is further configured as follows: in step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0018] The beneficial effects of the present invention are: 1. Through magnetron sputtering, heat treatment, lamination hot pressing and other steps, a graphene-copper composite material with nearly full density, good graphene-copper interface bonding and ultra-high conductivity can be prepared. In addition, this method has good controllability and is easy to mass produce.

[0019] 2. Through the steps of electroplating, heat treatment, lamination and hot pressing, a graphene-copper composite material with nearly full density, good graphene-copper interface bonding, and ultra-high conductivity can be prepared. In addition, this method has good controllability and is easy to mass produce.

[0020] 3. Through the steps of thermal evaporation, heat treatment, lamination hot pressing and the like, a graphene-copper composite material with nearly full density, good graphene-copper interface bonding and ultra-high conductivity can be prepared. Moreover, this method has good controllability and is easy for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 A process flow chart of Example 1 is shown.

[0022] Figure 2 A process flow diagram for Example 5 is shown.

[0023] Figure 3 A process flow diagram for Example 9 is shown.

[0024] Figure 4 A schematic diagram of the thermal evaporation process of Example 9 is shown. DETAILED DESCRIPTION

[0025] Those skilled in the art can refer to the content of this article and appropriately improve the process parameters. It should be particularly noted that all similar replacements and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0026] Example 1

[0027] This embodiment provides a method for preparing a highly conductive graphene copper composite material, comprising the following steps:

[0028] S1: Place the graphene-coated copper foil into the magnetron sputtering chamber.

[0029] S2: Using pure copper target as copper source, the graphene-coated copper foil is subjected to magnetron sputtering treatment, and a layer of copper is sputtered on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0030] S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil by lamination hot pressing to obtain a highly conductive graphene copper composite material.

[0031] The thickness of the graphene-coated copper foil in step S1 is 10-100 μm.

[0032] The thickness of the magnetron sputtered copper in step S2 is 1-1000 nm, and the magnetron sputtering time is 0.5-60 min; the magnetron sputtering chamber is vacuum treated, and the vacuum degree is 2.0×10-3 Pa-1.0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and sealed in vacuum for storage. It should be noted that the time of magnetron sputtering is determined by the thickness of the copper plating, that is, the thicker the copper plating, the longer the magnetron sputtering time is required.

[0033] In step S3, the temperature in the hot pressing chamber is firstly raised to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and then cooled to room temperature for 20-100 min.

[0034] The hot pressing chamber is first pressurized to 20-120MPa for 20-100min, then kept at constant pressure for 20-100min, and then depressurized to 0Pa for 20-100min. The hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0035] Example 2

[0036] The highly conductive graphene copper composite material was prepared by the method of Example 1. The graphene-coated copper foil and the magnetron sputtering copper target were purchased from outside. The preparation process was as follows:

[0037] S1: Place a graphene-coated copper foil with a thickness of 50 μm into a magnetron sputtering chamber.

[0038] S2: The surface area of ​​the graphene-coated copper foil was subjected to constant-speed magnetron sputtering copper plating using a magnetron sputtering process; a pure copper target with a purity of 99.9999% was used as the copper source, and the vacuum degree of the magnetron sputtering chamber was 5.0×10 -4 Pa, and the magnetron sputtering time is 25 min, so that a layer of copper is sputtered on the surface of the graphene-coated copper foil, and the copper plating thickness is 40 nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0039] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0040] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0041] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a diameter of 50.8 mm and a thickness of 4 mm.

[0042] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0043] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 110.2% IACS.

[0044] Example 3

[0045] The highly conductive graphene copper composite material was prepared by the method of Example 1. The graphene-coated copper foil and the magnetron sputtering copper target were purchased from outside. The preparation process was as follows:

[0046] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a magnetron sputtering chamber.

[0047] S2: The surface area of ​​the graphene-coated copper foil was subjected to constant-speed magnetron sputtering copper plating using a magnetron sputtering process; a pure copper target with a purity of 99.9999% was used as the copper source, and the vacuum degree of the magnetron sputtering chamber was 5.0×10 -4 Pa, and the magnetron sputtering time is 15 min, so that a layer of copper is sputtered on the surface of the graphene-coated copper foil, and the copper plating thickness is 25 nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0048] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0049] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0050] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a diameter of 50.8 mm and a thickness of 4 mm.

[0051] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0052] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 111.9% IACS.

[0053] Example 4

[0054] The highly conductive graphene copper composite material was prepared by the method of Example 1. The graphene-coated copper foil and the magnetron sputtering copper target were purchased from outside. The preparation process was as follows:

[0055] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a magnetron sputtering chamber.

[0056] S2: The surface area of ​​the graphene-coated copper foil was subjected to constant-speed magnetron sputtering copper plating using a magnetron sputtering process; a pure copper target with a purity of 99.9999% was used as the copper source, and the vacuum degree of the magnetron sputtering chamber was 5.0×10 -4 Pa, and the magnetron sputtering time is 35 min, so that a layer of copper is sputtered on the surface of the graphene-coated copper foil, and the copper plating thickness is 50 nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0057] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0058] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0059] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a diameter of 50.8 mm and a thickness of 4 mm.

[0060] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0061] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 108.9% IACS.

[0062] Example 5

[0063] The highly conductive graphene copper composite material was prepared by the method of Example 1. The graphene-coated copper foil and the magnetron sputtering copper target were purchased from outside. The preparation process was as follows:

[0064] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a magnetron sputtering chamber.

[0065] S2: The surface area of ​​the graphene-coated copper foil was subjected to constant-speed magnetron sputtering copper plating using a magnetron sputtering process; a pure copper target with a purity of 99.9999% was used as the copper source, and the vacuum degree of the magnetron sputtering chamber was 5.0×10 -4Pa, and the magnetron sputtering time is 60 min, so that a layer of copper is sputtered on the surface of the graphene-coated copper foil, and the copper plating thickness is 1000 nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0066] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0067] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0068] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a diameter of 50.8 mm and a thickness of 4 mm.

[0069] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa. According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 108.4% IACS.

[0070] Example 6

[0071] The highly conductive graphene copper composite material was prepared by the method of Example 1. The graphene-coated copper foil and the magnetron sputtering copper target were purchased from outside. The preparation process was as follows:

[0072] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a magnetron sputtering chamber.

[0073] S2: The surface area of ​​the graphene-coated copper foil was subjected to constant-speed magnetron sputtering copper plating using a magnetron sputtering process; a pure copper target with a purity of 99.9999% was used as the copper source, and the vacuum degree of the magnetron sputtering chamber was 5.0×10 -4 Pa, and the magnetron sputtering time is 1 min, so that a layer of copper is sputtered on the surface of the graphene-coated copper foil, and the copper plating thickness is 1 nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0074] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0075] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0076] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a diameter of 50.8 mm and a thickness of 4 mm.

[0077] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa. According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 106.7% IACS.

[0078] Example 7

[0079] This embodiment provides a method for preparing a highly conductive graphene copper composite material, comprising the following steps:

[0080] S1: Place the graphene-coated copper foil into an electroplating tank and add electroplating solution.

[0081] S2: electroplating the graphene-coated copper foil in step S1 by an electroplating process, depositing a layer of copper on the surface of the graphene-coated copper foil by electroplating to prepare a copper-plated graphene-coated copper foil.

[0082] S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

[0083] The thickness of the graphene-coated copper foil in step S1 is 10-100 μm.

[0084] The anode of the electroplating process in step S2 is a pure copper plate, the cathode is a titanium plate, and the current density of the electroplating process is 1-50A / dm 2 The electroplating time is 0.5-30min, the electroplating temperature is 25-70°C, and the copper plating thickness is 1-1000nm; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage. It should be noted that the current density, electroplating time and electroplating temperature all depend on the required copper plating thickness and quality.

[0085] In step S3, the temperature in the hot pressing chamber is firstly raised to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and then cooled to room temperature for 20-100 min.

[0086] The hot pressing chamber is first pressurized to 20-120MPa for 20-100min, then kept at constant pressure for 20-100min, and then depressurized to 0Pa for 20-100min. The hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0087] Example 8

[0088] The highly conductive graphene copper composite material was prepared by the method of Example 7. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0089] S1: Place a 50 μm thick graphene-coated copper foil into an electroplating tank and add electroplating solution. The graphene-coated copper foil selected in this embodiment has a length of 100 mm and a width of 80 mm.

[0090] S2: electroplating the graphene-coated copper foil to deposit a layer of copper on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0091] The plating solution temperature was controlled at 30°C and the current density was 15A / dm 2 The electroplating time is 20 minutes, the copper plating thickness is 1 μm, and a copper-plated graphene-coated copper foil is obtained.

[0092] S3: 16 pieces of 20 mm×20 mm graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0093] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0094] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0095] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 108.2% IACS.

[0096] Example 9

[0097] The highly conductive graphene copper composite material was prepared by the method of Example 7. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0098] S1: Place a 50 μm thick graphene-coated copper foil into an electroplating tank and add electroplating solution. The graphene-coated copper foil selected in this embodiment has a length of 100 mm and a width of 80 mm.

[0099] S2: electroplating the graphene-coated copper foil to deposit a layer of copper on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0100] The plating solution temperature was controlled at 25°C and the current density was 10A / dm 2 The electroplating time is 15 minutes, the copper plating thickness is 800 nm, and a copper-plated graphene-coated copper foil is obtained.

[0101] S3: 16 pieces of 20 mm×20 mm graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0102] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0103] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0104] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 107.4% IACS.

[0105] Example 10

[0106] The highly conductive graphene copper composite material was prepared by the method of Example 7. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0107] S1: Place a 50 μm thick graphene-coated copper foil into an electroplating tank and add electroplating solution. The graphene-coated copper foil selected in this embodiment has a length of 100 mm and a width of 80 mm.

[0108] S2: electroplating the graphene-coated copper foil to deposit a layer of copper on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0109] The plating solution temperature was controlled at 25°C and the current density was 10A / dm 2The electroplating time is 1 min, the copper plating thickness is 50 nm, and a copper-plated graphene-coated copper foil is obtained.

[0110] S3: 16 pieces of 20 mm×20 mm graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0111] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0112] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0113] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 108.5% IACS.

[0114] Embodiment 11

[0115] The highly conductive graphene copper composite material was prepared by the method of Example 7. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0116] S1: Place a 50 μm thick graphene-coated copper foil into an electroplating tank and add electroplating solution. The graphene-coated copper foil selected in this embodiment has a length of 100 mm and a width of 80 mm.

[0117] S2: electroplating the graphene-coated copper foil to deposit a layer of copper on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0118] The plating solution temperature was controlled at 25°C and the current density was 5A / dm 2 The electroplating time is 0.5 min, the copper plating thickness is 1 nm, and a copper-plated graphene-coated copper foil is obtained.

[0119] S3: 16 pieces of 20 mm×20 mm graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0120] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0121] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0122] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 104.1% IACS.

[0123] Example 12

[0124] The highly conductive graphene copper composite material was prepared by the method of Example 7. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0125] S1: Place a 50 μm thick graphene-coated copper foil into an electroplating tank and add electroplating solution. The graphene-coated copper foil selected in this embodiment has a length of 100 mm and a width of 80 mm.

[0126] S2: electroplating the graphene-coated copper foil to deposit a layer of copper on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0127] The plating solution temperature was controlled at 50°C and the current density was 40A / dm 2 The electroplating time is 25 minutes, the copper plating thickness is 1000 nm, and a copper-plated graphene-coated copper foil is obtained.

[0128] S3: 16 pieces of 20 mm×20 mm graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0129] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0130] The vacuum degree of the hot pressing chamber in this embodiment is 8.0×10 -4 Pa.

[0131] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 109.2% IACS.

[0132] Embodiment 13

[0133] This embodiment provides a method for preparing a highly conductive graphene copper composite material, comprising the following steps:

[0134] S1: Placing the graphene-coated copper foil into a thermal evaporation chamber.

[0135] S2: Using copper particles or copper wires as copper sources, the graphene-coated copper foil is subjected to vapor deposition treatment, and a layer of copper is vapor deposited on the surface of the graphene-coated copper foil to prepare a copper-plated graphene-coated copper foil.

[0136] S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

[0137] The thickness of the graphene-coated copper foil in step S1 is 10-100 μm.

[0138] The thickness of the copper layer deposited in step S2 is 1-1000 nm, and the deposition time is 0.5-50 min; the hot evaporation chamber is vacuum treated, and the vacuum degree is 1.0×10 -3 Pa-1,0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage. It should be noted that the evaporation time is determined according to the thickness of the copper plating, that is, the thicker the copper plating, the longer the evaporation time required.

[0139] In step S3, the temperature in the hot pressing chamber is firstly raised to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and then cooled to room temperature for 20-100 min.

[0140] The hot pressing chamber is first pressurized to 20-120MPa for 20-100min, then kept at constant pressure for 20-100min, and then depressurized to 0Pa for 20-100min. The hot pressing chamber is maintained in vacuum or filled with argon for protection.

[0141] Embodiment 14

[0142] The method of Example 13 was used to prepare a highly conductive graphene copper composite material. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0143] S1: Place a 50 μm thick graphene-coated copper foil into a thermal evaporation chamber.

[0144] S2: Using the evaporation process, the surface area of ​​the graphene-coated copper foil is subjected to constant-speed thermal evaporation of copper; a copper wire target with a purity of 99.9999% is used as the copper source, and the vacuum degree of the evaporation chamber is 5.0×10 -4 Pa, the evaporation heating current is 50A, and the evaporation time is 25min, so that a layer of copper is evaporated on the surface of the graphene-coated copper foil, and the copper plating thickness is 60nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0145] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0146] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0147] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a length of 15 mm and a diameter of 1 mm.

[0148] The vacuum degree of the hot pressing chamber in this embodiment is 1.0×10 -3 Pa.

[0149] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 112.1% IACS.

[0150] Embodiment 15

[0151] The method of Example 13 was used to prepare a highly conductive graphene copper composite material. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0152] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a thermal evaporation chamber.

[0153] S2: Using the evaporation process, the surface area of ​​the graphene-coated copper foil is subjected to constant-speed thermal evaporation of copper; a copper wire target with a purity of 99.9999% is used as the copper source, and the vacuum degree of the evaporation chamber is 5.0×10 -4 Pa, the evaporation heating current is 50A, and the evaporation time is 15min, so that a layer of copper is evaporated on the surface of the graphene-coated copper foil, and the copper plating thickness is 30nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0154] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0155] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0156] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a length of 15 mm and a diameter of 1 mm.

[0157] The vacuum degree of the hot pressing chamber in this embodiment is 1.0×10 -3 Pa.

[0158] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 108.2% IACS.

[0159] Example 16

[0160] The method of Example 13 was used to prepare a highly conductive graphene copper composite material. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0161] S1: Place a graphene-coated copper foil with a thickness of 25 μm into a thermal evaporation chamber.

[0162] S2: Using the evaporation process, the surface area of ​​the graphene-coated copper foil is subjected to constant-speed thermal evaporation of copper; a copper wire target with a purity of 99.9999% is used as the copper source, and the vacuum degree of the evaporation chamber is 5.0×10 -4 Pa, the evaporation heating current is 50A, and the evaporation time is 15min, so that a layer of copper is evaporated on the surface of the graphene-coated copper foil, and the copper plating thickness is 30nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0163] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 900°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0164] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0165] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a length of 15 mm and a diameter of 1 mm.

[0166] The vacuum degree of the hot pressing chamber in this embodiment is 1.0×10 -3 Pa.

[0167] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 107.9% IACS.

[0168] Embodiment 17

[0169] The method of Example 13 was used to prepare a highly conductive graphene copper composite material. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0170] S1: Place a 50 μm thick graphene-coated copper foil into a thermal evaporation chamber.

[0171] S2: Using the evaporation process, the surface area of ​​the graphene-coated copper foil is subjected to constant-speed thermal evaporation of copper; a copper wire target with a purity of 99.9999% is used as the copper source, and the vacuum degree of the evaporation chamber is 5.0×10 -4 Pa, the evaporation heating current is 50A, and the evaporation time is 0.5min, so that a layer of copper is evaporated on the surface of the graphene-coated copper foil, and the copper plating thickness is 1nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0172] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0173] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0174] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a length of 15 mm and a diameter of 1 mm.

[0175] The vacuum degree of the hot pressing chamber in this embodiment is 1.0×10 -3 Pa.

[0176] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 105.2% IACS.

[0177] Embodiment 18

[0178] The method of Example 13 was used to prepare a highly conductive graphene copper composite material. The graphene-coated copper foil was purchased from outside. The preparation process was as follows:

[0179] S1: Place a 50 μm thick graphene-coated copper foil into a thermal evaporation chamber.

[0180] S2: Using the evaporation process, the surface area of ​​the graphene-coated copper foil is subjected to constant-speed thermal evaporation of copper; a copper wire target with a purity of 99.9999% is used as the copper source, and the vacuum degree of the evaporation chamber is 5.0×10 -4 Pa, the evaporation heating current is 50A, and the evaporation time is 50min, so that a layer of copper is evaporated on the surface of the graphene-coated copper foil, and the copper plating thickness is 1000nm, thereby obtaining a copper-plated graphene-coated copper foil.

[0181] S3: 16 graphene-coated copper foils prepared in step S2 are placed in a vacuum hot pressing chamber for lamination hot pressing. Before hot pressing, the material is heated to 950°C for 40 minutes and kept at a constant temperature for 40 minutes. During this period, hot pressing is performed. After cooling for 40 minutes, the formed high-conductivity graphene-copper composite material is cooled to room temperature.

[0182] During the hot pressing process, the pressing intensity is 50 MPa, the pressing time is 40 min, the constant pressure time is 40 min, and finally the pressure is reduced for 40 min to reduce the pressure to 0 Pa, thereby obtaining a highly conductive graphene copper composite material.

[0183] The graphene-coated copper foil selected in this embodiment has a length of 20 mm and a width of 20 mm. The copper source has a length of 15 mm and a diameter of 1 mm.

[0184] The vacuum degree of the hot pressing chamber in this embodiment is 1.0×10 -3 Pa.

[0185] According to the Van der Pauw method, the electrical properties of the highly conductive graphene copper composite material prepared in step S3 were tested, and the electrical conductivity was 110.3% IACS.

[0186] In summary, the present invention, by the steps such as magnetron sputtering, heat treatment, lamination hot pressing, can prepare a graphene copper composite material close to full density, good graphene copper interface bonding, and ultra-high electrical conductivity, and the method has good controllability, and is easy to large-scale production. By the steps such as electroplating, heat treatment, lamination hot pressing, can prepare a graphene copper composite material close to full density, good graphene copper interface bonding, and ultra-high electrical conductivity, and the method has good controllability, and is easy to large-scale production. By thermal evaporation, heat treatment, the steps such as lamination hot pressing, can prepare a graphene copper composite material close to full density, good graphene copper interface bonding, and ultra-high electrical conductivity, and the method has good controllability, and is easy to large-scale production.

[0187] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be within the scope of protection of the present invention.

Claims

1. A method for preparing a highly conductive graphene copper composite material, characterized in that: The steps include: S1: placing the graphene-coated copper foil into the magnetron sputtering chamber; S2: Using a pure copper target as a copper source, magnetron sputtering is performed on the graphene-coated copper foil, and a layer of copper is sputtered on the surface of the graphene-coated copper foil to produce a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene copper composite material.

2. The method for preparing the highly conductive graphene copper composite material according to claim 1, characterized in that: In step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

3. The method for preparing the highly conductive graphene copper composite material according to claim 1, characterized in that: In step S2, the thickness of the magnetron sputtered copper is 1-1000 nm, and the magnetron sputtering time is 0.5-60 min; the magnetron sputtering chamber is vacuum treated, and the vacuum degree is 2.0×10 -3 Pa-1.0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

4. The method for preparing the highly conductive graphene copper composite material according to claim 1, characterized in that: In step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and then reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

5. A preparation scheme for a highly conductive graphene copper composite material, characterized in that: The steps include: S1: placing the graphene-coated copper foil into an electroplating tank and adding electroplating solution; S2: electroplating the graphene-coated copper foil in step S1 by an electroplating process, depositing a layer of copper on the surface of the graphene-coated copper foil by electroplating to prepare a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

6. The method for preparing the highly conductive graphene copper composite material according to claim 5, characterized in that: In step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

7. The method for preparing the highly conductive graphene copper composite material according to claim 5, characterized in that: The anode of the electroplating process in step S2 is a pure copper plate, and the cathode is a titanium plate; the current density of the electroplating process in step S2 is 1-50A / dm 2 , the electroplating time is 0.5-30min; the electroplating temperature in step S2 is 25-70°C, and the thickness of the copper plating is 1-1000nm; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

8. The method for preparing the highly conductive graphene copper composite material according to claim 5, characterized in that: In step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and then reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

9. A method for preparing a highly conductive graphene copper composite material, characterized in that: The steps include: S1: placing the graphene-coated copper foil into a thermal evaporation chamber; S2: using copper particles or copper wires as copper sources, performing a vapor deposition treatment on the graphene-coated copper foil, vapor-depositing a layer of copper on the surface of the graphene-coated copper foil, and preparing a copper-plated graphene-coated copper foil; S3: placing the copper-plated graphene-coated copper foil prepared in the multilayer step S2 into a hot pressing chamber, setting appropriate hot pressing temperature and pressure, and hot pressing the copper-plated graphene-coated copper foil using a laminated hot pressing method to obtain a highly conductive graphene-copper composite material.

10. The method for preparing the highly conductive graphene copper composite material according to claim 9, characterized in that: In step S1, the thickness of the graphene-coated copper foil is 10-100 μm.

11. The method for preparing the highly conductive graphene copper composite material according to claim 9, characterized in that: The thickness of the copper layer deposited in step S2 is 1-1000 nm, and the deposition time is 0.5-50 min; the hot evaporation chamber is subjected to vacuum treatment, and the vacuum degree is 1.0×10 -3 Pa-1.0×10 -4 Pa; the copper-plated graphene-coated copper foil prepared in step S2 is taken out and vacuum-sealed for storage.

12. The method for preparing the highly conductive graphene copper composite material according to claim 9, characterized in that: In step S3, the temperature in the hot pressing chamber is heated to 600-1100° C. for 20-100 min, then kept at a constant temperature for 20-100 min, and cooled to room temperature after the insulation, and the cooling time is 20-100 min; the pressure in the hot pressing chamber is pressurized to 20-120 MPa for 20-100 min, then kept at a constant pressure for 20-100 min, and then reduced to 0 Pa after the constant pressure is completed, and the decompression time is 20-100 min; the hot pressing chamber is maintained in vacuum or filled with argon for protection.

Citation Information

Patent Citations

  • High-conductivity graphene / copper-based layered composite material and preparation method thereof

    CN106584976A

  • Preparation method of copper / graphene composite material

    CN107697906A

  • Preparation method for graphene-reinforced copper-based composite material

    CN108193065A

  • Preparation method of heat-conducting copper foil graphite composite material

    CN110592543A

  • High-conductivity copper / graphene / copper composite material and preparation method thereof

    CN112962099A

Cited By

  • Interface regulation and control method of graphene copper composite material

    CN119502529A

  • Graphene copper composite wire and preparation method thereof

    CN119581137A

  • Copper-rich graphene ribbon-shaped precursor, method for preparing same and use thereof

    CN122897397A