Preparation method of iron-based amorphous alloy high-hardness coating of hybrid high-entropy alloy
By mixing iron-based amorphous alloy with high-entropy alloy powder and laser cladding, a mixed high-entropy alloy iron-based amorphous coating with significantly improved hardness was prepared, which solved the iron-based amorphous coating during laser cladding. The problem of decreasing hardness achieves high hardness and good bonding force.
Patent Information
- Application Number
- CN202310556750.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-26
AI Technical Summary
During the preparation process, the iron-based amorphous coating has poor coating performance due to the problem of decreasing the hardness of the laser cladding.
The iron-based amorphous alloy Fe41Co7Cr15Mo14C15B6Y2 powder and high-entropy alloy Al0.5CoCrFeNi powder were used to prepare the original powder of laser cladding and laser cladding was carried out through a semiconductor laser to form a high hardness of iron-based amorphous alloy mixed with high entropy alloy. coating.
The hardness of the coating is significantly improved, with an average hardness reaching 1400-1600HV0.2, solving the problem of decreasing laser cladding hardness. The preparation method is simple and suitable for large-scale industrial production.
Smart Images

Figure CN119020771A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of surface engineering technology, and mainly to a method for preparing a high-hardness coating of an iron-based amorphous alloy of a hybrid high-entropy alloy. Background Art
[0002] Amorphous alloy refers to the disordered topological arrangement of atoms in three-dimensional space under solid conditions, which has the characteristics of long-range disorder and short-range order. Compared with traditional crystalline alloys, this special atomic arrangement gives it excellent physical, chemical and mechanical properties. However, the direct application of bulk amorphous alloys as structural materials is limited by the alloy forming size and intrinsic brittleness. Therefore, applying it as an amorphous metal coating to the surface of the material can effectively improve the surface performance of the substrate and give full play to the excellent properties of amorphous alloys. Amorphous metal coatings have been widely used in petrochemical, electric power, marine and nuclear industries.
[0003] Iron-based amorphous materials are widely used in coating materials because of their relatively low price, good corrosion resistance, wear resistance and ultra-high hardness. Iron-based amorphous coatings are often prepared by laser cladding. High temperatures are generated during the laser cladding process. However, the crystallization temperature of iron-based amorphous materials is generally around 600°C. High temperatures will cause large-scale crystallization of iron-based amorphous materials, resulting in a significant decrease in the hardness of the coating. Summary of the invention
[0004] In order to solve the problem of the hardness of the iron-based amorphous coating decreasing due to laser cladding during the preparation process, the present application provides a method for preparing a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy, comprising:
[0005] The iron-based amorphous alloy Fe was mixed by planetary ball mill. 41 Co7Cr 15 Mo 14 C 15 B6Y2 powder and high entropy alloy Al 0.5 CoCrFeNi powder, to obtain the original laser cladding powder;
[0006] After drying the laser cladding raw powder for 2-4 hours, the powder is loaded into a powder feeder, and the surface of the substrate is cleaned to obtain a pre-treated substrate;
[0007] Laser cladding is performed on the pretreated substrate using a semiconductor laser according to laser cladding parameters to obtain a high-hardness iron-based amorphous alloy coating of a mixed high-entropy alloy.
[0008] The laser cladding raw powder prepared above has excellent laser forming and can be directly clad on carbon steel, pipeline steel and other steel materials, and the prepared coating has good bonding strength. The surface of the iron-based amorphous alloy high-hardness coating of the hybrid high-entropy alloy prepared above is smooth, without macro cracks, and the average hardness is 1400-1600HV0.2 , the hardness is greatly improved, solving the problem of the hardness reduction of the iron-based amorphous coating due to laser cladding during the preparation process. And the preparation method in this application is simple and suitable for industrial large-scale production.
[0009] Optionally, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 is 1000~1200HV 0.2 , the high entropy alloy Al 0.5 The average hardness of CoCrFeNi is 250~300HV 0.2 .
[0010] Optionally, in the laser cladding original powder, the high entropy alloy Al 0.5 CoCrFeNi and the Fe-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The mass ratio of B6Y2 is 1:48~50.
[0011] Optionally, the diameter of the large balls of the planetary ball mill is 10 mm, the diameter of the small balls is 6 mm, the ratio of large balls to small balls is 1:2, and the ball-to-material ratio is 2 to 4:1.
[0012] Optionally, the mixing time of the planetary ball mill is 1 hour, wherein the mixture rotates forward for 20 minutes and stops for 10 minutes, and rotates reversely for 20 minutes and stops for 10 minutes, and the rotation speed of the planetary ball mill is 170-230 r / min.
[0013] Optionally, the laser cladding parameters are:
[0014] The laser power is 2000-3000W, the scanning speed is 300-1000mm / min, the powder feeding speed is 20-30g / min, the distance between the laser cladding head and the substrate is 12-15mm, the spot diameter is 2.5-5mm, and three-beam powder feeding is used.
[0015] Optionally, the planetary ball mill mixing process and the laser cladding process are both carried out in an argon protective atmosphere, which can effectively prevent the alloy powder from being oxidized during the cladding process and reduce the content of impurities in the iron-based amorphous alloy powder.
[0016] The present application also provides a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy, which is prepared using any of the methods described above.
[0017] Optionally, the iron-based amorphous alloy high-hardness coating of the hybrid high-entropy alloy has a thickness of 1500-4000 μm, has no macro cracks and has greatly improved hardness.
[0018] The present invention provides a method for preparing a high-hardness coating of an iron-based amorphous alloy of a hybrid high-entropy alloy. 41 Co7Cr 15 Mo 14 C 15 A small amount of high entropy alloy Al is added to the B6Y2 powder 0.5 CoCrFeNi powder is ball-milled and mixed, and laser-clad to prepare the iron-based amorphous alloy high-hardness coating of the mixed high-entropy alloy in this application. The mixed powder prepared in this application has excellent laser forming and can be directly clad on steels such as carbon steel and pipeline steel, and the prepared coating has good interface bonding strength. The present application also provides an iron-based amorphous alloy high-hardness coating of a mixed high-entropy alloy prepared by the above method, the surface of the layer is smooth, there are no macro cracks, and the hardness is greatly improved. A method for solving the problem of the decrease in hardness of iron-based amorphous coatings due to laser cladding during the preparation process is provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solution of the present application, the drawings required for use in the embodiments are briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0020] Figure 1 Schematic diagrams of the appearance of iron-based amorphous powder, high entropy alloy powder and mixed powder, Figure a is iron-based amorphous alloy powder, Figure b is high entropy alloy powder, and Figure c is mixed powder;
[0021] Figure 2 XRD patterns of high entropy alloy powder, iron-based amorphous powder and amorphous powder of hybrid high entropy alloy;
[0022] Figure 3 The graph is a micro-Vickers hardness measurement result graph of the iron-based amorphous coating and the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy;
[0023] Figure 4 SEM micrograph of the microhardness of the mixed powder coating. DETAILED DESCRIPTION
[0024] The following embodiments are described in detail, and examples thereof are shown in the accompanying drawings. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The implementations described in the following embodiments do not represent all implementations consistent with the present application. They are only examples of systems and methods consistent with some aspects of the present application as detailed in the claims.
[0025] Embodiment 1:
[0026] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0027] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0028] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1000HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 250HV 0.2 .
[0029] For macroscopic morphology, see Figure 1 The iron-based amorphous powder and macroscopic morphology shown in Figure a are shown in Figure 1 The high entropy alloy powder described in Figure b is placed in a planetary ball mill at a mass ratio of 49:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 3:1. The ball mill is placed together in a ball mill, and the ball mill is evacuated and then injected with argon gas.
[0030] The ball mill was mixed for 60 min, wherein the forward rotation was 20 min and the rest was 10 min, and the reverse rotation was 20 min and the rest was 10 min, and the rotation speed was 200 r / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was dried for 3 h to obtain the original laser cladding powder. The macroscopic morphology of the original laser cladding powder can be seen in Figure 1 As shown in Figure c. Figure 1As can be seen from Figure c, the mixed powder is relatively uniform without clustering. The XRD spectra of high entropy alloy powder, iron-based amorphous powder and mixed high entropy alloy amorphous powder are as follows Figure 2 shown.
[0031] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing distance from substrate height 12.5mm, laser spot diameter 2.5mm, laser scanning speed 300mm / min, laser power 3000W, powder feeding speed 20g / min, three-beam powder feeding, and protective argon gas flow rate 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 4000μm.
[0032] The Vickers hardness distribution curves of the iron-based amorphous alloy high hardness coating and the iron-based amorphous coating of the hybrid high entropy alloy prepared above were tested, and the results were as follows Figure 3 As shown. Figure 3 It can be seen that the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy of the present invention is divided into three regions: a coating high hardness region, a coating dendrite hardness region, and a substrate low hardness region. The coating with the addition of high entropy alloy is much harder than the iron-based amorphous coating.
[0033] Figure 4 This is a scanning electron microscope photo of the microhardness of the amorphous coating of the hybrid high entropy alloy. There are no macro cracks in the coating, and the maximum microhardness is measured to be 1680.1HV 0.2 , the average hardness is 1519.3±35.7HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 38.7% higher than that of the ordinary iron-based amorphous coating.
[0034] Embodiment 2:
[0035] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0036] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0037] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1200HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 300HV 0.2 .
[0038] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 50:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed together in a ball mill, and the ball mill is evacuated and then injected with argon.
[0039] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 170 r / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0040] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy. The specific process parameters of laser cladding are: laser focusing distance substrate height 12mm, laser spot diameter 3mm, laser scanning speed 300mm / min, laser power 2000W, powder feeding speed 20g / min, three-beam powder feeding, protective argon gas flow rate 15L / min. The thickness of the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy with excellent surface performance prepared by the above method is 3500μm.
[0041] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1542HV 0.2 , the average hardness is 1429.3±25.4HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 30.5% higher than that of the ordinary iron-based amorphous coating.
[0042] Embodiment three:
[0043] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0044] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0045] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1150HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 270HV 0.2 .
[0046] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 48:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed together in a ball mill, and the ball mill is evacuated and then injected with argon.
[0047] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 230 r / min. After the mixing was completed, the mixture was dried for 2.5 h to obtain an amorphous powder of the hybrid high entropy alloy, i.e., the original powder for laser cladding.
[0048] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing height of 15mm from the substrate, laser spot diameter of 5mm, laser scanning speed of 1000mm / min, laser power of 3000W, powder feeding speed of 30g / min, three-beam powder feeding, and protective argon gas flow rate of 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 1500μm.
[0049] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1785HV 0.2 , the average hardness is 1584.3±26.4HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 44.6% higher than that of the ordinary iron-based amorphous coating.
[0050] Embodiment 4:
[0051] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0052] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0053] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1175HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 268HV 0.2 .
[0054] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 49:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed in a ball mill jar, which is evacuated and then injected with argon gas.
[0055] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 220 / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0056] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing height from substrate 13.5mm, laser spot diameter 4.3mm, laser scanning speed 800mm / min, laser power 2540W, powder feeding speed 26g / min, three-beam powder feeding, and protective argon gas flow rate 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 2050μm.
[0057] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1580.5HV 0.2 , the average hardness is 1467.3±36.5HV0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 34.0% higher than that of the ordinary iron-based amorphous coating.
[0058] Embodiment five:
[0059] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0060] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0061] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1160HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 285HV 0.2 .
[0062] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 49:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed in a ball mill jar, which is evacuated and then injected with argon gas.
[0063] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 190 r / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0064] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing height of 14.6mm from the substrate, laser spot diameter of 3.6mm, laser scanning speed of 450mm / min, laser power of 2685W, powder feeding speed of 26g / min, three-beam powder feeding, and protective argon gas flow rate of 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 2600μm.
[0065] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1594.6HV 0.2 , the average hardness is 1459.3±35.9HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 33.2% higher than that of the ordinary iron-based amorphous coating.
[0066] Embodiment six:
[0067] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0068] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0069] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1156HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 268HV 0.2 .
[0070] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 49:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 3:1. The ball mill is placed together in a ball milling jar, and the ball milling jar is evacuated and then injected with argon gas.
[0071] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 220 / min. After the mixing was completed, the amorphous powder of the hybrid high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0072] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing height from substrate 13.6mm, laser spot diameter 4.2mm, laser scanning speed 700mm / min, laser power 2550W, powder feeding speed 27g / min, three-beam powder feeding, and protective argon gas flow rate 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 2300μm.
[0073] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1689.4HV 0.2 , the average hardness is 1559.3±28.4HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 42.3% higher than that of the ordinary iron-based amorphous coating.
[0074] Embodiment seven:
[0075] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0076] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0077] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 powder is 1135HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 276HV 0.2 .
[0078] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 48:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed together in a ball mill, and the ball mill is evacuated and then injected with argon.
[0079] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 210 r / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0080] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy. The specific process parameters of laser cladding are: laser focusing height of 12.6mm from the substrate, laser spot diameter of 4mm, laser scanning speed of 800mm / min, laser power of 3000W, powder feeding speed of 30g / min, three-beam powder feeding, and protective argon gas flow rate of 15L / min. The thickness of the iron-based amorphous alloy high-hardness coating of a hybrid high-entropy alloy with excellent surface performance prepared by the above method is 3200μm.
[0081] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1687.6HV 0.2 , the average hardness is 1569.3±24.7HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 43.3% higher than that of the ordinary iron-based amorphous coating.
[0082] Embodiment eight:
[0083] The preparation method of the iron-based amorphous alloy coating of this embodiment is as follows:
[0084] No. 45 steel with a size of 200mm×200mm×10mm was selected as the substrate; the substrate surface oxide was removed by sandpaper polishing; the substrate surface was cleaned by anhydrous ethanol ultrasonic cleaning to remove the grinding debris and oil stains, thereby obtaining a pretreated substrate.
[0085] The composition and atomic percentage of the original powder are as follows: Fe 41 Co7Cr 15 Mo 14 C 15 B6Y2 (atomic percentage) is composed of seven elements. High entropy alloy powder is composed of Al 0.5 CoCrFeNi (atomic percentage) is composed of five elements. Among them, the iron-based amorphous alloy Fe 41 Co7Cr 15 Mo14 C 15 The average hardness of B6Y2 powder is 1154HV 0.2 , high entropy alloy Al 0.5 The average hardness of CoCrFeNi powder is 286HV 0.2 .
[0086] The iron-based amorphous powder and the high entropy alloy powder are placed in a planetary ball mill at a mass ratio of 49:1. The large balls of the planetary ball mill have a diameter of 10 mm, the small balls have a diameter of 6 mm, the large balls and small balls have a ratio of 1:2, and the ball-to-material ratio is 4:1. The ball mill is placed in a ball mill jar, which is evacuated and then injected with argon gas.
[0087] The ball milling was performed for 60 min, including 20 min forward rotation and 10 min rest, and 20 min reverse rotation and 10 min rest, with a rotation speed of 205 r / min. After the mixing was completed, the amorphous powder of the mixed high entropy alloy was obtained, that is, the original powder of the laser cladding.
[0088] The prepared laser cladding raw powder is introduced into the powder feeding equipment, and laser cladding is performed on the pretreated substrate to prepare the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy. The specific process parameters of laser cladding are: laser focusing height of 14.5mm from the substrate, laser spot diameter of 5mm, laser scanning speed of 600mm / min, laser power of 3000W, powder feeding speed of 25g / min, three-beam powder feeding, and protective argon gas flow rate of 15L / min. The thickness of the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy with excellent surface performance prepared by the above method is 1500μm.
[0089] There are no macro cracks in the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy prepared above, and the maximum microhardness is measured to be 1653.5HV 0.2 , the average hardness is 1459.3±28.7HV 0.2 The hardness of the amorphous coating of the hybrid high entropy alloy is 33.2% higher than that of the ordinary iron-based amorphous coating.
[0090] Similar parts between the embodiments provided in this application can be referenced to each other. The specific implementation methods provided above are only a few examples under the general concept of this application and do not constitute a limitation on the protection scope of this application. For those skilled in the art, any other implementation methods expanded based on the scheme of this application without creative work belong to the protection scope of this application.
Claims
1. A method for preparing a high-hardness iron-based amorphous alloy coating of a hybrid high-entropy alloy, characterized in that: include: The iron-based amorphous alloy Fe was mixed by planetary ball mill. 41 Co7Cr 15 Mo 14 C 15 B6Y2 powder and high entropy alloy Al 0.5 CoCrFeNi powder, to obtain the original laser cladding powder; After drying the laser cladding raw powder for 2-4 hours, the powder is loaded into a powder feeder, and the surface of the substrate is cleaned to obtain a pre-treated substrate; Laser cladding is performed on the pre-treated substrate using a semiconductor laser according to laser cladding parameters to obtain a high-hardness iron-based amorphous alloy coating of a mixed high-entropy alloy.
2. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 1, characterized in that: The iron-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The average hardness of B6Y2 is 1000~1200HV 0.2 , the high entropy alloy Al 0.5 The average hardness of CoCrFeNi is 250~300HV 0.2 .
3. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 2, characterized in that: In the laser cladding original powder, the high entropy alloy Al 0.5 CoCrFeNi and the Fe-based amorphous alloy Fe 41 Co7Cr 15 Mo 14 C 15 The mass ratio of B6Y2 is 1:48~50.
4. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 1, characterized in that: The diameter of the large ball of the planetary ball mill is 10 mm, the diameter of the small ball is 6 mm, the ratio of the large ball to the small ball is 1:2, and the ball-to-material ratio is 2-4:
1.
5. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 4, characterized in that: The mixing time of the planetary ball mill is 1 hour, including 20 minutes of forward rotation and 10 minutes of rest, and 20 minutes of reverse rotation and 10 minutes of rest. The rotation speed of the planetary ball mill is 170-230 r / min.
6. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 1, characterized in that: The laser cladding parameters are: The laser power is 2000-3000W, the scanning speed is 300-1000mm / min, the powder feeding speed is 20-30g / min, the distance between the laser cladding head and the substrate is 12-15mm, the spot diameter is 2.5-5mm, and three-beam powder feeding is used.
7. The method for preparing the iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 1, characterized in that: The mixing process using the planetary ball mill and the laser cladding process are both carried out in an argon protective atmosphere.
8. An iron-based amorphous alloy high hardness coating of a hybrid high entropy alloy, characterized in that: The coating is prepared by the method according to any one of claims 1 to 7.
9. The iron-based amorphous alloy high hardness coating of the hybrid high entropy alloy according to claim 8, characterized in that: The thickness of the coating is 1500-4000 μm.
Citation Information
Cited By
Magnetic field assisted superspeed laser cladding high-entropy amorphous coating and preparation method thereof
CN121087483A
Magnetic field assisted ultra-high speed laser cladding high-entropy amorphous coating and preparation method
CN121087483B
High-entropy amorphous coating material containing refractory particles as well as preparation method and application of high-entropy amorphous coating material