A multi-core prefabricated end circular lead-in optical cable
By improving the sheathing material and adding lubricating layers of the optical cable, the problem of poor bending and tensile resistance of existing fiber connectors is solved, the bending resistance and tensile strength of the optical cable is improved, the service life is extended and the service life is enhanced Reliability.
Patent Information
- Application Number
- CN202411379204.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The existing fiber optic connectors have poor bending and tensile resistance after insertion, resulting in insufficient reliability and affecting the communication performance and service life of the fiber.
The multi-core prefabricated end circular introduction optical cable is used to improve the material components of the inner sheath and outer sheath, and a lubricating layer is installed in the optical cable to improve the bending resistance and tensile strength of the optical cable, avoiding the sheath in the optical fiber. The connector is broken.
It improves the bending and tensile resistance of the optical cable, enhances the service life of the optical cable, and ensures the reliability and communication performance of the optical fiber connector.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of communication optical cable manufacturing, and in particular relates to a multi-core prefabricated terminated circular lead-in optical cable. Background Art
[0002] With the rapid development of optical communication networks and the continuous increase in broadband services, people's requirements for information transmission are getting higher and higher, and operators' demand for network transmission capacity is constantly increasing. Multi-core prefabricated terminated circular introduction optical cable is a new type of user access optical cable. Prefabricated termination components are generally used as connectors for optical cable connection. The two end faces of the optical fiber are precisely connected to maximize the coupling of the light energy output by the transmitting optical fiber to the receiving optical fiber. However, the optical fiber connector has poor bending and tensile resistance after mating, and its reliability is insufficient, which has a very large impact on the communication performance and service life of the optical fiber.
[0003] Existing fiber optic connectors include a connector body, a tail sheath, and an outer sheath. The sheath layer is stripped off the end of the optical cable near its end and inserted into the connector body. The two sections of optical fiber are connected by plugging different connector bodies. However, the tensile performance of the fiber optic connector after plugging is poor, and the internal reliability of the fiber optic connection node is also insufficient, which has a direct impact on the electrical communication performance and service life of the optical fiber. Summary of the invention
[0004] The structure of the circular introduction optical cable of the present invention basically includes the introduction optical cable including the circular introduction optical cable and the optical fiber connector. The optical fiber connector includes a fixing buckle, a supporting tube, a fixing head cover and a ceramic ferrule. The fixing buckle and the fixing head cover are respectively arranged at the two ends of the supporting tube, and buckles are respectively arranged on both sides of the fixing head cover. The ceramic ferrule is arranged at the front end of the fixing head cover. The optical cable passes through the fixing buckle, the supporting tube and the fixing head cover in sequence and is connected to the ceramic ferrule. The optical cable is fixed to the movable connection plug through the fixing buckle. Since the ferrule and the optical fiber connector are directly riveted together, when the optical cable is stretched and twisted, the position where the optical cable is connected to the connector will face large deformation and deformation stress. Once the sheath material is broken, it will involve the ferrule in the connector, affecting the optical performance of the connector.
[0005] In order to solve the above situation, the present invention provides a multi-core prefabricated terminated circular introduction optical cable, including a circular introduction optical cable and an optical fiber connector connected to the end of the circular introduction optical cable. The circular introduction optical cable includes a multi-core optical fiber, an inner sheath, a lubricating layer and an outer sheath. By improving the material components of the inner sheath and the outer sheath and providing the lubricating layer, the bending resistance and tensile strength of the optical cable are improved, and the optical cable sheath is prevented from breaking at the optical fiber connector position, thereby increasing the service life of the introduction optical cable.
[0006] The specific plan is as follows:
[0007] A multi-core prefabricated terminated circular lead-in optical cable, the optical cable comprising a multi-core optical fiber, an inner sheath, a lubricating layer and an outer sheath, wherein the inner sheath, the lubricating layer and the outer sheath are sequentially coated on the outer side of the multi-core optical fiber in order from inside to outside;
[0008] The inner sheath comprises styrene-butadiene rubber in parts by mass; the outer sheath comprises: 40-50 parts of high-density polyethylene; 30-35 parts of low-density polyethylene; 6-8 parts of ultra-high molecular weight polyethylene, 15-20 parts of ethylene-propylene rubber, 25-30 parts of hydrogenated styrene-butadiene block copolymer, 15-18 parts of carbon fiber filler, 5-10 parts of N,N'-methylene bis stearamide and 3-5 parts of antioxidant in parts by mass; wherein the carbon fiber filler is prepared by the following method:
[0009] (1) Graphite particles are mixed with carbon fibers, placed in a closed heating furnace, a mixed gas of oxygen and water vapor is introduced, heated and kept warm for surface oxidation, taken out, and then placed in hydrochloric acid, heated and kept warm for surface activation;
[0010] (2) adding the product of step 1 to a n-butanol solution containing zirconium n-butoxide, adding acetic acid, hydrolyzing, and then placing in a heating furnace for sintering;
[0011] (3) adding the product of step 2 to a dopamine aqueous solution, then adding tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine, adding dilute hydrochloric acid to adjust the pH value of the mixed solution for surface modification, then placing it as an anode and graphite as a cathode in a salt solution, applying current, and performing electrochemical anodic oxidation;
[0012] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, heated, and then added to a toluene solution containing polyethylene glycol, dibutyltin dilaurate is added, and heated for surface modification to obtain a carbon fiber filler.
[0013] Furthermore, the inner sheath comprises, in parts by mass: 50-55 parts of styrene-butadiene rubber, 25-30 parts of ethylene-vinyl acetate copolymer, 15-20 parts of hydrogenated styrene-butadiene block copolymer, 8-10 parts of glyceryl monostearate, 6-8 parts of dibenzothiazole disulfide, 3-5 parts of diisopropylbenzene peroxide, and 3-5 parts of antioxidant.
[0014] Furthermore, the lubricating layer comprises, by weight: 50-60 parts of polyvinyl alcohol, 20-25 parts of polyacrylonitrile, 20-25 parts of polyethylene glycol, 15-20 parts of polyvinyl pyrrolidone, 8-10 parts of nano aluminum hydroxide, 8-10 parts of nano zinc borate, 3-5 parts of plasticizer and 2-4 parts of sodium polyacrylate.
[0015] Furthermore, the carbon fiber filler is prepared by the following method:
[0016] (1) Graphite particles with a diameter of 0.5-1 micron and carbon fibers with a length of 100-150 microns are mixed in a mass ratio of 1:2-4, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60-75% by volume, heated to 110-130°C and kept warm for 2-4 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0-1.5 mol / L, heated to 60-80°C and kept warm for 1-3 hours, filtered, washed, and dried;
[0017] (2) adding the product of step 1 to a n-butanol solution containing 2-4 wt% zirconium n-butoxide, heating to 70-80°C, adding acetic acid, keeping warm for 5-10 hours, filtering, washing, drying, placing in a heating furnace, heating to 750-800°C and keeping warm for 3-5 hours;
[0018] (3) adding the product of step 2 to an aqueous solution containing 15-20 wt% dopamine, then adding tris(hydroxymethyl)aminomethane in an amount equal to that of dopamine, adding dilute hydrochloric acid to adjust the pH value of the mixed solution to 7.6-8.0, heating to 50°C for 10-15 min, washing, drying, using it as an anode and graphite as a cathode, placing it in an ammonium bicarbonate solution with a concentration of 4-6 wt%, applying a current of 2-4 mA / cm2 for 2-6 min, and performing electrochemical anodic oxidation;
[0019] (4) The product of step 3 is placed in a mixed solution of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75-80°C, maintained for 6-12 hours, filtered and washed; then added to a toluene solution containing 15-20wt% polyethylene glycol, dibutyltin dilaurate is added in an amount of 3-5wt%, heated to 75-85°C, maintained for 1-2 hours, and finally filtered, washed and dried to obtain the carbon fiber filler.
[0020] Furthermore, the plasticizer is selected from one or a combination of dibutyl phthalate, dimethyl phthalate, diethyl phthalate, dioctyl phthalate, dicyclohexyl phthalate, and diisobutyl phthalate.
[0021] Furthermore, the antioxidant is selected from one or more of antioxidant 1010, antioxidant 168, antioxidant 245, and antioxidant 264.
[0022] Compared with the prior art, the beneficial effects of the present invention are:
[0023] 1) The graphite particles and carbon fiber surfaces are oxidized with an oxidant, and then the surface is modified with zirconium oxide. At the same time, after being coated with dopamine, anodization is performed to dope nitrogen on the surface of the carbon fiber to form partial zirconium nitride and zirconium oxynitride, thereby improving the wear resistance of the sheath layer. At the same time, it can greatly improve the mechanical strength of the carbon fiber, thereby improving the sheath's performance in resisting stretching, torsion, and deformation.
[0024] 2) When coated with polyethylene glycol, graphite particles and carbon fibers can improve their affinity with other organic materials, thereby improving their dispersion performance. Graphite particles and carbon fibers will also aggregate and combine to form a fiber structure with protrusions, or form a local star network structure with particles as fiber convergence connection points, thereby improving the anchoring effect of the fiber in the polymer material, thereby improving the positional stability of the carbon fiber filler in the sheath material, thereby improving the bending resistance of the sheath material.
[0025] 3) The inner sheath is made of a material with higher elasticity, and a lubricating layer is added between the inner sheath and the outer sheath, thereby reducing the stress concentration between the inner and outer layers, improving the bending resistance of the sheath material, and increasing the service life. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific embodiments. In the present invention, the antioxidant used is antioxidant 1010 produced by BASF of Germany, and the plasticizer used is dibutyl phthalate produced by Guangdong Yuanda New Materials. However, the protection scope of the present invention is not limited to the following embodiments. Any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.
[0027] Example 1
[0028] The carbon fiber filler is prepared by the following method:
[0029] (1) Graphite particles with a diameter of 0.5 micrometers and carbon fibers with a length of 100 micrometers are mixed in a mass ratio of 1:2, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60% by volume, heated to 110°C and kept warm for 2 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0 mol / L, heated to 60°C and kept warm for 1 hour, filtered, washed, and dried;
[0030] (2) adding the product of step 1 to a n-butanol solution containing 2 wt% zirconium n-butoxide, heating to 70°C, adding acetic acid, keeping the temperature for 5 hours, filtering, washing, drying, placing in a heating furnace, heating to 750°C and keeping the temperature for 3 hours;
[0031] (3) The product of step 2 was added to an aqueous solution containing 15 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.6, and the mixture was heated to 50°C for 10 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in an ammonium bicarbonate solution with a concentration of 4 wt% and an applied density of 2 mA / cm 2 The current lasted for 2 min to carry out electrochemical anodization;
[0032] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75°C, maintained for 6 hours, filtered and washed; then added to a toluene solution containing 15wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 3wt%, heated to 75°C, maintained for 1 hour, and finally filtered, washed and dried to obtain the product.
[0033] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0034] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0035] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0036] Example 2
[0037] The carbon fiber filler is prepared by the following method:
[0038] (1) Graphite particles with a diameter of 0.7 micrometers and carbon fibers with a length of 120 micrometers were mixed in a mass ratio of 1:3, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor was introduced, wherein the oxygen content was 65% by volume, heated to 120°C and kept warm for 3 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.2 mol / L, heated to 70°C and kept warm for 2 hours, filtered, washed, and dried;
[0039] (2) adding the product of step 1 to a n-butanol solution containing 3 wt% zirconium n-butoxide, heating to 75°C, adding acetic acid, keeping the temperature for 7 hours, filtering, washing, drying, placing in a heating furnace, heating to 770°C and keeping the temperature for 4 hours;
[0040] (3) The product of step 2 was added to an aqueous solution containing 17 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.8, and the mixture was heated to 55°C for 12 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in an ammonium bicarbonate solution with a concentration of 5 wt% and an applied density of 3 mA / cm 2 The current was 3 min for electrochemical anodic oxidation.
[0041] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 77°C, maintained for 8 hours, filtered and washed; then added to a toluene solution containing 17wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 4wt%, heated to 80°C, maintained for 1.5 hours, and finally filtered, washed and dried to obtain the product.
[0042] The inner sheath comprises, by mass, 52 parts of styrene-butadiene rubber, 27 parts of ethylene-vinyl acetate copolymer, 16 parts of hydrogenated styrene-butadiene block copolymer, 9 parts of glyceryl monostearate, 7 parts of dibenzothiazole disulfide, 4 parts of diisopropylbenzene peroxide, and 4 parts of antioxidant.
[0043] The lubricating layer comprises, by weight: 53 parts of polyvinyl alcohol, 22 parts of polyacrylonitrile, 22 parts of polyethylene glycol, 17 parts of polyvinyl pyrrolidone, 9 parts of nano aluminum hydroxide, 9 parts of nano zinc borate, 4 parts of plasticizer and 3 parts of sodium polyacrylate;
[0044] The outer sheath comprises, by mass: 44 parts of high-density polyethylene; 32 parts of low-density polyethylene; 7 parts of ultra-high molecular weight polyethylene, 17 parts of ethylene-propylene rubber, 27 parts of hydrogenated styrene-butadiene block copolymer, 16 parts of carbon fiber filler, 6 parts of N,N'-methylene bisstearamide and 4 parts of antioxidant.
[0045] Example 3
[0046] The carbon fiber filler is prepared by the following method:
[0047] (1) Graphite particles with a diameter of 0.8 μm and carbon fibers with a length of 140 μm were mixed in a mass ratio of 1:3, placed in a closed heating furnace, introduced with a mixed gas of oxygen and water vapor, wherein the oxygen content was 72% by volume, heated to 120°C and kept warm for 3 h, taken out, and then placed in hydrochloric acid with a concentration of 1.4 mol / L, heated to 70°C and kept warm for 2 h, filtered, washed, and dried;
[0048] (2) adding the product of step 1 to a n-butanol solution containing 3 wt% zirconium n-butoxide, heating to 75°C, adding acetic acid, keeping the temperature for 8 hours, filtering, washing, drying, placing in a heating furnace, heating to 780°C and keeping the temperature for 4 hours;
[0049] (3) The product of step 2 was added to an aqueous solution containing 18 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.8, and the mixture was heated to 50°C for 12 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in a 5 wt% ammonium bicarbonate solution at a density of 3 mA / cm 2 The current was 5 min for electrochemical anodic oxidation.
[0050] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 78°C, maintained for 10 hours, filtered and washed; then added to a toluene solution containing 18wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 4wt%, heated to 82°C, maintained for 1.5 hours, and finally filtered, washed and dried to obtain the product.
[0051] The inner sheath comprises, by mass, 54 parts of styrene-butadiene rubber, 28 parts of ethylene-vinyl acetate copolymer, 18 parts of hydrogenated styrene-butadiene block copolymer, 9 parts of glyceryl monostearate, 7 parts of dibenzothiazole disulfide, 4 parts of diisopropylbenzene peroxide, and 4 parts of antioxidant.
[0052] The lubricating layer comprises, by weight: 58 parts of polyvinyl alcohol, 24 parts of polyacrylonitrile, 24 parts of polyethylene glycol, 18 parts of polyvinyl pyrrolidone, 9 parts of nano aluminum hydroxide, 9 parts of nano zinc borate, 4 parts of plasticizer and 3 parts of sodium polyacrylate;
[0053] The outer sheath comprises, by mass: 48 parts of high-density polyethylene; 34 parts of low-density polyethylene; 7 parts of ultra-high molecular weight polyethylene, 18 parts of ethylene-propylene rubber, 28 parts of hydrogenated styrene-butadiene block copolymer, 17 parts of carbon fiber filler, 8 parts of N,N'-methylene bisstearamide and 4 parts of antioxidant.
[0054] Example 4
[0055] The carbon fiber filler is prepared by the following method:
[0056] (1) Graphite particles with a diameter of 1 micron and carbon fibers with a length of 150 microns were mixed in a mass ratio of 1:4, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor was introduced, wherein the oxygen content was 75% by volume, heated to 130°C and kept warm for 4 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.5 mol / L, heated to 80°C and kept warm for 3 hours, filtered, washed, and dried;
[0057] (2) adding the product of step 1 to a n-butanol solution containing 4 wt% zirconium n-butoxide, heating to 80°C, adding acetic acid, keeping the temperature for 10 hours, filtering, washing, drying, placing in a heating furnace, heating to 800°C and keeping the temperature for 5 hours;
[0058] (3) adding the product of step 2 to an aqueous solution containing 20 wt% dopamine, then adding tris(hydroxymethyl)aminomethane in an amount equal to that of dopamine, adding dilute hydrochloric acid to adjust the pH value of the mixed solution to 8.0, heating to 60°C for 15 min, washing, drying, using it as an anode and graphite as a cathode, placing it in a 6 wt% ammonium bicarbonate solution, applying a current of 4 mA / cm2 for 6 min, and performing electrochemical anodic oxidation;
[0059] (4) The product of step 3 is placed in a mixed solution of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 80°C, maintained for 12 hours, filtered and washed; then added to a toluene solution containing 20wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 5wt%, heated to 85°C, maintained for 2 hours, and finally filtered, washed and dried to obtain the product.
[0060] The inner sheath comprises, by mass, 55 parts of styrene-butadiene rubber, 30 parts of ethylene-vinyl acetate copolymer, 20 parts of hydrogenated styrene-butadiene block copolymer, 10 parts of glyceryl monostearate, 8 parts of dibenzothiazole disulfide, 5 parts of diisopropylbenzene peroxide, and 5 parts of antioxidant.
[0061] The lubricating layer comprises, by weight: 60 parts of polyvinyl alcohol, 25 parts of polyacrylonitrile, 25 parts of polyethylene glycol, 20 parts of polyvinyl pyrrolidone, 10 parts of nano aluminum hydroxide, 10 parts of nano zinc borate, 5 parts of plasticizer and 4 parts of sodium polyacrylate;
[0062] The outer sheath comprises, by mass: 50 parts of high-density polyethylene; 35 parts of low-density polyethylene; 8 parts of ultra-high molecular weight polyethylene, 20 parts of ethylene-propylene rubber, 30 parts of hydrogenated styrene-butadiene block copolymer, 18 parts of carbon fiber filler, 10 parts of N,N'-methylene bisstearamide and 5 parts of antioxidant.
[0063] Comparative Example 1
[0064] The carbon fiber filler is commercially available carbon fiber with a length of 100 μm;
[0065] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0066] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0067] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0068] Comparative Example 2
[0069] The carbon fiber filler is prepared by the following method:
[0070] (1) Place a carbon fiber with a length of 100 microns in a closed heating furnace, introduce a mixed gas of oxygen and water vapor, wherein the oxygen content is 60% by volume, heat to 110°C and keep warm for 2 hours, take it out, and then place it in hydrochloric acid with a concentration of 1.0 mol / L, heat to 60°C and keep warm for 1 hour, filter, wash, and dry;
[0071] (2) adding the product of step 1 to a n-butanol solution containing 2 wt% zirconium n-butoxide, heating to 70°C, adding acetic acid, keeping the temperature for 5 hours, filtering, washing, drying, placing in a heating furnace, heating to 750°C and keeping the temperature for 3 hours;
[0072] (3) The product of step 2 was added to an aqueous solution containing 15 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.6, and the mixture was heated to 50°C for 10 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in an ammonium bicarbonate solution with a concentration of 4 wt% and an applied density of 2 mA / cm 2 The current lasted for 2 min to carry out electrochemical anodization;
[0073] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75°C, maintained for 6 hours, filtered and washed; then added to a toluene solution containing 15wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 3wt%, heated to 75°C, maintained for 1 hour, and finally filtered, washed and dried to obtain the product.
[0074] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0075] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0076] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0077] Comparative Example 3
[0078] The carbon fiber filler is prepared by the following method:
[0079] (1) Graphite particles with a diameter of 0.5 micrometers and carbon fibers with a length of 100 micrometers are mixed in a mass ratio of 1:2, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60% by volume, heated to 110°C and kept warm for 2 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0 mol / L, heated to 60°C and kept warm for 1 hour, filtered, washed, and dried;
[0080] (2) The product of step 1 was added to an aqueous solution containing 15 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.6, and the mixture was heated to 50°C for 10 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in an ammonium bicarbonate solution with a concentration of 4 wt% and an applied density of 2 mA / cm 2 The current lasted for 2 min to carry out electrochemical anodization;
[0081] (3) The product of step 2 is placed in a mixed solution of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75°C, maintained for 6 hours, filtered and washed; then added to a toluene solution containing 15wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 3wt%, heated to 75°C, maintained for 1 hour, and finally filtered, washed and dried to obtain the product.
[0082] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0083] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0084] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0085] Comparative Example 4
[0086] The carbon fiber filler is prepared by the following method:
[0087] (1) Graphite particles with a diameter of 0.5 micrometers and carbon fibers with a length of 100 micrometers are mixed in a mass ratio of 1:2, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60% by volume, heated to 110°C and kept warm for 2 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0 mol / L, heated to 60°C and kept warm for 1 hour, filtered, washed, and dried;
[0088] (2) adding the product of step 1 to a n-butanol solution containing 2 wt% zirconium n-butoxide, heating to 70°C, adding acetic acid, keeping the temperature for 5 hours, filtering, washing, drying, placing in a heating furnace, heating to 750°C and keeping the temperature for 3 hours;
[0089] (3) The product of step 2 is placed in a mixed solution of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75°C, maintained for 6 hours, filtered and washed; then added to a toluene solution containing 15wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 3wt%, heated to 75°C, maintained for 1 hour, and finally filtered, washed and dried to obtain the product.
[0090] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0091] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0092] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0093] Comparative Example 5
[0094] The carbon fiber filler is prepared by the following method:
[0095] (1) Graphite particles with a diameter of 0.5 micrometers and carbon fibers with a length of 100 micrometers are mixed in a mass ratio of 1:2, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60% by volume, heated to 110°C and kept warm for 2 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0 mol / L, heated to 60°C and kept warm for 1 hour, filtered, washed, and dried;
[0096] (2) adding the product of step 1 to a n-butanol solution containing 2 wt% zirconium n-butoxide, heating to 70°C, adding acetic acid, keeping the temperature for 5 hours, filtering, washing, drying, placing in a heating furnace, heating to 750°C and keeping the temperature for 3 hours;
[0097] (3) The product of step 2 was added to an aqueous solution containing 15 wt% dopamine, and then tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine was added. Dilute hydrochloric acid was added to adjust the pH value of the mixture to 7.6, and the mixture was heated to 50°C for 10 min. The mixture was washed and dried, and the mixture was used as an anode and graphite as a cathode in an ammonium bicarbonate solution with a concentration of 4 wt% and an applied density of 2 mA / cm 2 The current is applied for 2 minutes, and electrochemical anodization, washing and drying are performed to obtain the product.
[0098] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0099] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0100] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0101] Comparative Example 6
[0102] The carbon fiber filler is prepared by the following method:
[0103] (1) Graphite particles with a diameter of 0.5 micrometers and carbon fibers with a length of 100 micrometers are mixed in a mass ratio of 1:2, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60% by volume, heated to 110°C and kept warm for 2 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0 mol / L, heated to 60°C and kept warm for 1 hour, filtered, washed, and dried;
[0104] (2) adding the product of step 1 to a n-butanol solution containing 2 wt% zirconium n-butoxide, heating to 70°C, adding acetic acid, keeping the temperature for 5 hours, filtering, washing, drying, placing in a heating furnace, heating to 750°C and keeping the temperature for 3 hours;
[0105] (3) The product of step 2 is used as the anode and graphite is used as the cathode. They are placed in a 4 wt% ammonium bicarbonate solution and the applied density is 2 mA / cm 2 The current lasted for 2 min to carry out electrochemical anodization;
[0106] (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75°C, maintained for 6 hours, filtered and washed; then added to a toluene solution containing 15wt% polyethylene glycol, added dibutyltin dilaurate in an amount of 3wt%, heated to 75°C, maintained for 1 hour, and finally filtered, washed and dried to obtain the product.
[0107] The inner sheath comprises, by mass, 50 parts of styrene-butadiene rubber, 25 parts of ethylene-vinyl acetate copolymer, 15 parts of hydrogenated styrene-butadiene block copolymer, 8 parts of glyceryl monostearate, 6 parts of dibenzothiazole disulfide, 3 parts of diisopropylbenzene peroxide, and 3 parts of antioxidant.
[0108] The lubricating layer comprises, by weight: 50 parts of polyvinyl alcohol, 20 parts of polyacrylonitrile, 20 parts of polyethylene glycol, 15 parts of polyvinyl pyrrolidone, 8 parts of nano aluminum hydroxide, 8 parts of nano zinc borate, 3 parts of plasticizer and 2 parts of sodium polyacrylate.
[0109] The outer sheath comprises, by mass: 40 parts of high-density polyethylene; 30 parts of low-density polyethylene; 6 parts of ultra-high molecular weight polyethylene, 15 parts of ethylene-propylene rubber, 25 parts of hydrogenated styrene-butadiene block copolymer, 15 parts of carbon fiber filler, 5 parts of N,N'-methylene bisstearamide and 3 parts of antioxidant.
[0110] Comparative Example 7
[0111] The lubricating layer is omitted, and the remaining components of the inner sheath and the outer sheath are exactly the same as those in Example 1.
[0112] Experiments and Data
[0113] The performance of the optical cable is tested in accordance with the national standard GB / T29516 to obtain the tensile strength.
[0114] The performance of the optical cable was tested according to the national standard GB / T7424.1-E6, and the repeated bending: residual additional attenuation was obtained.
[0115] The test results of tensile strength and bending resistance of Examples 1-4 of the present invention and Comparative Examples 1-7 are shown in Table 1.
[0116] Table 1
[0117]
[0118] Tests and Results
[0119] As can be seen from Table 1, it can be seen from the data comparison of the embodiment and the comparative example 2 that after the graphite particles are added, the graphite particles and the carbon fibers will work together to improve the anchoring effect of the fibers in the polymer material, thereby improving the positional stability of the carbon fiber filler in the sheath material, thereby improving the bending resistance of the sheath material. As can be seen from the data comparison of the embodiment and the comparative examples 3-4 and 6, the surface is modified with zirconium oxide, and at the same time, after being coated with dopamine, anodized, nitrogen elements can be doped on the surface of the carbon fiber to form partial zirconium nitride and zirconium oxynitride, which can greatly improve the mechanical strength of the carbon fiber, thereby improving the performance of the sheath in terms of tensile resistance, distortion, and deformation. As can be seen from the data comparison of the embodiment and the comparative example 5, the graphite particles and the carbon fibers can form a structure with anchor points or a local network under the coating of polyethylene glycol, improve the dispersion performance, and improve the bending resistance of the sheath material. As can be seen from the data comparison of the embodiment and the comparative example 7, a lubricating layer is added between the inner sheath and the outer sheath, thereby reducing the stress concentration between the inner and outer layers, improving the bending resistance of the sheath material, and improving the service life. From the data comparison of the embodiment and comparative example 1, it can be seen that the modified composite carbon fiber of the present invention has a significant technical effect on improving the strength and life of the optical cable compared with the commercially available carbon fiber materials. Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it accordingly, and cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be covered within the protection scope of the present invention.
Claims
1. A multi-core prefabricated terminated circular introduction optical cable, the optical cable comprising a multi-core optical fiber, an inner sheath, a lubricating layer and an outer sheath, wherein the inner sheath, the lubricating layer and the outer sheath are sequentially coated on the outer side of the multi-core optical fiber in order from inside to outside; The inner sheath comprises styrene-butadiene rubber in parts by mass; the outer sheath comprises: 40-50 parts of high density polyethylene; 30-35 parts of low-density polyethylene; 6-8 parts of ultra-high molecular weight polyethylene, 15-20 parts of ethylene-propylene rubber, 25-30 parts of hydrogenated styrene-butadiene block copolymer, 15-18 parts of carbon fiber filler, 5-10 parts of N,N'-methylene bisstearamide and 3-5 parts of antioxidant; wherein the carbon fiber filler is prepared by the following method: (1) Graphite particles are mixed with carbon fibers, placed in a closed heating furnace, a mixed gas of oxygen and water vapor is introduced, heated and kept warm for surface oxidation, taken out, and then placed in hydrochloric acid, heated and kept warm for surface activation; (2) adding the product of step 1 to a n-butanol solution containing zirconium n-butoxide, adding acetic acid, hydrolyzing, and then placing in a heating furnace for sintering; (3) adding the product of step 2 to a dopamine aqueous solution, then adding tris(hydroxymethyl)aminomethane) in an amount equal to that of dopamine, adding dilute hydrochloric acid to adjust the pH value of the mixed solution for surface modification, then placing it as an anode and graphite as a cathode in a salt solution, applying current, and performing electrochemical anodic oxidation; (4) The product of step 3 is placed in a mixture of thionyl chloride and dimethylformamide, heated, and then added to a toluene solution containing polyethylene glycol, dibutyltin dilaurate is added, and heated for surface modification to obtain a carbon fiber filler.
2. The multi-core prefabricated terminated circular optical cable according to claim 1, characterized in that: The inner sheath comprises, by mass, 50-55 parts of styrene-butadiene rubber, 25-30 parts of ethylene-vinyl acetate copolymer, 15-20 parts of hydrogenated styrene-butadiene block copolymer, 8-10 parts of glyceryl monostearate, 6-8 parts of dibenzothiazole disulfide, 3-5 parts of diisopropylbenzene peroxide, and 3-5 parts of antioxidant.
3. The multi-core pre-terminated circular optical cable according to claim 1, characterized in that: The lubricating layer comprises, by weight: 50-60 parts of polyvinyl alcohol, 20-25 parts of polyacrylonitrile, 20-25 parts of polyethylene glycol, 15-20 parts of polyvinyl pyrrolidone, 8-10 parts of nano aluminum hydroxide, 8-10 parts of nano zinc borate, 3-5 parts of plasticizer and 2-4 parts of sodium polyacrylate.
4. The multi-core pre-terminated circular optical cable according to claim 1, characterized in that: The carbon fiber filler is prepared by the following method: (1) Graphite particles with a diameter of 0.5-1 micron and carbon fibers with a length of 100-150 microns are mixed in a mass ratio of 1:2-4, placed in a closed heating furnace, and a mixed gas of oxygen and water vapor is introduced, wherein the oxygen content is 60-75% by volume, heated to 110-130°C and kept warm for 2-4 hours, taken out, and then placed in hydrochloric acid with a concentration of 1.0-1.5 mol / L, heated to 60-80°C and kept warm for 1-3 hours, filtered, washed, and dried; (2) adding the product of step 1 to a n-butanol solution containing 2-4 wt% zirconium n-butoxide, heating to 70-80°C, adding acetic acid, keeping warm for 5-10 hours, filtering, washing, drying, placing in a heating furnace, heating to 750-800°C and keeping warm for 3-5 hours; (3) Add the product of step 2 to an aqueous solution containing 15-20wt% dopamine, then add tris(hydroxymethyl)aminomethane in an amount equal to that of dopamine, add dilute hydrochloric acid to adjust the pH value of the mixture to 7.6-8.0, heat to 50-60°C for 10-15 minutes, wash, dry, use it as an anode, and graphite as a cathode, place it in an ammonium bicarbonate solution with a concentration of 4-6wt%, and apply a density of 2-4mA / cm 2 The current lasts for 2-6 minutes to carry out electrochemical anodization; (4) The product of step 3 is placed in a mixed solution of thionyl chloride and dimethylformamide, wherein the volume ratio of thionyl chloride to dimethylformamide is 15:1, heated to 75-80°C, maintained for 6-12 hours, filtered and washed; then added to a toluene solution containing 15-20wt% polyethylene glycol, dibutyltin dilaurate is added in an amount of 3-5wt%, heated to 75-85°C, maintained for 1-2 hours, and finally filtered, washed and dried to obtain the carbon fiber filler.
5. The multi-core pre-terminated circular optical cable according to claim 3, characterized in that: The plasticizer is selected from one or a combination of dibutyl phthalate, dimethyl phthalate, diethyl phthalate, dioctyl phthalate, dicyclohexyl phthalate, and diisobutyl phthalate.
6. The multi-core pre-terminated circular optical cable according to any one of claims 1 to 5, characterized in that: The antioxidant is selected from one or more of antioxidant 1010, antioxidant 168, antioxidant 245, and antioxidant 264.
Citation Information
Patent Citations
Fast two-step crosslinked polyethylene insulation material and preparation technology thereof
CN104610636A
Optical cable with strong torsion resistance
CN105929497A