Negative photoresist developing solution composition as well as preparation method and application thereof
By adjusting the components such as amidine compounds and surfactants in the developer formulation, the problems of high metal ions, poor stability and pollution of negative photoresist developer in the prior art are solved, and the high stability of the developer is achieved and multi-substrate corrosion inhibition effect.
Patent Information
- Application Number
- CN202411263618.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing negative photoresist developer has high metal ion content, poor development stability, insufficient development capacity, easy to generate bubbles and contamination, and it is difficult to suppress corrosion on various substrates or metal layers.
A negative photoresist developer composition containing organic ammonium acid by adjusting the combination and proportion of amidine-based compounds, buffers, Gemini-type surfactants, compound solubilizers, anti-fouling promoters and flattening regulators is prepared. and ionic liquids, low foam type Gemini surfactant is used to improve the stability and corrosion inhibition of the developer.
The metal ion content of the developer is reduced, the development stability and capacity are improved, and bubble generation is reduced. It is not easy to produce back-stickness and residue after development, and has a good corrosion inhibition effect on different substrates and metal layers.
Smart Images

Figure CN118884786A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wet electronic chemicals, and in particular to a negative photoresist developer composition and a preparation method and application thereof. Background Art
[0002] At present, TFT-LCD (thin film transistor liquid crystal display) technology is still the mainstream technology in the field of panel display, and color filter (CF) is an important component for TFT-LCD display screen to realize color display. In the photolithography process of manufacturing CF, in order to obtain various fine circuit images required, it is necessary to first coat a negative photoresist on a substrate to form a thin film, then expose it, and dissolve and remove the unexposed part of the photoresist film with a developer to obtain the required circuit pattern. In the preparation process of CF, negative photoresists such as black matrix photoresist (BM), color photoresist (RGB), gap column photoresist (PS) and protective layer photoresist (OC) need to be used successively, and the use of each photoresist needs to go through the photolithography process of surface cleaning-coating, pre-baking-exposure-development-development post-detection-post-baking.
[0003] With the rapid development of TFT-LCD, the touch screen market has also developed from resistive to capacitive. The core component of the capacitive touch screen, the touch sensor, also needs to use negative photoresist for development wiring and insulation bridge. Therefore, the selection of a developer with excellent comprehensive performance plays a vital role in improving product yield. The main components of negative photoresist include alkali-soluble resins such as acrylic resin, crosslinking agents, photoinitiators, pigments, dispersants, leveling agents and solvents; after the negative photoresist is exposed, the exposed area undergoes a photo-initiated polymerization reaction and is insoluble in the developer, while the unexposed part is dissolved in the developer, thereby producing a development pattern.
[0004] However, the existing negative photoresist developers on the market still have several shortcomings: (1) Inorganic alkalis such as potassium hydroxide and sodium hydroxide are generally used as the main developer, which contain a large amount of potassium ions and sodium ions that are easy to cause conductive short circuits in device circuits. In addition, this type of developer has a large content of metal ions and is not easy to be cleaned, and is easy to remain on the surface of the substrate. (2) A large amount of foam will be generated during the spray development process, affecting the development accuracy of the photoresist and easily causing development residues; (3) The development effect is poorly stable, the development capacity is small, and frequent tank changes are required, resulting in increased manufacturing costs; (4) After repeated use, the developer is easy to form insoluble residues or residues, which are easy to stick back to the glass substrate or the photoresist surface to form film stains, causing device surface contamination, incomplete local development, and difficulty in forming accurate photoresist images. In addition, more importantly, it is difficult to inhibit the corrosion of various substrates or metal layers, and it is inevitable to produce different degrees of corrosiveness.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a negative photoresist developer composition and a preparation method and application thereof. The negative photoresist developer composition overcomes the drawbacks of the existing developer formulation system, such as high metal ion content, poor development stability, insufficient development capacity, easy bubbles, and easy re-adhesion and contamination of glass substrates and photoresist layers after repeated use. The developer formulation system is regulated by adjusting the combination and proportion of amidine compounds, buffers, Gemini surfactants, compound solubilizers, leveling regulators, and anti-fouling accelerator components in the formulation, and the development effect, development life, and development resolution of different negative photoresists and the corrosion inhibition of different substrates or underlying metal layers are improved, thereby broadening the development compatibility of the developer composition.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] In a first aspect, the present invention provides a negative photoresist developer composition, wherein the negative photoresist developer composition comprises, by weight:
[0009] 0.1-34 parts of amidine compounds, 2-18 parts of compound solubilizers, 0.8-32 parts of Gemini surfactants, 0.1-8 parts of buffers, 0.5-20 parts of antifouling promoters, and 0.4-7 parts of leveling regulators;
[0010] Wherein, the composite solubilizing agent comprises organic acid ammonium and ionic liquid.
[0011] Preferably, the amidine compound comprises a diazabicyclic compound and / or an acid salt of a diazabicyclic compound.
[0012] Preferably, the amidine compound is selected from 1,5-diazabicyclo[4.3.0]non-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,8-diazabicyclo[5.4.0]undec-7-enecarboxylate, 1,8-diazabicyclo[5.4.0]undec-7-eneoctanoate, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-eneacetic acid Any one or a combination of at least two of the following: 1,5-diazabicyclo[4.3.0]non-5-ene acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene methoxy acetate, 1,5-diazabicyclo[4.3.0]non-5-ene methoxy acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene ethoxy acetate or 1,5-diazabicyclo[4.3.0]non-5-ene ethoxy acetate.
[0013] Preferably, the mass ratio of the organic acid ammonium to the ionic liquid satisfies the following formula I and formula II:
[0014] When 2%≤M 1 +M 2 ≤5%, 0.8≤M 2 / M 1 ≤2 Formula I;
[0015] When 5%<M 1 +M 2 ≤18%, 0.1≤M 2 / M 1 ≤1 Formula II;
[0016] Among them, M 1 represents the percentage of the organic acid ammonium in the total mass of the negative photoresist developer composition, M 2 represents the percentage of the ionic liquid in the total mass of the negative photoresist developer composition.
[0017] Preferably, the organic ammonium acid is selected from any one or a combination of at least two of ammonium gluconate, ammonium tartrate, ammonium alginate, ammonium benzoate, ammonium citrate or ammonium maleate, preferably any one or a combination of at least two of ammonium maleate, ammonium gluconate or ammonium alginate.
[0018] Preferably, the ionic liquid comprises an imidazole ionic liquid as shown in the following formula I:
[0019]
[0020] Wherein, R is selected from C1 to C3 straight chain alkyl, anion X - Any one selected from bromide ion, nitrate ion, tetrafluoroborate ion, hexafluorophosphate ion or bis(trifluoromethanesulfonyl)imide ion.
[0021] Preferably, the ionic liquid is selected from any one of 1-aminoethyl-3-methylimidazolium bromide, 1-aminoethyl-3-methylimidazolium nitrate, 1-aminoethyl-3-methylimidazolium tetrafluoroborate, 1-aminoethyl-3-methylimidazolium hexafluorophosphate, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-aminopropyl-3-methylimidazolium bromide, 1-aminopropyl-3-methylimidazolium nitrate, 1-aminopropyl-3-methylimidazolium tetrafluoroborate, 1-aminopropyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide or 1-aminopropyl-3-methylimidazolium hexafluorophosphate, or a combination of at least two thereof, preferably 1-aminoethyl-3-methylimidazolium tetrafluoroborate and / or 1-aminopropyl-3-methylimidazolium tetrafluoroborate.
[0022] Preferably, the Gemini surfactant comprises a Gemini surfactant as shown in the following formula II:
[0023]
[0024] Wherein, R' is selected from C1-C5 straight chain or branched alkyl, and R" is selected from methyl or hydroxyl.
[0025] Preferably, the Gemini surfactant is selected from any one or a combination of at least two of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 4,7-dimethyl-5-decyne-4,7-diol, 2,5,8,11-dimethyl-6-dodecyne-5,8-diol or 3,6-dimethyl-4-octyne-3,6-diol, preferably 2,4,7,9-tetramethyl-5-decyne-4,7-diol and / or 4,7-dimethyl-5-decyne-4,7-diol.
[0026] Preferably, the buffer is selected from 2-amino-2-hydroxymethyl-1,3-propanediol and / or 2-bis(2-hydroxyethyl)amino-2-hydroxymethyl-1,3-propanediol, preferably 2-amino-2-hydroxymethyl-1,3-propanediol.
[0027] Preferably, the anti-fouling promoter is selected from fluorine-containing compounds.
[0028] Preferably, the fluorine-containing compound includes a fluorine-containing compound as shown in the following formula III:
[0029]
[0030] Wherein, R'' is selected from C1-C5 straight-chain or branched perfluoro-substituted alkyl groups.
[0031] Preferably, the fluorine-containing compound is selected from any one of perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid, perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid or perfluoro-2,5-dimethyl-3,6-dioxanononanoic acid or a combination of at least two thereof, preferably perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid and / or perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid.
[0032] Preferably, the leveling regulator is selected from 2,3,4-trihydroxybenzophenone.
[0033] Preferably, the negative photoresist developer composition further comprises a solvent.
[0034] Preferably, the solvent comprises water.
[0035] Preferably, the amount of water added is 20 to 90 parts.
[0036] In a second aspect, the present invention provides a method for preparing the negative photoresist developer composition as described in the first aspect, the preparation method comprising the following steps:
[0037] The amidine compound, the composite solubilizer, the Gemini surfactant, the buffer, the anti-fouling accelerator and the leveling regulator are mixed according to a proportion to obtain the negative photoresist developer composition.
[0038] Preferably, the method for preparing the negative photoresist developer composition comprises the following steps:
[0039] (a) mixing the amidine compound, the composite solubilizer, the buffer and part of the solvent for a first time, and then adding the antifouling promoter for a second time to obtain a mixed solution A; adding the Gemini surfactant to the remaining solvent, stirring and mixing, to obtain a mixed solution B;
[0040] (b) adding the mixed solution A to the mixed solution B and stirring and mixing them to obtain the negative photoresist developer composition.
[0041] Preferably, in step (a), the partial solvent accounts for 40-60% of the total mass of the solvent.
[0042] Preferably, in the process of preparing the mixed solution A in step (a), the first stirring and mixing time is 1 to 2 hours.
[0043] Preferably, in the process of preparing the mixed solution A in step (a), the second stirring and mixing time is 0.5 to 1 hour.
[0044] Preferably, in the process of preparing the mixed solution B in step (a), the stirring and mixing time is 1 to 1.5 hours.
[0045] Preferably, in the process of preparing the negative photoresist developer composition in step (b), the stirring and mixing time is 0.5 to 1 hour.
[0046] Preferably, the stirring and mixing temperatures in step (a) and step (b) are independently 15 to 45°C.
[0047] Preferably, step (b) is followed by step (c): filtering the negative photoresist developer composition in series using filters with pore sizes of 0.5 μm and 0.1 μm to obtain a finished product of the negative photoresist developer composition.
[0048] In a third aspect, the present invention provides a use of the negative photoresist developer composition as described in the first aspect in the manufacture of integrated circuits, flat panel displays or semiconductor lighting chips.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) The present invention uses amidine compounds as the main developing agent, which not only has the developing ability of a strong base, but is also less aggressive to the glass substrate and the metal (oxide) film layer than inorganic bases and ammonium hydroxide-based organic bases. It can also avoid the influence of contaminating ions such as sodium ions and potassium ions in inorganic bases on the electrical properties and manufacturing yield of the device. At the same time, the addition of a buffer can effectively avoid the problem of a decrease in developing ability and the easy generation of developing residues after a period of use of traditional developers.
[0051] (2) The ionic liquid selected in the present invention has a solubilizing effect and also has a corrosion inhibition effect on the substrate and the contact metal layer during the development process; at the same time, the low-foaming Gemini surfactant is used to increase the wettability and affinity of the developer composition to the photoresist component, which is also a key component for improving the compounding stability of the developer composition, and enables the developer to have a low-bubble or no-foaming effect during the spray development process; in addition, the Gemini surfactant can also cooperate with the ionic liquid component to enhance the protection of the substrate and the metal layer.
[0052] (3) The negative photoresist developer provided by the present invention can be diluted at a high multiple and has a wide process temperature range, and has the advantage of low transportation cost; and is not prone to re-sticking and residue after continuous development. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0054] Figure 1 This is a picture taken with an optical microscope provided in Example 1.
[0055] Figure 2 This is a cross-sectional scanning electron microscope image provided for Example 1.
[0056] Figure 3 This is a picture taken with an optical microscope provided in Example 2.
[0057] Figure 4 This is a cross-sectional scanning electron microscope image provided for Example 2.
[0058] Figure 5 This is a picture taken with an optical microscope provided for Comparative Example 1.
[0059] Figure 6 The optical microscope image provided for Comparative Example 2. DETAILED DESCRIPTION
[0060] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0061] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0062] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] In a first aspect, the present invention provides a negative photoresist developer composition, wherein the negative photoresist developer composition comprises, by weight:
[0064] 0.1 to 34 parts of amidine compounds, 2 to 18 parts of compound solubilizers, 0.8 to 32 parts of Gemini surfactants, 0.1 to 8 parts of buffers, 0.5 to 20 parts of antifouling promoters, and 0.4 to 7 parts of leveling regulators.
[0065] Wherein, the composite solubilizing agent comprises organic acid ammonium and ionic liquid.
[0066] In the present invention, the developer formulation system is regulated by adjusting the combination and proportion of the amidine compound, buffer, Gemini surfactant, compound solubilizer, leveling regulator, and anti-fouling promoter components in the formula, so that the negative photoresist developer composition overcomes the disadvantages of the existing developer formulation system, such as high metal ion content, poor development stability, insufficient development capacity, easy bubbles, and easy re-adhesion and contamination of glass substrates and photoresist layers after repeated use, as well as the development effect, development life, and development resolution of different negative photoresists and the corrosion inhibition of different substrates or underlying metal layers, thereby broadening the development compatibility of the developer composition. In addition, the negative photoresist developer prepared by the present invention can be diluted by a high multiple and has the characteristics of a wide process temperature range, has the advantages of low transportation costs, and is not easy to produce re-adhesion and residues after continuous development.
[0067] As an optional embodiment, in the negative photoresist developer composition, the content of the amidine compound is 0.1 to 34 parts, for example, it can be 0.1 parts, 0.2 parts, 0.4 parts, 0.6 parts, 0.8 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 4 parts, 5 parts, 6 parts, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, etc.
[0068] As an optional embodiment, in the negative photoresist developer composition, the content of the complex solubilizer is 2 to 18 parts, for example, it can be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, etc.
[0069] As an optional embodiment, in the negative photoresist developer composition, the content of the Gemini-type surfactant is 0.8 to 32 parts, for example, it can be 0.8 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, etc.
[0070] As an optional embodiment, in the negative photoresist developer composition, the content of the buffer is 0.1 to 8 parts, for example, it can be 0.1 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts, 5.5 parts, 6 parts, 6.5 parts, 7 parts, 7.5 parts, 8 parts, etc.
[0071] As an optional embodiment, in the negative photoresist developer composition, the content of the anti-fouling promoter is 0.5 to 20 parts, for example, it can be 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0072] As an optional embodiment, in the negative photoresist developer composition, the content of the leveling regulator is 0.4 to 7 parts, for example, it can be 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, etc.
[0073] As an optional embodiment, the amidine compound is selected from 1,5-diazabicyclo[4.3.0]non-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene formate, 1,8-diazabicyclo[5.4.0]undec-7-ene octanoate, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene formate, Any one or a combination of at least two of 1,5-diazabicyclo[4.3.0]non-5-ene acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene methoxy acetate, 1,5-diazabicyclo[4.3.0]non-5-ene methoxy acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene ethoxy acetate or 1,5-diazabicyclo[4.3.0]non-5-ene ethoxy acetate.
[0074] Among them, the structural formula of 1,5-diazabicyclo[4.3.0]non-5-ene (hereinafter referred to as DBN) is:
[0075] Among them, the structural formula of 1,8-diazabicyclo[5.4.0]undec-7-ene (hereinafter referred to as DBU) is:
[0076] Among them, the structural formula of 1,8-diazabicyclo[5.4.0]undec-7-enecarboxylate is:
[0077] Among them, the structural formula of 1,8-diazabicyclo[5.4.0]undec-7-eneoctanoate is:
[0078] In the present invention, amidine compounds are selected as the main raw materials for developing imaging, which can react with the macromolecular resin of the non-exposed area photoresist to form a macromolecular resin salt with better solubility; at the same time, they can dissolve or soften and peel off the initiator, dispersant, auxiliary agent and other components in the non-exposed photoresist.
[0079] As an optional embodiment, the mass ratio of the organic acid ammonium and the ionic liquid satisfies the following formula I and formula II:
[0080] When 2%≤M 1 +M 2 ≤5%, 0.8≤M 2 / M 1 ≤2 Formula I;
[0081] When 5%<M 1 +M 2 ≤18%, 0.1≤M 2 / M 1 ≤1 Formula II.
[0082] Among them, M 1 represents the percentage of the organic acid ammonium in the total mass of the negative photoresist developer composition, M 2 represents the percentage of the ionic liquid in the total mass of the negative photoresist developer composition.
[0083] As an optional embodiment, the organic ammonium acid is selected from any one or a combination of at least two of ammonium gluconate, ammonium tartrate, ammonium alginate, ammonium benzoate, ammonium citrate or ammonium maleate, preferably any one or a combination of at least two of ammonium maleate, ammonium gluconate or ammonium alginate.
[0084] As an optional embodiment, the ionic liquid includes an imidazole ionic liquid as shown in the following formula I:
[0085]
[0086] Wherein, R is selected from C1-C3 straight-chain or branched alkyl groups, for example, methyl, ethyl or n-propyl.
[0087] Among them, the anion X - Selected from bromide ion (Br - ), nitrate ion (NO 3 - ), tetrafluoroborate ion (BF 4 - ), hexafluorophosphate ion (PF 6 - ) or bis(trifluoromethanesulfonyl)imide ion ([NTf 2 ] - )
[0088] As an optional embodiment, the ionic liquid includes an imidazole ionic liquid as shown in the following formula I-1 and / or I-2:
[0089]
[0090] Among them, the anion X - Selected from bromide ion (Br - ), nitrate ion (NO 3 - ), tetrafluoroborate ion (BF 4 - ), hexafluorophosphate ion (PF 6 - ) or bis(trifluoromethanesulfonyl)imide ion ([NTf 2 ] - )
[0091] As an optional embodiment, the ionic liquid is selected from any one of 1-aminoethyl-3-methylimidazolium bromide, 1-aminoethyl-3-methylimidazolium nitrate, 1-aminoethyl-3-methylimidazolium tetrafluoroborate, 1-aminoethyl-3-methylimidazolium hexafluorophosphate, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-aminopropyl-3-methylimidazolium bromide, 1-aminopropyl-3-methylimidazolium nitrate, 1-aminopropyl-3-methylimidazolium tetrafluoroborate, 1-aminopropyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide or 1-aminopropyl-3-methylimidazolium hexafluorophosphate, or a combination of at least two thereof, preferably 1-aminoethyl-3-methylimidazolium tetrafluoroborate and / or 1-aminopropyl-3-methylimidazolium tetrafluoroborate.
[0092] In the present invention, the compound solubilizer can increase the dissolution amount of the resultant polymer composite salt in the developer system and soften the composite salt, which is beneficial to prolong the service life of the developer and inhibit the polymer composite salt crystal residue from remaining in the developer tank and pipeline in the later stage of development. In addition, the ionic liquid in the compound solubilizer also has the effect of inhibiting the corrosion of aluminum, copper, ITO film and silicon or glass substrate. The ratio between the raw material usage in the compound solubilizer also directly affects the use effect of the developer, so there are certain restrictions on the raw material ratio.
[0093] As an optional embodiment, the Gemini surfactant includes a Gemini surfactant as shown in the following formula II:
[0094]
[0095] Wherein, R' is selected from C1-C5 straight chain or branched alkyl groups, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl or neopentyl.
[0096] Wherein, R" is selected from methyl or hydroxyl.
[0097] As an optional embodiment, the Gemini surfactant is selected from any one or a combination of at least two of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 4,7-dimethyl-5-decyne-4,7-diol, 2,5,8,11-dimethyl-6-dodecyne-5,8-diol or 3,6-dimethyl-4-octyne-3,6-diol, preferably 2,4,7,9-tetramethyl-5-decyne-4,7-diol and / or 4,7-dimethyl-5-decyne-4,7-diol.
[0098] Among them, the structural formula of 2,4,7,9-tetramethyl-5-decyne-4,7-diol (TMDD for short) is:
[0099] Among them, the structural formula of 4,7-dimethyl-5-decyne-4,7-diol (DDTM for short) is:
[0100] Among them, the structural formula of 2,5,8,11-dimethyl-6-dodecene-5,8-diol is:
[0101] Among them, the structural formula of 3,6-dimethyl-4-octyne-3,6-diol is:
[0102] In the present invention, Gemini surfactant plays a role in reducing the surface tension of the developer on the photoresist film, increasing the wettability and affinity of the developer composition to the photoresist adhesive component, and is also a key component for improving the compounding stability of the developer composition. It also cooperates with the ionic liquid to inhibit the corrosive attack of the developer on the substrate during the development process, and enables the developer to have a low bubble or no bubble effect during the spray development process.
[0103] As an optional embodiment, the buffer is selected from 2-amino-2-hydroxymethyl-1,3-propanediol and / or 2-bis(2-hydroxyethyl)amino-2-hydroxymethyl-1,3-propanediol, preferably 2-amino-2-hydroxymethyl-1,3-propanediol.
[0104] In the present invention, the buffer mainly plays the role of timely ionization and replenishment of the hydroxide ions consumed in the developer system, maintaining the stability of development and maintaining the service life of the developer. At the same time, the buffer also has the effect of assisting the main developer to accelerate the penetration into the photoresist film layer, thereby accelerating the development speed of the developer system.
[0105] As an optional embodiment, the anti-fouling promoter is selected from fluorine-containing compounds.
[0106] As an optional embodiment, the fluorine-containing compound includes a fluorine-containing compound as shown in the following formula III:
[0107]
[0108] Wherein, R'' is selected from C1-C5 straight chain or branched perfluoro substituted alkyl groups, for example, it can be perfluoromethyl, perfluoroethyl, perfluoro-n-propyl, perfluoro-isopropyl, perfluoro-n-butyl, perfluoro-isobutyl, perfluoro-sec-butyl, perfluoro-tert-butyl, perfluoro-n-pentyl, perfluoro-isopentyl or perfluoro-neopentyl.
[0109] As an optional embodiment, the fluorine-containing compound is selected from any one of perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid, perfluoro-2,5-dimethyl-3,6-dioxanoic acid or perfluoro-2,5-dimethyl-3,6-dioxanononanoic acid, or a combination of at least two thereof, preferably perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid and / or perfluoro-2,5-dimethyl-3,6-dioxanoic acid.
[0110] Among them, the structural formula of perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid (abbreviated as K1) is:
[0111] Among them, the structural formula of perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid (abbreviated as K2) is:
[0112] Among them, the structural formula of perfluoro-2,5-dimethyl-3,6-dioxanononanoic acid (abbreviated as K3) is:
[0113] In the present invention, the anti-fouling promoter exhibits extremely low surface tension characteristics due to its unique molecular structure, and can cooperate with Gemini surfactant to improve the wettability of the developer to the photoresist and the glass substrate. At the same time, it can be temporarily adsorbed on the glass substrate and the photoresist layer in the exposure area during the development process, thereby increasing the repulsion between the glass substrate and the insoluble polymer salts in the developer and the hydrophobic molecules such as photoinitiators and pigment molecules, thereby avoiding the increase in the concentration of photoresist components in the developer in the late stage of development and the resulting back-adhesion pollution to the glass substrate. After the development is completed, the anti-fouling promoter is easily rinsed with water, and has low toxicity and environmental protection.
[0114] As an optional embodiment, the leveling agent is selected from 2,3,4-trihydroxybenzophenone.
[0115] In the present invention, the leveling regulator can effectively adjust the development slope angle of the photoresist line during the development process to improve the yield of the subsequent coating or coating process, so that the developed photoresist line presents a smooth cone angle, thereby achieving a good development profile.
[0116] As an optional embodiment, the negative photoresist developer composition further includes a solvent.
[0117] As an optional embodiment, the solvent includes water.
[0118] As an optional embodiment, the water is ultrapure water with a resistivity of not less than 18 mΩ at 25°C.
[0119] As an optional embodiment, the amount of water added is 20 to 90 parts, for example, it can be 20 parts, 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, 85 parts, 90 parts, etc.
[0120] As an optional embodiment, water is added in an amount sufficient to make up the total mass fraction of the negative photoresist developer composition to 100 parts.
[0121] That is, in the present invention, the residual water refers to the residual water in the components of the developer composition of the present invention excluding the amidine compound, buffer, Gemini surfactant, complex solubilizer, leveling regulator, anti-fouling promoter and optionally other raw materials, and the total mass fraction of water and other raw materials is 100 parts.
[0122] In the present invention, the negative photoresist developer composition can meet the development and patterning requirements of different types of negative photoresists in yellow light process manufacturing based on the coordinated combination of different components and specific development process conditions, while avoiding the influence of the introduction of metal ions in the formula on the device manufacturing yield and electrical reliability performance, and effectively improving the development quality.
[0123] In a second aspect, the present invention provides a method for preparing the negative photoresist developer composition as described in the first aspect, the preparation method comprising the following steps:
[0124] The amidine compound, the composite solubilizer, the Gemini surfactant, the buffer, the anti-fouling accelerator and the leveling regulator are mixed according to a proportion to obtain the negative photoresist developer composition.
[0125] As an optional embodiment, the method for preparing the negative photoresist developer composition comprises the following steps:
[0126] (a) mixing the amidine compound, the composite solubilizer, the buffer and part of the solvent for a first time, and then adding the antifouling promoter for a second time to obtain a mixed solution A; adding the Gemini surfactant to the remaining solvent, stirring and mixing, to obtain a mixed solution B;
[0127] (b) adding the mixed solution A to the mixed solution B and stirring and mixing them to obtain the negative photoresist developer composition.
[0128] As an optional embodiment, in step (a), the partial solvent accounts for 40-60% of the total mass of the solvent, for example, it can be 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58%, 60%, etc.
[0129] As an optional embodiment, in step (a), during the preparation of the mixed solution A, the first stirring and mixing time is 1 to 2 hours, for example, it can be 1 hour, 1.1 hours, 1.2 hours, 1.3 hours, 1.4 hours, 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2 hours, etc.
[0130] As an optional embodiment, in step (a), during the preparation of the mixed solution A, the second stirring and mixing time is 0.5 to 1 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, etc.
[0131] As an optional embodiment, in step (a), during the preparation of the mixed solution B, the stirring and mixing time is 1 to 1.5 h, for example, 1 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, etc.
[0132] As an optional embodiment, in step (b), during the preparation of the negative photoresist developer composition, the stirring and mixing time is 0.5 to 1 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, etc.
[0133] As an optional embodiment, the stirring and mixing temperatures in step (a) and step (b) are each independently 15 to 45°C, for example, 15h, 16h, 18h, 20h, 22h, 24h, 26h, 28h, 30h, 32h, 34h, 36h, 38h, 40h, etc.
[0134] Preferably, step (b) is followed by step (c): filtering the negative photoresist developer composition in series using filters with pore sizes of 0.5 μm and 0.1 μm to obtain a finished product of the negative photoresist developer composition.
[0135] In a third aspect, the present invention provides a use of the negative photoresist developer composition as described in the first aspect in the manufacture of integrated circuits, flat panel displays or semiconductor lighting chips.
[0136] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0137] The raw material names represented by the abbreviations in the following examples and comparative examples are as follows:
[0138] DBN─1,5-diazabicyclo[4.3.0]non-5-ene;
[0139] DBU─1,8-diazabicyclo[5.4.0]undec-7-ene;
[0140] TMDD─2,4,7,9-tetramethyl-5-decyne-4,7-diol;
[0141] DDTM─4,7-dimethyl-5-decyne-4,7-diol;
[0142] K1─Perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid;
[0143] K2─Perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid;
[0144] K3─Perfluoro-2,5-dimethyl-3,6-dioxanononanoic acid;
[0145] H1─2-amino-2-hydroxymethyl-1,3-propanediol;
[0146] H2─2-Bis(2-hydroxyethyl)amino-2-hydroxymethyl-1,3-propanediol;
[0147] Z1─ammonium gluconate;
[0148] Z2─ammonium maleate;
[0149] Z3─Ammonium alginate
[0150] L1─1-aminoethyl 3-methylimidazolium tetrafluoroborate;
[0151] L2─1-aminopropyl 3-methylimidazolium tetrafluoroborate;
[0152] THBP─2,3,4-trihydroxybenzophenone.
[0153] Examples 1 to 9
[0154] Examples 1 to 9 respectively provide negative photoresist developer compositions of different components and proportions. The weight fractions of each negative photoresist developer composition are shown in Table 1:
[0155] Table 1
[0156]
[0157]
[0158] The negative photoresist developer composition is prepared by the following steps:
[0159] S1. Weigh the amidine compound, buffer, Gemini surfactant, compound solubilizer, leveling regulator, antifouling promoter and ultrapure water according to the formula raw materials and proportions for later use.
[0160] S2. While stirring, add 1 / 2 amount of water, amidine compound, composite solubilizer and buffer to the preparation kettle A in sequence, stir and mix at 30°C for 1.5 hours until uniform, then slowly add anti-fouling promoter, continue stirring and dissolving at 30°C for 45 minutes to obtain mixed solution A; add the remaining 1 / 2 amount of water to the preparation kettle B, slowly add Gemini surfactant under stirring, stir at 30°C for 1.2 hours to obtain mixed solution B.
[0161] S3. While stirring, slowly inject the mixed solution A into the mixing kettle containing the mixed solution B. After the addition is completed, continue stirring at 30° C. for 45 minutes to obtain a developer composition.
[0162] S4, filtering the developer composition in series with 0.5 μm and 0.1 μm filters to obtain a final negative photoresist developer composition product.
[0163] Example 10
[0164] This embodiment provides a negative photoresist developer composition, which is different from Example 1 only in that the amidine compound DBN is replaced by an amidine compound TBD (1,5,7-triazabicyclo[4.4.0]decene-5-ene) of equal mass, and other components and preparation methods are consistent with Example 1.
[0165] Embodiment 11
[0166] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that ammonium gluconate is replaced with ammonium benzoate of equal mass, and other components and preparation methods are consistent with those of Embodiment 1.
[0167] Example 12
[0168] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that 1-aminoethyl-3-methylimidazolium tetrafluoroborate is replaced with an equal mass of N-butylpyridinium tetrafluoroborate, and other components and preparation methods are consistent with Embodiment 1.
[0169] Embodiment 13
[0170] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the amount of Z1 is reduced to 6 parts, the amount of L1 is increased to 9 parts, and the other components and preparation methods are consistent with Embodiment 1.
[0171] Embodiment 14
[0172] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the amount of Z1 is increased to 14 parts, the amount of L1 is reduced to 1 part, and the other components and preparation method are consistent with Embodiment 1.
[0173] Embodiment 15
[0174] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 2 only in that the amount of Z1 is reduced to 0.5 parts, and the amount of L1 is increased to 1.5 parts. Other components and preparation methods are consistent with those of Embodiment 2.
[0175] Example 16
[0176] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 2 only in that the amount of Z1 is increased to 1.5 parts, the amount of L1 is reduced to 0.5 parts, and the other components and preparation methods are consistent with those of Embodiment 2.
[0177] Embodiment 17
[0178] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the surfactant TMDD is replaced by an equal mass of hexadecyldimethylethylenediamine salt, and the other components and preparation method are consistent with those of Embodiment 1.
[0179] Embodiment 18
[0180] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the buffer H1 is replaced with an equal mass of sodium citrate, and other components and preparation methods are consistent with Embodiment 1.
[0181] Embodiment 19
[0182] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the anti-fouling promoter K1 is replaced with an equal mass of perfluorononylbenzenesulfonic acid, and the other components and preparation method are consistent with those of Embodiment 1.
[0183] Embodiment 20
[0184] This embodiment provides a negative photoresist developer composition, which is different from Embodiment 1 only in that the leveling regulator THBP is replaced with an equal mass of 2-hydroxy-4-methoxybenzophenone, and other components and preparation methods are consistent with Embodiment 1.
[0185] Comparative Examples 1 to 5
[0186] Comparative Examples 1 to 5 provide negative photoresist developer compositions of different components and proportions, respectively. The weight fractions of each negative photoresist developer composition are shown in Table 2:
[0187] Table 2
[0188]
[0189] Comparative Example 6
[0190] This comparative example provides a negative photoresist developer composition, which is different from Example 1 only in that the amidine compound DBN is replaced by an equal mass of monoethanolamine, and the other components and preparation method are consistent with Example 1.
[0191] Comparative Example 7
[0192] This comparative example provides a negative photoresist developer composition, which is different from Example 1 only in that organic acid ammonium Z1 is no longer added, the content of ionic liquid L1 is increased to 15 parts, and other components and preparation methods are consistent with Example 1.
[0193] Comparative Example 8
[0194] This comparative example provides a negative photoresist developer composition, which is different from Example 1 only in that the ionic liquid L1 is no longer added, the content of the organic acid ammonium Z1 is increased to 15 parts, and the other components and preparation method are consistent with Example 1.
[0195] Test Case
[0196] Test samples: the negative photoresist developer compositions provided in Examples 1 to 20 and the negative photoresist developer compositions provided in Comparative Examples 1 to 8.
[0197] Test method: The developing effect, developing residue, developing efficiency, substrate corrosion, operating temperature range, foaming, re-tack, and developing capacity of the negative photoresist developer provided by the present invention were evaluated according to the following method:
[0198] ① Manufacturing of test samples with photoresist film layer:
[0199] A glass substrate with a size of 50 mm×50 mm is used as a substrate, and A glue (negative OC photoresist) or B glue (negative wiring photoresist) with a thickness of 0.8 to 1.2 μm is coated by spin coating. The specific steps are as follows: (1) The glass substrate is cleaned with a special glass cleaning liquid, and then rinsed with high-purity water and dried for standby use; (2) The substrate is placed on a support body in a coating machine, and a layer of photoresist is evenly coated on the substrate at a certain speed under a vacuum state; (3) The coated substrate is placed on a 110° C. hot plate for baking and curing for 120 seconds, and after curing, it is cooled to room temperature for standby use; (4) A mask is placed on the glass substrate obtained in step (3), and an i-line 365 nm ultraviolet photolithography machine is used for exposure, thereby obtaining a test sample with a photoresist film layer.
[0200] ②Development effect:
[0201] The developer composition sample provided above was diluted 20 to 500 times, and the test sample was immersed in the diluted developer for development, and then taken out and rinsed with ultrapure water for 100 seconds. After drying with nitrogen, the developed test sample was obtained. The pattern on the substrate was observed with an optical microscope to see whether it was clear and the edge was flat. The evaluation criteria were as follows:
[0202] ☆: The graphics are clear, the edges are clean, and the surface is smooth without burrs;
[0203] ★: The graphics are clear, the edges are clean, and there are no uneven or rough edges;
[0204] ×: The image is not clear and the edges are not clean.
[0205] ③Development residue:
[0206] Use a scanning electron microscope to observe whether there is residue in the pixel-free area of the pattern area of the above substrate after development. The evaluation criteria are as follows:
[0207] ◇: No residue;
[0208] ◆: Small amount of residue;
[0209] ※:Large amount of residue.
[0210] ④Development line loss:
[0211] The developed test piece was optically observed, and the actual line width of the 10μm line was measured. The difference between the actual line width and the theoretical line width was taken. The evaluation criteria were as follows:
[0212] I: CD loss ≤ 0.5 μm;
[0213] II: 0.5μm<CD loss≤0.8μm;
[0214] III: CD loss>0.8μm.
[0215] ⑤Corrosiveness:
[0216] The developed test piece was split and the effect of the developer on the coating on the glass substrate under the SEM electron microscope was checked. The evaluation criteria were as follows:
[0217] ○: non-corrosive;
[0218] ●: There is a slight amount of corrosion;
[0219] ×: There is obvious corrosion.
[0220] ⑥ Foaming property:
[0221] 20 mL of each developer composition sample was added to a 100 mL measuring cylinder, vertically shaken 30 times within 15 seconds, and the foam height was measured after standing for 15 minutes. The evaluation criteria were as follows:
[0222] □: less than 2 cm;
[0223] ■: Between 2 and 4 cm;
[0224] ×: 4cm or more.
[0225] ⑦Process temperature range:
[0226] Take 40 mL of each developer composition sample and place it in a 100 mL beaker, put it in a magnetic stirring water bath, and slowly heat it under stirring. Use an electronic thermometer to measure the temperature of the developer in the beaker, record the temperature when the developer becomes turbid and reaches the turbidity point, then slowly cool the beaker, and read the temperature again when the developer is clear. After averaging the above turbid temperature and the clear temperature, make the following evaluation criteria based on the following temperatures:
[0227] △: above 43℃, wide temperature range;
[0228] ▲: 40~43℃, moderate temperature range;
[0229] ×: Below 35°C, the temperature range is narrow.
[0230] ⑧Development capacity level
[0231] Take 200 mL of each of the above developer composition samples, add 2 g of glue A or glue B, mix and shake well, filter with 3 μm filter paper, and then dry the filter paper at 100°C to constant weight. Weigh the weight of the filter paper to obtain the net weight G of the filter paper. The evaluation criteria are as follows:
[0232] √: When R≤0.02g, the dispersion stability is good;
[0233] ※: 0.02g<R<0.04g, dispersion stability is average;
[0234] ×: R≥0.04g, the dispersion stability is poor.
[0235] ⑨ Degree of back adhesion:
[0236] Take 200 mL of negative photoresist developer with the dilution ratio in Table 3, add 2 g of photoresist A or photoresist B, mix and stir, and continue to soak the developed and well-developed test piece in it for 120 seconds. Take out and observe the surface of the test piece with an OM lithography microscope to see if there is any sticking or scum. The evaluation criteria are as follows:
[0237] A: There is no scum or adhesive on the glue line and non-glue line areas of the test piece;
[0238] B: There is a very small amount of scum or back-adhesion on the glue line or non-glue line area of the test piece;
[0239] C: There is obvious scum or back-adhesion on the glue line or non-glue line area of the test piece.
[0240] ⑩Development consistency:
[0241] Take 200 mL of negative photoresist developer with the dilution ratio in Table 3, develop 10 test pieces continuously, and then observe the development effect and consistency of the development line loss of each test piece with an OM lithography microscope. The evaluation criteria are as follows:
[0242] A: The development results of the 10 test pieces are consistent;
[0243] B: The development results of the 10 test pieces are generally consistent;
[0244] C: The consistency of the development effect and the development line loss of the 10 test pieces is poor.
[0245] The specific evaluation results are shown in Table 3 and Table 4:
[0246] Table 3
[0247]
[0248]
[0249] Table 4
[0250]
[0251]
[0252] As shown in Table 3 and Table 4, the negative photoresist developers prepared in Examples 1-9 of the present invention have good defoaming properties, developing capacity and corrosion inhibition, and show good developing performance and a wide process temperature range. The graphics after development are clear, the edges are clean, and the surface is flat without burrs. The loss of the developing line after development is small, no residue appears, and the developing consistency and anti-sticking performance are excellent. Figure 1 to Figure 6 As shown; Comparative Examples 1 and 2 without Gemini surfactant both had poor development effects, and the development capacity level and development consistency became worse. In addition, Comparative Example 2, in which the amidine compound in Comparative Example 1 was further replaced with NaOH, also showed obvious corrosiveness; and Comparative Example 3, in which the amidine compound was replaced with KOH or the ionic liquid component was not added to the formula, as well as Comparative Example 4 without anti-fouling and anti-adhesive agent and Comparative Example 5 without corrosion inhibitor all showed some insufficient performance, and all failed to obtain good development results.
[0253] From the comparison between Example 1 and Example 10, it can be seen that when an ether compound having a structure not preferred in the present application is selected as the main raw material, its dissolution or softening and peeling effect is reduced compared with that of Example 1.
[0254] From the comparison between Example 1 and Examples 11 to 12, it can be seen that the organic acid ammonium and ionic liquid selected as the compound solubilizer which are not preferred in the present application are more corrosive to various substrates and have poorer development consistency than Example 1.
[0255] From the comparison between Example 1 and Examples 13 to 14, and between Example 2 and Examples 15 to 16, it can be seen that the ratio of the compounded solubilizer does not satisfy Formula II / Formula I of the present application, that is, the ratio of the organic acid ammonium and the ionic liquid is not within the preferred range, which directly affects the use effect of the developer. Compared with Example 1 or 2, it is more corrosive to various substrates, and not only does it cause re-sticking, but the development consistency is also poor.
[0256] From the comparison between Example 1 and Example 17, it can be seen that the Gemini surfactant with a non-preferred structure of the present application has poor wettability and affinity for the photoresist component and cannot produce a good synergistic effect with the ionic liquid, so it is more likely to corrode the substrate during the development process.
[0257] From the comparison between Example 1 and Example 18, it can be seen that the selection of a buffering agent that is not of the preferred structure of the present application has limited effect on maintaining development stability and maintaining the service life of the developer.
[0258] From the comparison between Example 1 and Example 19, it can be seen that if an anti-fouling promoter other than the preferred structure of the present application is selected, it is difficult to cooperate with the Gemini surfactant to improve the wettability of the developer to the photoresist and the glass substrate, and as the concentration of the photoresist component in the later developer increases, it is more likely to cause back-sticking contamination to the glass substrate.
[0259] From the comparison between Example 1 and Example 20, it can be seen that when a leveling regulator having a structure other than the preferred structure of the present application is selected, the yield of the subsequent coating or gluing process is relatively poor.
[0260] From the comparison between Example 1 and Comparative Example 6, it can be seen that when the organic base is selected as the main raw material for developing imaging, the problem of poor developing effect occurs, the bubble performance is poor, and the developing capacity level and the developing consistency are significantly reduced.
[0261] From the comparison between Example 1 and Comparative Examples 7 to 8, it can be seen that the lack of any one of the compound solubilizers will cause the developer to more easily produce back-adhesion pollution on the glass substrate, and the development consistency will be significantly reduced; among them, the lack of organic ammonium acid will also lead to a significant decrease in the development capacity level, and the lack of ionic liquid will cause the developer to show obvious corrosiveness.
[0262] In summary, the present invention uses amidine compounds as alkaline source developers, which have the developing ability of strong alkalis and are less corrosive than inorganic alkalis and ammonium hydroxide organic alkalis; adding a buffer can effectively avoid the problem of the traditional developer having a reduced developing ability and easily generating developing residues after a period of use; the ionic liquid in the formula has both a solubilizing effect and a corrosion inhibition effect on the substrate and the contact metal layer during the development process; a low-foaming Gemini surfactant is used to increase the wettability and affinity of the developer composition to the photoresist glue component, which is also a key component to improve the compounding stability of the developer composition, and enables the developer to have a low-bubble or no-foaming effect during the spray development process. In addition, the negative photoresist developer prepared by the present invention can be diluted by a high multiple and has the characteristics of a wide process temperature range, has the advantages of low transportation costs, and is not easy to produce back-sticking and residues after continuous development.
[0263] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A negative photoresist developer composition, It is characterized in that The negative photoresist developer composition comprises, by mass: 0.1-34 parts of amidine compounds, 2-18 parts of compound solubilizers, 0.8-32 parts of Gemini surfactants, 0.1-8 parts of buffers, 0.5-20 parts of antifouling promoters, and 0.4-7 parts of leveling regulators; Wherein, the composite solubilizing agent comprises organic acid ammonium and ionic liquid.
2. The negative photoresist developer composition according to claim 1, It is characterized in that The amidine compound is selected from 1,5-diazabicyclo[4.3.0]non-5-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,8-diazabicyclo[5.4.0]undec-7-ene formate, 1,8-diazabicyclo[5.4.0]undec-7-ene octanoate, 1,4-diazabicyclo[2.2.2]octane, 1,8-diazabicyclo[5.4.0]undec-7-ene acetate, Any one of 1,5-diazabicyclo[4.3.0]non-5-ene acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene methoxy acetate, 1,5-diazabicyclo[4.3.0]non-5-ene methoxy acetate, 1,8-diazabicyclo[5.4.0]undec-7-ene ethoxy acetate or 1,5-diazabicyclo[4.3.0]non-5-ene ethoxy acetate or a combination of at least two thereof.
3. The negative photoresist developer composition according to claim 1, It is characterized in that The mass ratio of the organic acid ammonium and the ionic liquid satisfies the following formula I and formula II: When 2%≤M 1 +M 2 ≤5%, 0.8≤M 2 / M 1 ≤2Formula I; When 5%<M 1 +M 2 ≤18%, 0.1≤M 2 / M 1 ≤1 Formula II; Among them, M 1 represents the percentage of the organic acid ammonium in the total mass of the negative photoresist developer composition, M 2 represents the percentage of the ionic liquid in the total mass of the negative photoresist developer composition; Preferably, the organic ammonium acid is selected from any one or a combination of at least two of ammonium gluconate, ammonium tartrate, ammonium alginate, ammonium benzoate, ammonium citrate or ammonium maleate, preferably any one or a combination of at least two of ammonium maleate, ammonium gluconate or ammonium alginate; Preferably, the ionic liquid comprises an imidazole ionic liquid as shown in the following formula I: Wherein, R is selected from C1 to C3 straight chain alkyl, anion X - Any one selected from bromide ion, nitrate ion, tetrafluoroborate ion, hexafluorophosphate ion or bis(trifluoromethanesulfonyl)imide ion; Preferably, the ionic liquid is selected from any one of 1-aminoethyl-3-methylimidazolium bromide, 1-aminoethyl-3-methylimidazolium nitrate, 1-aminoethyl-3-methylimidazolium tetrafluoroborate, 1-aminoethyl-3-methylimidazolium hexafluorophosphate, 1-aminoethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-aminopropyl-3-methylimidazolium bromide, 1-aminopropyl-3-methylimidazolium nitrate, 1-aminopropyl-3-methylimidazolium tetrafluoroborate, 1-aminopropyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide or 1-aminopropyl-3-methylimidazolium hexafluorophosphate, or a combination of at least two thereof, preferably 1-aminoethyl-3-methylimidazolium tetrafluoroborate and / or 1-aminopropyl-3-methylimidazolium tetrafluoroborate.
4. The negative photoresist developer composition according to claim 1, It is characterized in that The Gemini surfactants include the Gemini surfactants shown in the following formula II: Wherein, R' is selected from C1-C5 straight or branched alkyl, and R" is selected from methyl or hydroxyl; Preferably, the Gemini surfactant is selected from any one or a combination of at least two of 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 4,7-dimethyl-5-decyne-4,7-diol, 2,5,8,11-dimethyl-6-dodecyne-5,8-diol or 3,6-dimethyl-4-octyne-3,6-diol, preferably 2,4,7,9-tetramethyl-5-decyne-4,7-diol and / or 4,7-dimethyl-5-decyne-4,7-diol.
5. The negative photoresist developer composition according to claim 1, It is characterized in that The buffer is selected from 2-amino-2-hydroxymethyl-1,3-propanediol and / or 2-bis(2-hydroxyethyl)amino-2-hydroxymethyl-1,3-propanediol, preferably 2-amino-2-hydroxymethyl-1,3-propanediol.
6. The negative photoresist developer composition according to claim 1, It is characterized in that The anti-fouling promoter is selected from fluorine-containing compounds; Preferably, the fluorine-containing compound includes a fluorine-containing compound as shown in the following formula III: Wherein, R'' is selected from C1-C5 straight or branched perfluoro substituted alkyl; Preferably, the fluorine-containing compound is selected from any one of perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid, perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid or perfluoro-2,5-dimethyl-3,6-dioxanononanoic acid or a combination of at least two thereof, preferably perfluoro-2,5-dimethyl-3,6-dioxaheptanoic acid and / or perfluoro-2,5-dimethyl-3,6-dioxaoctanoic acid.
7. The negative photoresist developer composition according to claim 1, It is characterized in that The leveling regulator is selected from 2,3,4-trihydroxybenzophenone; Preferably, the negative photoresist developer composition further comprises a solvent; Preferably, the solvent comprises water; Preferably, the amount of water added is 20 to 90 parts.
8. A method for preparing a negative photoresist developer composition according to any one of claims 1 to 7, It is characterized in that The preparation method comprises the following steps: The amidine compound, the composite solubilizer, the Gemini surfactant, the buffer, the anti-fouling accelerator and the leveling regulator are mixed according to a proportion to obtain the negative photoresist developer composition.
9. The method for preparing the negative photoresist developer composition according to claim 8, It is characterized in that The preparation method comprises the following steps: (a) stirring and mixing the amidine compound, the composite solubilizer, the buffer and part of the solvent for the first time, and then adding the antifouling promoter for the second time to obtain a mixed solution A; adding the Gemini surfactant to the remaining solvent, stirring and mixing, to obtain a mixed solution B; (b) adding the mixed solution A to the mixed solution B and stirring and mixing to obtain the negative photoresist developer composition; Preferably, in step (a), the partial solvent accounts for 40 to 60% of the total mass of the solvent; Preferably, in the process of preparing the mixed solution A in step (a), the first stirring and mixing time is 1 to 2 hours; Preferably, in the process of preparing the mixed solution A in step (a), the second stirring and mixing time is 0.5 to 1 h; Preferably, in the process of preparing the mixed solution B in step (a), the stirring and mixing time is 1 to 1.5 hours; Preferably, in the process of preparing the negative photoresist developer composition in step (b), the stirring and mixing time is 0.5 to 1 h; Preferably, the stirring and mixing temperatures in step (a) and step (b) are independently 15 to 45° C.; Preferably, step (b) is followed by step (c): filtering the negative photoresist developer composition in series using filters with pore sizes of 0.5 μm and 0.1 μm to obtain a finished product of the negative photoresist developer composition.
10. Use of the negative photoresist developer composition according to any one of claims 1 to 7 in the manufacture of integrated circuits, flat panel displays or semiconductor lighting chips.
Citation Information
Cited By
Crown ether type surfactant, preparation method thereof and photoresist developing solution
CN119735573A
Crown ether surfactant, preparation method thereof, and photoresist developer
CN119735573B