Preparation method and application of coating film of tantalum capacitor, and tantalum capacitor

Through the combination of impregnation decomposition method and electrolysis method, a uniform and continuous manganese dioxide layer is formed, which solves the problem of difficulty in capacitance in tantalum capacitors, improves the performance and stability of the capacitor, reduces the number of impregnations, and reduces the dielectric layer risk of deterioration.

CN118888331APending Publication Date: 2024-11-01CHINA ZHENHUA GRP XINYUN ELECTRONICS COMP ANDDEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410966656.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing methods are difficult to form a uniform and continuous manganese dioxide layer in the tantalum capacitors, which leads to difficulty in capacitance. Especially during the process of reducing the particle size of the tantalum powder, repeated impregnation leads to deterioration of the Ta2O5 dielectric layer.

Method used

By combining impregnation decomposition and electrolysis, the impregnation decomposition method forms a first coat layer on the surface of the tantalum substrate and the internal voids. The electrolysis method forms a second coat layer in the internal voids. The manganese dioxide layer uniformly covers and fills the first coat layer. to improve the capacity extraction capability.

Benefits of technology

Through this method, the coating rate and capacitance output of manganese dioxide are significantly improved, the number of repeated impregnation and decomposition methods is reduced, the risk of deterioration of Ta2O5 dielectric layer is reduced, and the product quality and capacitor performance are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118888331A_ABST
    Figure CN118888331A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a coating of a tantalum capacitor and the tantalum capacitor, and relates to the technical field of capacitors. Comprising the steps that a first coating layer is formed on the surface of a tantalum substrate and in internal gaps through a dipping decomposition method, a prefabricated part is prepared, a second coating layer is formed in the internal gaps of the prefabricated part through an electrolytic method, the gaps of the first coating layer are covered and / or filled with the second coating layer, and the first coating layer and the second coating layer are both manganese dioxide layers. The immersion decomposition method and the electrolytic method are combined, the immersion decomposition method can react on the surface of the tantalum matrix and in gaps which can enter the tantalum matrix to generate manganese dioxide, and the manganese dioxide can be uniformly distributed on the surface of the first coating layer along current through the decomposition effect of the electrolytic method; or the manganese dioxide layer is covered in a gap where the first coating layer cannot penetrate, and is connected with the first coating layer to form a continuous and uniform manganese dioxide layer, so that the capacity lead-out effect of the capacitor is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of capacitors, and in particular to a method for preparing a tantalum capacitor film and an application thereof, and a tantalum capacitor. Background Art

[0002] Solid electrolyte chip tantalum electrolytic capacitors are one of the most important basic electronic components in electronic engineering and are widely used in communication equipment, audio-visual systems, electrical instruments and other fields. The coating process is the process of coating the solid electrolyte manganese dioxide on the tantalum oxide film. Through the overall coating of manganese dioxide on the surface and inside of the tantalum oxide film, the capacitance of the capacitor can be drawn from the anode along the manganese dioxide on the surface to the cathode. Therefore, the uniform and continuous coating of manganese dioxide on the surface of the tantalum oxide film is crucial for the extraction of the capacitor capacity.

[0003] With the rapid development of electronic technology, tantalum electrolytic capacitors are developing rapidly towards miniaturization, large capacity, high reliability and long life. Therefore, tantalum electrolytic capacitors require tantalum powder to have high specific capacity or ultra-high specific capacity. The particle size of such high specific capacity or ultra-high specific capacity tantalum powder is smaller, resulting in a large number of small internal voids in the tantalum block formed. Manganese dioxide prepared by existing methods cannot penetrate into these tiny voids, resulting in difficulty in extracting capacity.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a tantalum capacitor film and its application, and a tantalum capacitor.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for preparing a film of a tantalum capacitor, comprising forming a first film layer on the surface and internal voids of a tantalum substrate by an immersion decomposition method to obtain a preform, and forming a second film layer in the internal voids of the preform by an electrolysis method, wherein the second film layer covers and / or fills the voids of the first film layer, and both the first film layer and the second film layer are manganese dioxide layers.

[0008] In a second aspect, the present invention provides a tantalum capacitor, using the material prepared by the preparation method of any one of the aforementioned embodiments as the anode and the dielectric layer, and using carbon / silver as the cathode.

[0009] In a third aspect, the present invention provides an application of a material prepared by the preparation method according to any one of the aforementioned embodiments in improving the capacity extraction of a tantalum capacitor.

[0010] The present invention has the following beneficial effects:

[0011] The present invention provides a tantalum capacitor film preparation method and its application, and a tantalum capacitor. By combining an immersion decomposition method and an electrolysis method, the immersion decomposition method can react to generate manganese dioxide on the surface of a tantalum substrate and in the internal accessible gaps. The preform obtained by the immersion decomposition method is subjected to an electrolysis method. Due to the electrolysis, the manganese dioxide can be evenly distributed on the surface of a first film layer along the current, or covered in gaps that the first film layer cannot penetrate, and connected to the first film layer to form a continuous and uniform manganese dioxide layer. When applied to tantalum capacitors, the uniform distribution of manganese dioxide on the surface of the tantalum substrate and the internal channels can improve the lead-out of the capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0013] Figure 1 A schematic diagram of the structure of a tantalum capacitor provided as an experimental example of the present invention. DETAILED DESCRIPTION

[0014] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0015] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0016] In a first aspect, the present invention provides a method for preparing a film of a tantalum capacitor, comprising forming a first film layer on the surface and internal voids of a tantalum substrate by an immersion decomposition method to obtain a preform, and forming a second film layer in the internal voids of the preform by an electrolysis method, wherein the second film layer covers and / or fills the voids of the first film layer, and both the first film layer and the second film layer are manganese dioxide layers.

[0017] Among them, the tantalum substrate includes an anode formed of pure tantalum and a Ta2O5 dielectric layer formed on one side of the pure tantalum. The formation process of the Ta2O5 dielectric layer can be prepared by existing methods, such as anodizing, oxidizing one side of the pure tantalum to generate Ta2O5. Since the internal structure of Ta2O5 is loose and porous, the manganese dioxide layer formed by the first film layer and the second film layer covers the surface of the tantalum substrate and the gaps inside the Ta2O5 dielectric layer.

[0018] Due to the requirements of miniaturization, large capacity, high reliability and long life for tantalum electrolytic capacitors, tantalum powder needs to have high specific capacity or ultra-high specific capacity. The particle size of such high specific capacity or ultra-high specific capacity tantalum powder is smaller, resulting in small and numerous gaps inside the Ta2O5 dielectric layer. In order to ensure that the gaps inside the Ta2O5 dielectric layer are all covered by MnO2, the tantalum substrate is currently immersed in a manganese-containing solution and then thermally decomposed to generate MnO2 on the surface and in the gaps inside the tantalum substrate to extract the capacitance.

[0019] However, the inventors have found that with the development of tantalum capacitors, the particle size of tantalum powder has decreased, and the gaps inside the Ta2O5 dielectric layer have become smaller and their number has increased. In order to cover all the gaps inside the Ta2O5 dielectric layer with a manganese dioxide layer, repeated impregnation is required. However, repeated impregnation will also be accompanied by multiple thermal decompositions, which will cause the Ta2O5 dielectric layer to degrade and affect product performance.

[0020] The present invention adopts a combination of an impregnation decomposition method and an electrolysis method for preparation. The first coating layer prepared by the impregnation decomposition method covers the surface of the tantalum substrate and the gaps inside the Ta2O5 dielectric layer. Then, the electrolysis method is used to electrolyze and generate MnO2 in the gaps of the Ta2O5 dielectric layer inside the tantalum substrate. Since the electrolysis method is implemented by the flow of electric current, it can penetrate into the smaller gaps inside the Ta2O5 dielectric layer to achieve the growth of MnO2, thereby ensuring that more capacitance can be drawn out, which is conducive to promoting the innovation and progress of tantalum capacitors.

[0021] The present invention combines the impregnation decomposition method with the electrolysis method to not only improve the coverage rate of manganese dioxide and increase the capacitance extraction, but also reduce the number of repetitions of the impregnation decomposition method, reduce the possibility of degradation of the Ta2O5 dielectric layer, and ensure product quality.

[0022] In an optional embodiment, in order to ensure that the manganese dioxide layer can be evenly coated and continuously covered on the surface of the tantalum substrate and ensure the capacitance extraction capability, it is necessary to repeat the immersion decomposition method at least twice to form the first coating layer.

[0023] However, multiple impregnations may lead to degradation of the Ta2O5 dielectric layer in the tantalum matrix. Therefore, preferably, the impregnation decomposition method is repeated ≤ 10 times; more preferably, the impregnation decomposition method is repeated 3 to 8 times.

[0024] In an optional embodiment, the impregnation decomposition method includes impregnating the tantalum substrate in a manganese-containing impregnation solution, and after the impregnation is completed, dehydration, decomposition and cooling are performed in sequence.

[0025] In an optional embodiment, the impregnation time is 2 minutes to 15 minutes, for example, it can be any value among 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes or 15 minutes, or a range surrounded by any two of the above values, and any value within the range. The purpose of impregnation is to allow the manganese-containing impregnation solution to fully enter the voids inside the Ta2O5 dielectric layer so that during thermal decomposition, MnO2 is generated by in-situ reaction in the voids. Therefore, sufficient impregnation time is required to ensure the depth of the manganese dioxide layer entering the voids and the thickness of the manganese dioxide layer.

[0026] After the impregnation is completed, it is necessary to remove the moisture in the manganese-containing impregnation solution remaining on the surface and inside of the tantalum substrate, so the tantalum substrate needs to be dehydrated, and the dehydration temperature is 60°C to 120°C, for example, it can be any value of 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, or a range surrounded by any two of the above values, and any value within the range; the dehydration time is 2min to 15min, for example, it can be any value of 2min, 3min, 4min, 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min, or a range surrounded by any two of the above values, and any value within the range.

[0027] After dehydration is completed, the tantalum substrate is thermally decomposed so that the manganese ions remaining in the manganese-containing impregnation solution react in situ to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The decomposition temperature is 200°C to 350°C, for example, it can be any value of 200°C, 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, 340°C or 350°C, or a range surrounded by any two of the above values, and any value within the range; the decomposition time is 4min to 15min, for example, it can be any value of 4min, 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min, or a range surrounded by any two of the above values, and any value within the range.

[0028] The tantalum substrate after thermal decomposition is taken out and cooled at room temperature. The cooling time is 6 minutes to 20 minutes. For example, it can be any value among 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes or 20 minutes, or a range surrounded by any two of the above values, and any value within the range.

[0029] In an optional embodiment, in order to ensure the performance and morphology of the manganese dioxide layer, the concentration of the solute in the manganese-containing impregnation solution is 0.75 g / cm 3 ~2.05g / cm 3 ; For example, it can be 0.75g / cm 3 , 1.00g / cm 3 , 1.25g / cm 3 , 1.50g / cm 3 , 1.75g / cm 3 , 2.00g / cm 3 or 2.05g / cm 3 Any value in , or a range formed by any two of the above values, and any value in the range.

[0030] Preferably, the manganese-containing impregnation solution includes any one of manganese nitrate or manganese carbonate. For example, the solute in the manganese-containing impregnation solution may be manganese nitrate.

[0031] In an optional embodiment, the electrolysis method includes using the preform as an anode and the alloy material as a cathode, and performing electrolysis in a manganese-containing electrolyte. The flow of current during the electrolysis process forms a manganese dioxide layer in the gaps inside the Ta2O5 dielectric layer that are difficult for the manganese-containing impregnation solution to penetrate. The manganese dioxide layer formed by the electrolysis method and the manganese dioxide layer formed by the impregnation decomposition method together cover the surface and internal gaps of the tantalum substrate, which is beneficial to improving the extraction rate of the capacitance.

[0032] Preferably, the manganese-containing electrolyte is an aqueous solution of a soluble manganese salt, and the manganese-containing electrolyte includes one or more of potassium permanganate, potassium manganate, manganese sulfate, manganese nitrate, manganese acetate, and manganese chloride.

[0033] Preferably, the concentration of the solute in the manganese-containing electrolyte is 80-100 g / L, for example, it can be any value among 80 g / L, 82 g / L, 84 g / L, 86 g / L, 88 g / L, 90 g / L, 92 g / L, 94 g / L, 96 g / L, 98 g / L or 100 g / L, or a range surrounded by any two of the above values, and any value within the range.

[0034] Preferably, the electrolysis time is 6 to 10 hours, for example, it can be any value among 6 hours, 7 hours, 8 hours, 9 hours or 10 hours, or a range surrounded by any two of the above values, and any value within the range.

[0035] Preferably, the cell voltage is 2-5V, for example, it can be any value among 2V, 3V, 4V or 5V, or a range surrounded by any two of the above values, and any value within the range.

[0036] Preferably, the current intensity is 5-10A, for example, it can be any value among 5A, 6A, 7A, 8A, 9A or 10A, or a range surrounded by any two of the above values, and any value within the range.

[0037] By controlling the electrolysis parameters within the above range, it can be ensured that a layer of manganese dioxide is coated inside the Ta2O5 dielectric layer, thereby improving the capacitance extraction capability.

[0038] Preferably, the alloy material includes any one of a stainless steel plate, an aluminum alloy plate, a titanium alloy plate and a copper alloy plate.

[0039] In an optional embodiment, the method further includes drying and cooling the preform after electrolysis.

[0040] Preferably, the drying temperature is 70° C. to 100° C., the drying time is 20 min to 40 min, and the cooling is performed at room temperature for 5 min to 10 min.

[0041] In an alternative embodiment, the tantalum substrate is a tantalum block formed by pressing tantalum powder.

[0042] Preferably, the particle size of the tantalum powder is 1 to 5 μm.

[0043] In a second aspect, the present invention provides a tantalum capacitor, using the material prepared by the preparation method of any one of the aforementioned embodiments as the anode and the dielectric layer, and using carbon / silver as the cathode.

[0044] In a third aspect, the present invention provides an application of a material prepared by the preparation method according to any one of the aforementioned embodiments in improving the capacity extraction of a tantalum capacitor.

[0045] Example 1

[0046] This embodiment provides a method for preparing a tantalum capacitor film, comprising the following steps:

[0047] S01. Immersion decomposition method: The tantalum substrate formed by the anode of pure tantalum metal and the Ta2O5 dielectric layer is treated by the immersion decomposition method.

[0048] S011, immerse the tantalum substrate in 1.10g / cm 3 The tantalum substrate is placed in a manganese nitrate solution for 8 minutes, then dehydrated at 95°C for 8 minutes, and then placed in a coating furnace at a temperature of 250°C and an oxygen content of 5% for decomposition for 7 minutes, and finally cooled at room temperature for 6 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The above steps of S011 are repeated 3 times.

[0049] S012, immerse the tantalum substrate of step S011 in 1.52g / cm 3The tantalum substrate is placed in a manganese nitrate solution for 6 minutes, then dehydrated at 75°C for 6 minutes, and then placed in a coating furnace at a temperature of 270°C and an oxygen content of 5% for decomposition for 6 minutes, and finally cooled at room temperature for 6 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The above steps of S012 are repeated 3 times to obtain a preform. The preform has a first coating layer of MnO2 on the surface and inside of the tantalum substrate by an immersion decomposition method. The first coating layer completely covers the surface of the tantalum substrate and covers part of the surface of the internal voids of the Ta2O5 dielectric layer.

[0050] S02. Electrolysis

[0051] The preform obtained in step S012 is used as the anode and the stainless steel plate is used as the cathode. They are immersed in a solution with a manganese sulfate concentration of 90 g / L and electrolyzed for 8 hours, wherein the cell voltage is 3 V and the current intensity is 7.5 A. Then they are dried at 80°C for 30 minutes and finally cooled at room temperature for 6 minutes. The voids inside the tantalum matrix are filled with MnO2 produced by electrolysis, thereby increasing the coating area of ​​MnO2 inside the tantalum matrix and improving the capacitance extraction capability.

[0052] Example 2

[0053] This embodiment provides a method for preparing a tantalum capacitor film, comprising the following steps:

[0054] S01. Immersion decomposition method: The tantalum substrate formed by the anode of pure tantalum metal and the Ta2O5 dielectric layer is treated by the immersion decomposition method.

[0055] S011, immerse the tantalum substrate in 1.13g / cm 3 The tantalum substrate is placed in a manganese nitrate solution for 6 minutes, then dehydrated at 80°C for 6 minutes, and then placed in a coating furnace at a temperature of 255°C and an oxygen content of 5% for 8 minutes, and finally cooled at room temperature for 10 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The above steps of S011 are repeated 4 times.

[0056] S012, immerse the tantalum substrate of step S011 in 1.51g / cm 3 The tantalum substrate is placed in a manganese nitrate solution for 8 minutes, then dehydrated at 85°C for 5 minutes, and then placed in a coating furnace at a temperature of 273°C and an oxygen content of 5.5% for decomposition for 5 minutes, and finally cooled at room temperature for 10 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The above steps of S012 are repeated 4 times to obtain a preform. The preform has a first coating layer of MnO2 on the surface and inside of the tantalum substrate by an immersion decomposition method. The first coating layer completely covers the surface of the tantalum substrate and covers part of the surface of the internal voids of the Ta2O5 dielectric layer.

[0057] S02. Electrolysis

[0058] The preform obtained in step S012 is used as the anode and the stainless steel plate is used as the cathode. They are immersed in a solution with a manganese sulfate concentration of 80 g / L and electrolyzed for 8 hours, wherein the cell voltage is 3.5 V and the current intensity is 8 A. Then they are dried at 85°C for 40 minutes and finally cooled at room temperature for 6 minutes. The voids inside the tantalum matrix are filled with MnO2 produced by electrolysis, thereby increasing the coating area of ​​MnO2 inside the tantalum matrix and improving the capacitance extraction capability.

[0059] Comparative Example 1

[0060] This comparative example provides a method for preparing a tantalum capacitor film, and the specific steps are as follows:

[0061] S01. Immersion decomposition method: The tantalum substrate formed by the anode of pure tantalum metal and the Ta2O5 dielectric layer is treated by the immersion decomposition method.

[0062] S011, immerse the tantalum substrate in 1.10g / cm 3 The tantalum substrate is placed in a manganese nitrate solution for 8 minutes, then dehydrated at 95°C for 8 minutes, and then placed in a coating furnace at a temperature of 250°C and an oxygen content of 5% for decomposition for 7 minutes, and finally cooled at room temperature for 6 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate. The above steps of S011 are repeated 3 times.

[0063] S012, immerse the tantalum substrate of step S011 in 1.52g / cm 3 The tantalum substrate is placed in a manganese nitrate solution for 6 minutes, then dehydrated at 75°C for 6 minutes, and then placed in a coating furnace at a temperature of 270°C and an oxygen content of 5% for decomposition for 6 minutes, and finally cooled at room temperature for 6 minutes to form a manganese dioxide layer on the surface and inside of the tantalum substrate, and the above steps of S012 are repeated 3 times.

[0064] Comparative Example 2

[0065] This comparative example provides a method for preparing a tantalum capacitor film, and the different steps are similar to those of Example 1, except that MnO2 is prepared only by electrolysis.

[0066] Test Example 1

[0067] The same method was used to prepare the materials provided in Example 1, Example 2 and Comparative Examples 1-2 into B-shell tantalum capacitors and H-shell tantalum capacitors, respectively. Specifically, the tantalum capacitor uses the pure tantalum side of the tantalum matrix as the anode, the dielectric layer is the Ta2O5 dielectric layer of the tantalum matrix, and graphite and silver are formed on the surface of the dielectric layer as the cathode, such as Figure 1 As shown. Among them, the specifications of the tantalum capacitor in the B shell are 10V, 100μF; the specifications of the tantalum capacitor in the H shell are 10V, 1000μF.

[0068] The tantalum capacitors prepared above were subjected to performance tests using a TH2615E capacitance measuring instrument at a test frequency of 120 Hz, and the results shown in Table 1 below were obtained.

[0069] Table 1 Performance of Tantalum Capacitors

[0070] Capacity of B case / μF Capacity of H case / μF Example 1 97.5 937 Example 1 97.7 942 Comparative Example 1 91.5 866 Comparative Example 2 43.7 415

[0071] It can be seen from Table 1 that the actual capacity of the tantalum capacitor obtained by the method of the embodiment of the present invention is higher than the actual capacity of the tantalum capacitor obtained by the method of the comparative example, which shows that the method of the embodiment of the present invention can significantly improve the capacitance extraction capability.

[0072] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a tantalum capacitor film, characterized in that: The method comprises forming a first film layer on the surface and in the internal voids of a tantalum substrate by an impregnation decomposition method to obtain a preform, and forming a second film layer in the internal voids of the preform by an electrolytic method, wherein the second film layer covers and / or fills the voids of the first film layer, and both the first film layer and the second film layer are manganese dioxide layers; The tantalum substrate includes pure tantalum and a Ta2O5 dielectric layer formed on one side of the pure tantalum.

2. The preparation method according to claim 1, characterized in that: The impregnation decomposition method comprises placing the tantalum substrate in a manganese-containing impregnation solution for immersion, and after the impregnation is completed, dehydration, decomposition and cooling are performed in sequence.

3. The preparation method according to claim 2, characterized in that: The immersion time is 2 min to 15 min; the dehydration temperature is 60° C. to 120° C., and the dehydration time is 2 min to 15 min; the decomposition temperature is 200° C. to 350° C., and the decomposition time is 4 min to 15 min; and the cooling time is 6 min to 20 min.

4. The preparation method according to claim 2, characterized in that: The manganese concentration in the manganese-containing impregnation solution is 0.75 g / cm 3 ~2.05g / cm 3 ; Preferably, the manganese-containing impregnation solution comprises any one of manganese nitrate or manganese carbonate.

5. The preparation method according to any one of claims 2 to 4, characterized in that: The method comprises repeating the immersion decomposition method at least twice to form the first film layer; Preferably, the immersion decomposition method is repeated ≤ 10 times; more preferably, the immersion decomposition method is repeated 3 to 8 times.

6. The preparation method according to claim 1, characterized in that: The electrolysis method comprises using the preform as an anode, using the alloy material as a cathode, and performing electrolysis in a manganese-containing electrolyte; Preferably, the manganese-containing electrolyte is an aqueous solution of a soluble manganese salt, and the manganese-containing electrolyte includes one or more of potassium permanganate, potassium manganate, manganese sulfate, manganese nitrate, manganese acetate, and manganese chloride; Preferably, the alloy material includes any one of a stainless steel plate, an aluminum alloy plate, a titanium alloy plate and a copper alloy plate.

7. The preparation method according to claim 1 or 6, characterized in that: It also includes drying and cooling the preform after electrolysis; Preferably, the drying temperature is 70° C. to 100° C., the drying time is 20 min to 40 min, and the cooling is performed at room temperature for 5 min to 10 min.

8. The preparation method according to claim 1, characterized in that: The tantalum matrix is ​​a tantalum block formed by pressing tantalum powder; Preferably, the particle size of the tantalum powder is 1-5 μm.

9. A tantalum capacitor, characterized in that: The material prepared by the preparation method according to any one of claims 1 to 8 is used as the anode and the dielectric layer, and carbon / silver is used as the cathode.

10. Use of a material obtained by the preparation method according to any one of claims 1 to 8 in improving the capacity extraction of a tantalum capacitor.