Metal-gas battery based on flexible self-supporting carbon fiber catalyst
The flexible self-supported carbon fiber catalyst prepared through electrostatic textile technology solves the energy efficiency and cycle life of metal-gas batteries, achieves high-efficiency energy density and low-cost battery performance, and avoids the use of current collectors.
Patent Information
- Application Number
- CN202410914447.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
Metal-gas batteries have limited energy efficiency under high charging and discharge current density, short cycle life, existing catalyst preparation processes are complex and costly, and require loading on current collectors to reduce energy density.
Electrostatic textile technology is used to prepare flexible self-supporting carbon fiber catalysts rich in surface defects. As the positive electrode material of metal-gas batteries, catalytic activity is improved by doping precious metals or transition metal compounds into carbon fibers, and no current collectors are required.
It improves the energy utilization rate and energy density of the battery, reduces costs, extends the cycle life of the battery, and achieves high catalytic activity at low overpotentials, avoiding the reduction of volume energy density caused by the use of current collectors.
Smart Images

Figure CN118888933A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal-gas batteries, and in particular to a metal-gas battery based on a flexible self-supporting carbon fiber catalyst. Background Art
[0002] It is of great significance to develop renewable energy to reduce the use of fossil energy. The intermittent problem of renewable energy has stimulated the rapid development of energy storage equipment. Secondary batteries, as a high-efficiency electrochemical energy storage technology, are the most important research field in the current development of new energy; among them, high energy density, long cycle life, high safety and low cost are the top priorities in the development of secondary batteries.
[0003] Among secondary battery technologies, metal-gas batteries are considered to be one of the most promising devices, showing theoretical energy densities comparable to petroleum and being green and environmentally friendly. However, there are several huge challenges to their practical application, including limited energy efficiency - especially at high charge and discharge current densities, and limited cycle life. Unlike the intercalation reactions observed in lithium-ion batteries, discharge in metal-gas batteries involves oxygen reduction reactions occurring at multiphase interfaces, typically involving electrodes, electrolytes, and gases. This results in the production of solid discharge products that form electronically insulating deposits on the active surface, disrupting charge transport and significantly limiting battery performance.
[0004] Although many cathode catalyst materials have been explored, including precious metal-based catalysts, transition metal-based catalysts, and carbon material-based catalysts, the existing catalysts either have high costs due to complicated preparation processes or scarce raw materials, or have poor electrochemical performance of the battery due to low catalytic activity. In addition, the current catalysts need to be loaded on carbon paper or nickel foam current collectors, and the use of these current collectors greatly reduces the volume energy density or mass energy density.
[0005] Therefore, there is an urgent need to explore and develop new flexible self-supporting catalysts, which is an important strategy to accelerate the commercialization of metal-gas batteries. Designing a low-cost, high-catalytically active, and excellent-performance cathode catalyst will bring more application possibilities to metal-gas batteries. Summary of the invention
[0006] In view of the above problems existing in the prior art, the present invention provides a metal-gas battery based on a flexible self-supporting carbon fiber catalyst. The flexible self-supporting catalyst of the present invention has low cost, simple preparation method, and surface characteristics with high catalytic activity, which can solve the problems of low energy utilization and poor performance caused by high overpotential in metal-gas batteries. The use of the flexible self-supporting carbon positive electrode can eliminate the need for a current collector, greatly improving the energy density of the battery.
[0007] The technical solution of the present invention is as follows:
[0008] A metal-gas battery based on a flexible self-supporting carbon fiber catalyst, wherein the positive electrode of the metal-gas battery adopts a flexible self-supporting carbon fiber catalyst; the flexible self-supporting carbon fiber catalyst is a carbon fiber material rich in surface defects.
[0009] Furthermore, the flexible self-supporting carbon fiber catalyst is prepared by electrospinning technology.
[0010] Furthermore, the preparation process of the electrospinning technology includes the following steps:
[0011] S1. Dissolve polyacrylonitrile PAN powder in a solvent at room temperature, stir thoroughly to obtain a PAN solution, and load the solution into a syringe pump with a capillary;
[0012] S2, using a high voltage power supply to electrospin the needle tip, and using a rotating drum collector covered with a conductive thin layer to collect the spun fiber precursor;
[0013] S3, pre-oxidizing the collected precursor fiber film in air at 100-400° C. for 1-3 hours;
[0014] S4, keeping the pre-oxidized precursor at 750-950° C. for 1-10 hours under an argon atmosphere;
[0015] S5. Cool to room temperature in the furnace, turn off the argon gas, take out the sample, and obtain a flexible self-supporting carbon fiber catalyst with high surface catalytic activity.
[0016] Preferably, in step S1, the solvent includes N,N-dimethylformamide DMF, dimethyl sulfoxide, cyclopentane or ethyl nitrate. In step S1, the ratio of PAN to the solvent is not limited, and the stirring time is not limited, as long as PAN is completely dissolved. Preferably, the mass concentration of the dissolved PAN solution can be 1-50%; the stirring time can be 2-20 hours.
[0017] Preferably, in step S2, the high voltage power supply provides a voltage of 10-30 kV. In step S2, in order to ensure stable electrospinning, the PAN solution is added at a certain rate, preferably 0.1-100 uL / min.
[0018] The present invention further provides a metal-gas battery, wherein precious metals, transition metals, precious metal compounds, or transition metal compounds are doped into the flexible self-supporting carbon fiber to improve the electrocatalytic properties of the flexible self-supporting carbon fiber.
[0019] Preferably, the noble metal or transition metal includes molybdenum, cobalt, ruthenium, copper, iron, nickel or manganese.
[0020] Preferably, the noble metal compound includes phosphate, acetate, oxalate, carbonate, carbide, nitride, oxide, phosphide, sulfide, chloride, iodide, bromide, or fluoride of a noble metal;
[0021] Preferably, the transition metal compound includes phosphates, acetates, oxalates, carbonates, carbides, nitrides, oxides, phosphides, sulfides, chlorides, iodides, bromides, or fluorides of transition metals.
[0022] More preferably, the doping amount of the noble metal, transition metal, noble metal compound, or transition metal compound is 0.001-10 wt % of the raw material powder for preparing the flexible self-supporting carbon fiber catalyst.
[0023] Furthermore, the above-mentioned metal-gas batteries of the present invention include but are not limited to Li-O2, Na-O2, K-O2, Al-O2, Zn-O2, Mg-O2, Ca-O2, etc. and lithium-air batteries, sodium-air batteries, potassium-air batteries, aluminum-air batteries, zinc-air batteries, magnesium-air batteries, calcium-air batteries, etc.
[0024] The beneficial technical effects of the present invention are:
[0025] 1. The present invention uses the prepared flexible self-supporting carbon fiber with high surface catalytic activity as the positive electrode of the metal gas battery, which can effectively reduce the battery charge and discharge overpotential, thereby making the battery have a higher energy utilization rate. Through research, it is found that the reason is that the surface of the prepared carbon fiber has a higher degree of carbon defects.
[0026] In addition, the surface defect structure of carbon fiber can be regulated by compounding other materials (including precious metals, transition metals or their compounds, etc.). Under the premise of not affecting the toughness of carbon fiber, the electronic structure and catalytic properties of carbon fiber surface can be further regulated, showing higher catalytic activity of oxygen reduction and oxidation reactions in the tested metal-oxygen batteries and metal-air batteries.
[0027] 2. When the flexible self-supporting carbon fiber prepared by the present invention is used as the positive electrode of the metal gas battery, a current collector is not required, which greatly improves the battery energy density and has good flexibility, thus providing a possibility for the design of flexible batteries.
[0028] 3. The surface of the flexible self-supporting carbon fiber prepared by the present invention has a rich variety and number of defects (high I in Raman test). D / I G ratio), thus having a higher surface catalytic efficiency, and the performance can even exceed that of some precious metal catalysts. In addition, the flexible self-supporting carbon fiber preparation process provided by the present invention is simple, which greatly reduces the cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a SEM image of the flexible self-supporting carbon fiber prepared in Example 1;
[0030] Figure 2 This is the Raman test result of the flexible self-supporting carbon fiber prepared in Example 1;
[0031] Figure 3 is the original impedance of the metal-gas battery prepared in Example 1;
[0032] Figure 4 is the post-discharge impedance of the metal-gas battery prepared in Example 1;
[0033] Figure 5 The post-charge impedance of the metal-gas battery prepared in Example 1;
[0034] Figure 6 The first cycle charge and discharge results of the metal-gas battery prepared in Example 1;
[0035] Figure 7 The first cycle charge and discharge results of the metal-gas battery prepared in Comparative Example 1-1;
[0036] Figure 8 This is the first cycle charge and discharge result of the metal-gas battery prepared in Example 2. DETAILED DESCRIPTION
[0037] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Embodiment 1:
[0039] (1) First, a flexible self-supporting carbon fiber catalyst material is prepared, comprising the following steps:
[0040] S1. Dissolve 1 g of polyacrylonitrile (PAN) powder in 10 ml of N,N-dimethylformamide (DMF) at room temperature and stir for 12 hours to prepare a PAN solution of a certain concentration, which is then loaded into a plastic syringe pump with a capillary.
[0041] S2. Use a high voltage power supply to provide a voltage of 21 kV to the needle tip and the rotating drum collector covered with carbon paper. To ensure stable electrospinning, the solution is added at 5 μl / min. Then a flexible self-supporting carbon catalyst precursor is obtained.
[0042] S3. Pre-oxidize the flexible self-supporting carbon catalyst precursor in air at 260° C. for 2 hours.
[0043] S4. Keep the pre-oxidized flexible self-supporting carbon catalyst precursor at 950° C. for 2 hours in an argon atmosphere.
[0044] S5. Cool to room temperature in the furnace, turn off the argon gas, take out the sample, and obtain a flexible self-supporting carbon fiber catalyst.
[0045] The flexible self-supporting carbon fiber catalyst was cut into discs with a diameter of 12 mm. Scanning electron microscopy showed the morphology and structure as follows Figure 1 As shown in the figure, it can be seen that the diameter of the carbon fiber is about 200nm. The Raman test results are as follows Figure 2 As shown, the prepared flexible self-supporting carbon fiber catalyst has a high I D / I G , D peak originates from the six-carbon ring A 1g breathing mode, which is activated only when there is a defect, and the G peak corresponds to the E 2g phonons, which is proportional to the number of sp2-bonded carbon atoms. It is worth noting that I D / I G The ratio is a key indicator of carbon crystallinity and is often used to evaluate the quality of carbon nanomaterials. D / I G The ratio indicates the increase of defects and surface active sites, which manifests as higher catalytic reactivity in oxygen reduction reaction (ORR) and oxygen evolution reaction (OER) of metal-gas batteries.
[0046] (2) Preparation of metal-gas batteries:
[0047] The battery was assembled in a glove box filled with argon atmosphere using a CR2032 button-type battery case with a hole on one side, a hole diameter of 2 mm, and a hole density of 8 holes / cm 2 The negative electrode is a magnesium sheet, the positive electrode is a carbon-based catalyst with a diameter of 12 mm prepared by step (1), the electrolyte is a mixed solution of 0.5 M bis(trifluoromethylsulfonyl)imide magnesium dissolved in EMIMBF4 and triethylene glycol dimethyl ether (volume ratio of 1:9), and the diaphragm is a glass fiber diaphragm.
[0048] Place the positive electrode material on one side of the battery shell opening and the magnesium sheet on the other side of the battery shell, and assemble according to the normal assembly sequence of button batteries. Press the above components together in a button battery sealing machine to complete the battery assembly.
[0049] (3) Place the assembled battery in a 1000ml self-made sealed can, fill it with oxygen and seal it. At a current density of 200mA / g and a cut-off specific capacity of 500mAh / g, perform a discharge-then-charge test. The battery impedance is as follows: Figure 3-5 As shown in the figure, it can be seen that the original impedance of the battery is very small. After discharge, the impedance increases significantly, indicating that discharge products with poor conductivity are deposited. After charging, the impedance almost returns to its original state, indicating that the discharge products are almost completely decomposed during the charging process.
[0050] The results of the first cycle of charge and discharge are as follows Figure 6 As shown, the overvoltage is only 0.45V, indicating that it has high energy efficiency. The overvoltage of the magnesium-oxygen battery in the prior art is about 1.2V, which is 0.75V lower than that of the present invention, indicating that the spinning material prepared by the present invention has high catalytic activity and can undergo charge and discharge reactions at a lower overpotential, which significantly improves the energy efficiency of the battery. In addition, the prepared self-supporting catalyst material does not contain precious metal elements and has low material cost.
[0051] Comparative Example 1-1:
[0052] (1) Preparation of common positive electrode materials:
[0053] 5 mg of commercial graphene and 5 mg of conductive carbon black Super P were prepared into a mixed material. 10 mg of the mixed material was mixed with 50 mg of a 5 wt.% polyvinylidene fluoride solution (the solvent of the polyvinylidene fluoride solution was N-methylpyrrolidone), and N-methylpyrrolidone solvent was continuously added until the catalyst slurry had a suitable thickness, and then fully ground in an agate mortar until it was uniform.
[0054] The positive electrode material was uniformly coated on a pre-cut nickel foam substrate with a thickness of 0.3 mm and a diameter of 12 mm, and vacuum dried at 100° C. for 12 h.
[0055] The commercial graphene and the conductive carbon black Super P are loaded on the flaky nickel foam to form a porous conductive network structure with a pore size of 0.23 mm, and the open pore area of the overall electrode accounts for 98% of the total area.
[0056] Among them, the loading amount of commercial graphene is about 0.2mg / cm 2 .
[0057] (2) Preparation of metal-gas batteries:
[0058] The battery was assembled in a glove box filled with argon atmosphere using a CR2032 button-type battery case with a hole on one side, a hole diameter of 2 mm, and a hole density of 8 holes / cm 2The negative electrode is a magnesium sheet, the positive electrode is graphene and conductive carbon black Super P loaded on flaky nickel foam, the electrolyte is 0.5M bis(trifluoromethylsulfonyl)imide magnesium dissolved in a mixed solution of EMIMBF4 and triethylene glycol dimethyl ether (volume ratio of 1:9), and the diaphragm is a glass fiber diaphragm.
[0059] The positive electrode material is placed on one side of the battery shell opening, and the magnesium sheet is placed on the other side of the battery shell. The assembly can be carried out according to the normal assembly sequence of button batteries. The above components are pressed into one in a button battery sealing machine to complete the battery assembly.
[0060] (3) Place the assembled battery in a 1000ml self-made sealed can, fill it with oxygen and seal it. At a current density of 200mA / g and a cut-off specific capacity of 500mAh / g, perform a discharge-then-charge test. The results of the first cycle of charge and discharge are as follows: Figure 7 As shown, the battery overpotential is large, resulting in low energy utilization.
[0061] From the performance comparison, it can be seen that the carbon fiber electrode with rich defects on the surface prepared by the present invention has higher catalytic activity compared with this electrode, and can undergo charge and discharge reactions at lower overpotentials, significantly improving the energy efficiency of the battery, and has good conductivity and toughness, and can be used directly in the battery as a self-supporting electrode, avoiding the loss of active surface caused by the addition of binders in the additional electrode preparation process and the decrease in battery energy density caused by the use of current collectors.
[0062] Comparative Example 1-2:
[0063] (1) Preparation of nano-molybdenum carbide-carbon fiber composite catalyst positive electrode material.
[0064] According to the inventors’ previous research method “High-Rate Nonaqueous Mg–CO2 Batteries Enabled by Mo2C-Nanodot-Embedded Carbon Nanofibers” (Wenbo Liu et al., Small, Issue 20, 2023, https: / / doi.org / 10.1002 / smll.202306576), Mo2C-NDs@CNF catalyst material (Mo2C content is 39.9wt.%) was prepared by electrospinning technology.
[0065] (2) Preparation of metal-gas batteries: Since the obtained carbon fiber contains inorganic salt Mo2C, the fiber has poor toughness and cannot be used as a self-supporting electrode. Therefore, an electrode preparation process is still required. The method for preparing the battery is compared with that of Comparative Example 1-1, except that commercial graphene is replaced with Mo2C-NDs@CNF catalyst material, and the rest is the same.
[0066] (3) Test results: The overvoltage of the battery obtained in this comparative example in the metal oxygen battery is 0.6V, which is higher than 0.45V in Example 1, and the energy efficiency is relatively low. This is mainly due to the high content of Mo2C in the spun fiber of the document. When it is applied to oxygen or air batteries, the catalytic activity mainly comes from the surface defects of the carbon fiber. The excessively high Mo2C content affects the catalytic effect of the carbon fiber.
[0067] Comparative Examples 1-3:
[0068] (1) Preparation of RuO2 / Pt–C composite catalyst positive electrode material.
[0069] According to the research method of the existing literature "A Bismuth-Based Protective Layer for MagnesiumMetal Anode in Noncorrosive Electrolytes" (Yimin Zhao et al., ACS Energy Letters, Issue 6, 2021, https: / / doi.org / 10.1021 / acsenergylett.1c01243), RuO2 / Pt–C catalyst material was prepared by solution method.
[0070] (2) Preparation of metal-gas battery: The method for preparing the battery is the same as that of Comparative Example 1-1, except that the commercial graphene is replaced with RuO2 / Pt-C catalyst material dripped on carbon paper, and the rest is the same.
[0071] (3) Test results: The overvoltage of the battery prepared in this comparative example is 1.4V, which is higher than 0.45V of Example 1, and the energy efficiency is relatively low. This indicates that the spinning material prepared by the present invention has a high catalytic activity, and can undergo charge and discharge reactions at a relatively low overpotential, which significantly improves the energy efficiency of the battery. In addition, the electrode prepared by the present invention has a self-supporting property, which avoids the additional electrode preparation process and the loss of electrode surface area and battery energy density caused by the preparation process. In addition, the carbon fiber positive electrode with catalytic properties prepared by the present invention does not contain precious metal elements, and the material cost is low.
[0072] Embodiment 2:
[0073] The magnesium sheet negative electrode in Example 1 was replaced with a lithium sheet negative electrode, and the electrolyte was replaced with a 1.0 M solution of lithium bis(trifluoromethylsulfonyl)imide dissolved in triethylene glycol dimethyl ether. Others were the same as in Example 1. Figure 8 As shown, the overvoltage is only 1.1V, which has a high energy utilization rate.
[0074] Comparative Example 2:
[0075] The magnesium sheet negative electrode in Comparative Example 1 was replaced with a lithium sheet negative electrode, and the electrolyte was replaced with a 1.0M solution of lithium bis(trifluoromethylsulfonyl)imide dissolved in triethylene glycol dimethyl ether, and the rest was consistent with Example 1. The first cycle overvoltage of the battery was 2.0V, with a low energy utilization rate.
[0076] Embodiment 3:
[0077] The magnesium sheet negative electrode in Example 1 was replaced with a sodium sheet negative electrode, and the electrolyte was replaced with a 1.0M sodium bis(trifluoromethylsulfonyl)imide solution dissolved in triethylene glycol dimethyl ether, and the rest was consistent with Example 1. The results showed that the overvoltage was only 1.0V, with a high energy utilization rate.
[0078] Comparative Example 3:
[0079] The magnesium sheet negative electrode in Comparative Example 1 was replaced with a sodium sheet negative electrode, and the electrolyte was replaced with a 1.0M sodium bis(trifluoromethylsulfonyl)imide solution dissolved in triethylene glycol dimethyl ether, and the rest was consistent with Comparative Example 1. The first cycle overvoltage of the battery was 2.2V, with a low energy utilization rate.
[0080] Embodiment 4:
[0081] The oxygen atmosphere in Example 1 was replaced with air, and the rest was the same as Example 1. The results showed that the overvoltage was only 0.5 V, which had a high energy utilization rate.
[0082] Comparative Example 4:
[0083] The oxygen atmosphere in Comparative Example 1 was replaced with air, and the rest was the same as Comparative Example 1. The first cycle overvoltage of the battery was 2.3 V, which had a low energy utilization rate.
[0084] Embodiment 5:
[0085] The oxygen atmosphere in Example 2 was replaced with air, and the rest was the same as Example 2. The results showed that the overvoltage was only 1.2 V, which had a high energy utilization rate.
[0086] Comparative Example 5:
[0087] The oxygen atmosphere in Comparative Example 2 was replaced with air, and the rest was the same as Comparative Example 2. The overvoltage of the first cycle of the battery was 2.1 V, which had a lower energy utilization rate.
[0088] Embodiment 6:
[0089] The oxygen atmosphere in Example 3 was replaced with air, and the rest was the same as Example 3. The battery overvoltage was only 0.9V.
[0090] Comparative Example 6:
[0091] The oxygen atmosphere in Comparative Example 3 was replaced with air, and the rest was the same as Comparative Example 3. The overvoltage of the first cycle of the battery was 2.4V, which had a low energy utilization rate.
[0092] Embodiment 7:
[0093] The DMF in Example 1 was replaced with dimethyl sulfoxide, and the rest was the same as Example 1. The overvoltage of the first cycle of the battery was only 0.6V, which had a high energy utilization rate.
[0094] Embodiment 8:
[0095] The DMF in Example 1 was replaced with ethyl nitrate, and the rest was the same as Example 1. The overvoltage of the first cycle of the battery was only 0.65V, which had a high energy utilization rate.
[0096] Embodiment 9:
[0097] A trace amount of phosphomolybdic acid (wherein the mass of phosphomolybdic acid is 1% of the mass of PAN powder) is added to the PAN solution prepared in Example 1, and the rest is consistent with Example 1. The carbon fiber prepared by this method contains a trace amount of molybdenum carbide, but unlike the large amount of molybdenum carbide in Comparative Example 1-1 that affects the toughness and catalytic activity of the carbon fiber, a trace amount of molybdenum carbide can further regulate the defects on the surface of the carbon fiber without affecting the toughness of the carbon fiber, thereby further improving the catalytic activity of the carbon fiber. Therefore, the first-cycle overvoltage of the magnesium oxygen battery is only 0.4V, which further reduces the overvoltage, indicating that it has a higher energy utilization rate.
[0098] Embodiment 10:
[0099] A trace amount of cobalt acetate (wherein the mass of cobalt acetate is 1% of the mass of PAN powder) is added to the PAN solution prepared in Example 1, and the rest is the same as Example 1. The carbon fiber prepared by this method contains a trace amount of cobalt, which can further regulate the defects on the surface of the carbon fiber without affecting the toughness of the carbon fiber, thereby further improving the catalytic activity of the carbon fiber. Therefore, the first-cycle overvoltage of the magnesium oxygen battery is only 0.41V, which further reduces the overvoltage, indicating that it has a higher energy utilization rate.
[0100] Embodiment 11:
[0101] A trace amount of ruthenium acetate (wherein the mass of ruthenium acetate is 1% of the mass of PAN powder) is added to the PAN solution prepared in Example 1, and the rest is the same as Example 1. The carbon fiber prepared by this method contains a trace amount of ruthenium, which can further regulate the defects on the surface of the carbon fiber without affecting the toughness of the carbon fiber, thereby further improving the catalytic activity of the carbon fiber. Therefore, the first-cycle overvoltage of the magnesium oxygen battery is only 0.39V, which further reduces the overvoltage, indicating that it has a higher energy utilization rate.
[0102] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes, and can be fully applicable to various fields suitable for the present invention. For those familiar with the art, for those of ordinary skill in the art, various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principle and spirit of the present invention. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A metal-gas battery based on a flexible self-supporting carbon fiber catalyst, characterized in that: The positive electrode of the metal-gas battery adopts a flexible self-supporting carbon fiber catalyst; the flexible self-supporting carbon fiber catalyst is a carbon fiber material rich in surface defects.
2. The metal-gas battery according to claim 1, characterized in that: The flexible self-supporting carbon fiber catalyst is prepared by adopting electrostatic spinning technology.
3. The metal-gas battery according to claim 2, characterized in that: The preparation process of the electrospinning technology comprises the following steps: S1. Dissolve polyacrylonitrile PAN powder in a solvent at room temperature, stir thoroughly to obtain a PAN solution, and load the solution into a syringe pump with a capillary; S2, using a high voltage power supply to electrospin the needle tip, and using a rotating drum collector covered with a conductive thin layer to collect the spun fiber precursor; S3, pre-oxidizing the collected precursor fiber film in air at 100-400° C. for 1-3 hours; S4, keeping the pre-oxidized precursor at 750-950° C. for 1-10 hours under an argon atmosphere; S5. Cool to room temperature in the furnace, turn off the argon gas, take out the sample, and obtain a flexible self-supporting carbon fiber catalyst with high surface catalytic activity.
4. The metal-gas battery according to claim 3, characterized in that: In step S1, the solvent includes N,N-dimethylformamide DMF, dimethyl sulfoxide, sulfolane or ethyl nitrate.
5. The metal-gas battery according to claim 3, characterized in that: In step S2, the high voltage power supply provides a voltage of 10-30 kV.
6. The metal-gas battery according to claim 1, characterized in that: Precious metals, transition metals, precious metal compounds, or transition metal compounds are doped into the flexible self-supporting carbon fibers to improve the electrocatalytic properties of the flexible self-supporting carbon fibers.
7. The metal-gas battery according to claim 6, characterized in that: The noble metal and transition metal include molybdenum, cobalt, ruthenium, copper, iron, nickel or manganese.
8. The metal-gas battery according to claim 6, characterized in that: The noble metal compound includes a phosphate, acetate, oxalate, carbonate, carbide, nitride, oxide, phosphide, sulfide, chloride, iodide, bromide, or fluoride of a noble metal; The transition metal compound includes phosphates, acetates, oxalates, carbonates, carbides, nitrides, oxides, phosphides, sulfides, chlorides, iodides, bromides, or fluorides of transition metals.
9. The metal-gas battery according to claim 6, characterized in that: The doping amount of the noble metal, transition metal, noble metal compound, or transition metal compound is 0.001-10 wt % of the raw material powder for preparing the flexible self-supporting carbon fiber catalyst.
10. The metal-gas battery according to claim 1 or 6, characterized in that: The metal-gas batteries include but are not limited to Li-O2, Na-O2, K-O2, Al-O2, Zn-O2, Mg-O2, Ca-O2 and lithium-air batteries, sodium-air batteries, potassium-air batteries, aluminum-air batteries, zinc-air batteries, magnesium-air batteries, and calcium-air batteries.
Citation Information
Cited By
Metal fluoride-phosphide self-supporting electrode, preparation thereof and application of metal fluoride-phosphide self-supporting electrode in electrolyzed water
CN119663357A
Metal fluoride-phosphide self-supporting electrodes, their preparation and use in electrolysis of water
CN119663357B