Preparation process of sintered material substrate coating
By using sintered copper paste on ceramic substrates and drying and sintering in a nitrogen atmosphere, the problem of poor wetting behavior between ceramic substrates and copper foil is solved, and adhesion and compatibility are improved, suitable for large-scale production and high voltage Device usage.
Patent Information
- Application Number
- CN202410799460.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-11-01
AI Technical Summary
The existing direct copper clad technology is difficult to form good wetting behavior between the ceramic substrate and the copper foil, resulting in difficult control of the interface oxygen content and pore problems, limiting the compatibility and adhesion of the process and affecting the stability of the substrate or device.
The sintered copper paste is coated on the ceramic substrate by preset attachment method, and dried and sintered in a nitrogen atmosphere. The connection between the substrate and the coating is enhanced by adhesive. It is suitable for a variety of ceramic substrates, including AlN and Al2O3 ceramics. The substrate, the sintering temperature and time are adjustable.
It improves the adhesion and connectivity between the ceramic substrate and the cladding, enhances the compatibility and flexibility of the process, is suitable for large-scale production, is suitable for high-power and high-voltage devices, and reduces costs.
Smart Images

Figure CN118890792A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging, and in particular relates to a preparation process of a sintered material substrate coating. Background Art
[0002] In the field of semiconductor device manufacturing, substrate coating is one of the key preparation steps. Its purpose is to improve the performance of the substrate and enhance its stability and reliability. As the connecting element between electronic components and substrates, substrate coating materials need to have excellent conductivity and adhesion, as well as certain corrosion resistance. Copper, due to its excellent electrical and thermal conductivity, has become one of the mainstream materials used for substrate coating in the market.
[0003] Direct Bonded Copper (DBC) is a common substrate metallization method in the industry. This technology allows the copper foil coated on the substrate surface to wet with the ceramic substrate surface under high temperature conditions, forming a connection with a certain strength. However, not all ceramic substrates can form good wetting behavior with copper foil (such as AlN ceramic substrates), which limits the compatibility of this process to a certain extent. At the same time, this process may lead to problems such as difficulty in controlling the oxygen content between the interface and the presence of pores that cannot be completely eliminated at the interface between the coating and the substrate, which affects the adhesion of the coating and causes failure of the substrate or device. Summary of the invention
[0004] An object of the present invention is to provide a process for preparing a sintered material substrate coating, which can solve the problem of narrow application range of existing processes.
[0005] According to a first aspect of the present invention, there is provided a process for preparing a sintered material substrate coating, comprising:
[0006] Covering the sintered copper paste on the ceramic substrate by a preset attachment method to form a sintered copper layer on the surface of the ceramic substrate;
[0007] Drying the ceramic substrate covered with the sintered copper layer in a nitrogen atmosphere at a first preset temperature for a first preset time;
[0008] The dried ceramic substrate is sintered in a nitrogen atmosphere at a second preset temperature for a second preset time.
[0009] Optionally, the preset attachment method includes: screen printing, inkjet printing, and laser direct writing.
[0010] Optionally, the sintered copper paste includes metal powder, an organic carrier, and a binder.
[0011] Optionally, the metal powder includes at least one of the following: nano copper particles and micro copper particles.
[0012] Optionally, the organic vehicle includes an organic solvent and a thickener.
[0013] Optionally, the binder includes at least one of the following: glass powder and metal oxide.
[0014] Optionally, the first preset temperature and the first preset time are determined according to the volatilization temperature and capacity of the organic carrier.
[0015] Optionally, the thickness of the sintered copper layer formed on the surface of the ceramic substrate is 10-300 μm.
[0016] Optionally, the ceramic substrate includes an AlN ceramic substrate or an Al2O3 ceramic substrate.
[0017] Optionally, the second preset temperature is 500-1000° C., and the second preset time is 10-60 min.
[0018] The beneficial effects of the present invention are as follows: the sintered copper paste provided in the present invention forms a good adhesion effect with the substrate interface through the function of the binder, thereby enhancing the connection between the substrate interface and the coating. At the same time, the sintered copper paste provided in the present invention has good wetting behavior with various types of ceramic substrates, thereby improving the compatibility and flexibility of process applications. The preparation process involved in the present invention is simple, low-cost, has excellent economic benefits, and is suitable for large-scale production. The thickness of the sintered copper layer described in the present invention can be adjusted according to the actual application situation, and can be applied to the use of high-power and high-voltage devices, thereby enhancing the wide application of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a flowchart of a process for preparing a sintered material substrate coating in one embodiment of the present invention.
[0020] Figure 2 It is a flow chart of a process for preparing a sintered material substrate coating in another embodiment of the present invention.
[0021] Figure 3 The present invention is a flowchart of a process for preparing a sintered material substrate coating in another embodiment of the present invention. DETAILED DESCRIPTION
[0022] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0023] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0024] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0025] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0026] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0027] In the specification and claims of the present invention, if the term "first" or "second" is involved, it may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more. In addition, "and / or" in the specification and claims means at least one of the connected objects, and the character " / " generally means that the related objects are in an "or" relationship.
[0028] Direct copper coating technology is to use copper oxygen-containing eutectic liquid to directly coat copper on the ceramic substrate. Its basic principle is to introduce an appropriate amount of oxygen between copper and ceramic before or during the coating process. Within the appropriate temperature range, copper and oxygen form CuO (copper oxide) eutectic liquid. Direct copper coating technology uses this eutectic liquid to react chemically with the ceramic substrate on the one hand, and to wet the copper foil on the other hand to achieve the combination of the ceramic substrate and the copper plate. However, direct copper coating technology is prone to produce micropores between the ceramic substrate and the copper layer, which in turn causes the substrate to fail.
[0029] like Figure 1 As shown, this embodiment introduces a preparation process of a sintered material substrate coating, including steps 1100-1300.
[0030] Step 1100: coating a sintered copper paste on a ceramic substrate by a preset attachment method to form a sintered copper layer on the surface of the ceramic substrate.
[0031] Ceramic substrate refers to a special process board in which copper foil is directly bonded to the surface of a ceramic substrate at high temperature. Ceramic substrate has excellent insulation performance, high thermal conductivity, excellent soft solderability and high adhesion strength, and can be etched with various patterns like PCB (Printed Circuit Board) board, and has a large current carrying capacity. The ceramic substrate in this embodiment can be an AlN (aluminum nitride) ceramic substrate or an Al2O3 (aluminum oxide) ceramic substrate.
[0032] Ceramic substrates can be used in many different fields. For example, ceramics can basically be used as carriers of integrated circuits, and circuit functions can be realized by manufacturing microcircuits and components on their surface. Ceramic substrates can also be used to manufacture various sensors, such as temperature sensors, humidity sensors, and gas sensors. Ceramic substrates can also be made into various micro components, such as power dividers, couplers, and isolators. The shape and thickness of the sintered copper layer can be adjusted according to actual needs, and sintered layers of different shapes and thicknesses can be formed according to different usage scenarios of the ceramic substrate. For example, the thickness of the sintered copper layer can be 10-300μm.
[0033] The preset attachment method can be any one of screen printing, inkjet printing, and laser direct writing. Screen printing refers to using a screen as a base and making a screen printing plate with graphics through a photosensitive platemaking method. Laser direct writing technology uses a laser beam with variable intensity to perform variable metering exposure on the material on the surface of the substrate to form a corresponding pattern. When using the inkjet printing method, the sintered copper paste is sprayed onto the ceramic substrate through a nozzle to form a sintered layer.
[0034] In one example, the ceramic substrate is an Al2O3 ceramic substrate, and the preset attachment method is screen printing. Before the sintered copper paste is coated on the Al2O3 ceramic substrate, the Al2O3 ceramic substrate is first cleaned and dried. Specifically, the Al2O3 ceramic substrate is immersed in an acetone solution, ultrasonically cleaned for 20-30 minutes, and dried in an air atmosphere. Then, the sintered copper paste is coated on the cleaned and dried Al2O3 ceramic substrate by screen printing, and a sintered copper layer with a preset pattern and a certain thickness is formed on the surface of the substrate.
[0035] In another example, the ceramic substrate is an AlN ceramic substrate, and the preset attachment method is screen printing. Specifically, a nylon screen with a mesh size of 280, a wire diameter of 28 μm, and a mask thickness of 30 μm can be used to print the sintered copper paste on the AlN ceramic substrate, and the slurry is left to level for 10 minutes to form a sintered copper layer of a certain thickness on the surface of the substrate.
[0036] Step 1200: Drying the ceramic substrate covered with the sintered copper layer in a nitrogen atmosphere at a first preset temperature for a first preset time.
[0037] After the sintered copper layer is formed on the surface of the ceramic substrate, the ceramic substrate is dried. The first preset temperature is the temperature when the ceramic substrate is dried, and the first preset time is the time for drying the ceramic substrate. The first preset temperature and the first preset time can be determined according to the specific composition of the sintered copper paste. In this embodiment, the ceramic substrate is dried in a nitrogen atmosphere.
[0038] Step 1300: sintering the dried ceramic substrate in a nitrogen atmosphere at a second preset temperature for a second preset time.
[0039] After drying the ceramic substrate, continue to sinter the ceramic substrate in a nitrogen atmosphere. Through the sintering process, a connection with a certain strength is formed between the ceramic substrate and the sintered copper layer, and the preparation of the copper coating of the ceramic substrate is completed. The second preset temperature and the second preset time can be determined according to the type of the ceramic substrate and the composition of the sintered copper paste. For example, the second preset temperature is 500-1000°C, and the second preset time is 10-60min.
[0040] In this embodiment, the sintered copper paste includes metal powder, organic carrier, and binder. The metal powder includes at least one of the following: nano copper particles and micro copper particles. The organic carrier includes an organic solvent and a thickener. The binder includes at least one of the following: glass powder and metal oxide.
[0041] The metal powder may be nano copper particles. The metal powder may also be micron copper particles. The metal powder may also be a mixture of nano copper particles and micron copper particles. Nano copper particles refer to copper particles with a size of nanometers, and micron copper particles refer to copper particles with a size of micrometers. The corresponding metal powder may be selected according to the type of ceramic substrate. For example, when the ceramic substrate is an Al2O3 ceramic substrate, the metal powder in the sintered copper paste may be a mixture of micro-nano copper particles. When the ceramic substrate is an AlN ceramic substrate, the metal powder in the sintered copper paste may be nano copper particles.
[0042] The organic carrier includes an organic solvent and a thickener, such as a pine alcohol-polyacrylate resin system and a pine alcohol-ethyl cellulose system. The corresponding organic carrier can be selected according to the type of the ceramic substrate. For example, when the ceramic substrate is an Al2O3 ceramic substrate, the organic carrier can be a pine alcohol-polycarbonate acrylate system. When the ceramic substrate is an AlN ceramic substrate, the organic carrier can be a pine alcohol-ethyl cellulose system.
[0043] The binder may be glass powder. The binder may also be metal oxide. The binder may also be a mixture of glass powder and metal oxide. The corresponding binder may be selected according to the type of the ceramic substrate. For example, when the ceramic substrate is an Al2O3 ceramic substrate, the binder may be SnO2-P2O5- and TeO2-V2O5-based glass powder. When the ceramic substrate is an AlN ceramic substrate, the binder may be borate glass powder.
[0044] The sintered copper paste provided in the present invention forms a good adhesion effect with the substrate interface through the function of the binder, thereby enhancing the connection between the substrate interface and the coating. At the same time, the sintered copper paste provided in the present invention has good wetting behavior with various types of ceramic substrates, thereby improving the compatibility and flexibility of process applications.
[0045] In this embodiment, the first preset temperature and the first preset time are determined according to the volatilization temperature and capacity of the organic carrier.
[0046] The first preset temperature is the temperature at which the ceramic substrate is dried, and the first preset time is the time for drying the ceramic substrate. Since different organic carriers have different volatilization temperatures and capacities, in order to avoid affecting the performance of the ceramic substrate, different drying temperatures and drying times are required when drying the ceramic substrate according to different organic carriers.
[0047] For example, when the organic carrier is a terpineol-polycarbonate acrylate system, the first preset temperature may be 200° C. and the first preset time may be 60 minutes. When the organic carrier is a terpineol-ethyl cellulose system, the first preset temperature may be 150° C. and the first preset time may be 20 minutes.
[0048] like Figure 2 As shown, this embodiment introduces a preparation process of a sintered material substrate coating, including steps 2100-2500.
[0049] Step 2100: Immerse the Al2O3 ceramic substrate in an acetone solution, perform ultrasonic cleaning for 20 to 30 minutes, and complete drying in an air atmosphere.
[0050] Step 2200: The sintered copper paste is coated on the cleaned and dried Al2O3 ceramic substrate by screen printing, so as to form a sintered copper layer with a preset pattern and a certain thickness on the surface of the substrate.
[0051] Step 2300: Place the Al2O3 ceramic substrate covered with the sintered copper layer in a nitrogen atmosphere and dry it at 200°C for 40 minutes.
[0052] Step 2400: placing the dried Al2O3 ceramic substrate in a nitrogen atmosphere and sintering it at 600°C for 60 minutes.
[0053] Step 2500: Sintering is completed and the temperature is lowered to room temperature, completing the preparation of the metal copper coating on the surface of the Al2O3 ceramic substrate.
[0054] In this embodiment, the metal powder in the sintered copper paste is a mixture of micro-nano copper particles, the organic carrier is a pine alcohol-polycarbonate acrylate system, and the binder is SnO2-P2O5- and TeO2-V2O5-based glass powder. The printed sintered layer has a thickness of 50 μm.
[0055] like Figure 3 As shown, this embodiment introduces a preparation process of a sintered material substrate coating, including steps 3100-3400.
[0056] Step 3100: Use a nylon screen with a mesh size of 280, a wire diameter of 28 μm, and a mask thickness of 30 μm to print the sintered copper paste on the AlN ceramic substrate, and let it stand for 10 minutes to wait for the slurry to level and form a sintered copper layer of a certain thickness on the substrate surface.
[0057] Step 3200: Place the AlN ceramic substrate covered with the sintered copper layer in a nitrogen atmosphere and dry it at 150° C. for 20 minutes.
[0058] Step 3300: Place the AlN ceramic substrate after drying in a nitrogen atmosphere and keep it at 850° C. for 30 minutes.
[0059] Step 3400: Sintering is completed and the temperature is lowered to room temperature, completing the preparation of the metal copper coating on the surface of the AlN ceramic substrate.
[0060] In this embodiment, the metal powder in the sintered copper paste is nano copper particles, the organic carrier is a pine alcohol-ethyl cellulose system, and the binder is a borate glass powder.
[0061] The present invention has the following beneficial effects: (1) The sintered copper paste provided in the present invention forms a good adhesion effect with the substrate interface through the function of the binder, thereby enhancing the connection between the substrate interface and the coating. At the same time, the sintered copper paste provided in the present invention has good wetting behavior with various types of ceramic substrates, thereby improving the compatibility and flexibility of process applications. (2) The preparation process involved in the present invention is simple, low-cost, has excellent economic benefits, and is suitable for large-scale production. (3) The thickness of the sintered copper layer described in the present invention can be adjusted according to the actual application situation, and can be suitable for the use of high-power and high-voltage devices, thereby enhancing the wide application of the process.
[0062] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. A process for preparing a sintered material substrate coating, It is characterized in that include: Covering the sintered copper paste on the ceramic substrate by a preset attachment method to form a sintered copper layer on the surface of the ceramic substrate; Drying the ceramic substrate covered with the sintered copper layer in a nitrogen atmosphere at a first preset temperature for a first preset time; The dried ceramic substrate is sintered in a nitrogen atmosphere at a second preset temperature for a second preset time.
2. The process for preparing the sintered material substrate coating according to claim 1, It is characterized in that The preset attachment methods include: screen printing, inkjet printing, and laser direct writing.
3. The process for preparing the sintered material substrate coating according to claim 1, It is characterized in that The sintered copper paste comprises metal powder, an organic carrier and a binder.
4. The process for preparing the sintered material substrate coating according to claim 3, It is characterized in that The metal powder includes at least one of the following: nano copper particles and micro copper particles.
5. The process for preparing the sintered material substrate coating according to claim 3, It is characterized in that The organic vehicle includes an organic solvent and a thickener.
6. The process for preparing the sintered material substrate coating according to claim 3, It is characterized in that The binder includes at least one of the following: glass powder and metal oxide.
7. The process for preparing the sintered material substrate coating according to claim 3, It is characterized in that The first preset temperature and the first preset time are determined according to the volatilization temperature and capacity of the organic carrier.
8. The process for preparing a sintered material substrate coating according to claim 1, It is characterized in that The thickness of the sintered copper layer formed on the surface of the ceramic substrate is 10-300 μm.
9. The process for preparing a sintered material substrate coating according to claim 1, It is characterized in that The ceramic substrate comprises an AlN ceramic substrate, an Al 2 O 3 Ceramic substrate.
10. The process for preparing a sintered material substrate coating according to claim 1, It is characterized in that The second preset temperature is 500-1000° C., and the second preset time is 10-60 min.