Preparation method of PTFE-based high-frequency copper-clad plate

The thermal expansion of PTFE-based copper clad plate was solved by grafting reaction with cyclohexane and vinylsilane coupling agent under anhydrous and oxygen-free atmosphere with PTFE-based copper clad plates. The problem of high coefficients achieves PTFE-based high-frequency copper clad plate with low dielectric loss and low thermal expansion coefficient, meeting the needs of high-frequency circuits.

CN118890793APending Publication Date: 2024-11-01WUZHEN LABORATORY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410899611.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The thermal expansion coefficient of PTFE-based copper clad plate is relatively high, which affects the alignment between the printed circuit layers, increases the risk of cracking of PCB through-hole plating and cracking of wires and pads, and has high dielectric loss, making it difficult to meet the needs of high-frequency circuits.

Method used

By grafting reaction with cyclohexane and vinylsilane coupling agent under anhydrous and oxygen-free atmosphere, PTFE powder grafted with silane coupling agent is formed and PTFE powder is formed with inorganic filler. The dehydration and condensation reaction is carried out in the solvent to enhance the compatibility and interface force of PTFE with the inorganic filler, and reduce the thermal expansion coefficient and dielectric loss.

Benefits of technology

It effectively reduces the thermal expansion coefficient of PTFE-based copper clad plate, and the dielectric loss is less than 0.001, meeting the application needs of high-frequency circuits, and improving the ability of inorganic fillers to suppress the thermal motion of PTFE macromolecular chains.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004930121240000081
    Figure BDA0004930121240000081
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of high-frequency copper-clad plates, and provides a preparation method of a PTFE-based high-frequency copper-clad plate in order to solve the problem that the thermal expansion coefficient of a PTFE-based copper-clad plate in the prior art is too high, and the preparation method comprises the following steps: adding PTFE powder activated by tert-butyllithium, cyclohexane and a vinyl silane coupling agent in an anhydrous and oxygen-free atmosphere; after heating reaction, washing and drying, adding into an ethanol water solution, then adding an inorganic filler, and after heating reaction, filtering, washing and drying to obtain PTFE-inorganic filler composite powder; and dispersing the PTFE-inorganic filler composite powder in a PTFE emulsion to obtain slurry, coating a copper foil with the slurry, removing the solvent, coating the other medium surface with the copper foil, and pressing at high temperature and high pressure to obtain the PTFE-based copper-clad plate. According to the preparation method, the interfacial acting force of PTFE and the inorganic filler is improved, the thermal expansion coefficient of the PTFE-based copper-clad plate is reduced, and the high-frequency dielectric property is considered.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high-frequency copper-clad laminate preparation, and in particular to a method for preparing a PTFE-based high-frequency copper-clad laminate. Background Art

[0002] In recent years, with the rapid development of satellite communications, autonomous driving technology, and 5.5G communication technology, electronic components have been moving towards high frequency. The dielectric loss of polytetrafluoroethylene (PTFE) can reach the ten thousand level. At the same time, it has extremely low water absorption, excellent heat resistance and chemical resistance, making it an ideal high-frequency copper clad laminate substrate.

[0003] However, there is no active group in the PTFE molecular chain, which is a non-polar material. The interfacial force with the inorganic filler is very weak, resulting in the inorganic filler being unable to effectively inhibit the thermal motion of the PTFE macromolecules, causing the thermal expansion coefficient of the PTFE-based copper-clad laminate to be high, affecting the interlayer alignment of the printed circuit (PCB), and increasing the risks of cracking of the PCB through-hole plating, cracking of the wire and the pad. Chinese patent CN104647868A discloses a method for preparing a polytetrafluoroethylene copper-clad laminate, wherein a PTFE emulsion is mixed and dispersed with an inorganic filler of different dielectric constants, and after impregnation, gluing, heating and drying, the copper-clad laminate is hot-pressed for 3 to 6 hours at a temperature of 450°C and a pressure of 15 to 20 MPa under a vacuum condition of 90 to 100 KPa. The dielectric constant of the copper-clad laminate prepared under this technology is controllable and the peeling strength is high, but due to the poor compatibility of PTFE with the inorganic filler, the interfacial force is weak, and the thermal expansion coefficient of the copper-clad laminate is too high. Chinese patent CN108189520A discloses a method for preparing a modified polytetrafluoroethylene copper-clad laminate, wherein one or more of AA, MAH and GMA are used as grafting monomers to modify PTFE powder treated with sodium naphthalene, the modified PTFE and an inorganic filler modified with a silane coupling agent are dispersed into a slurry, which is then coated on a copper foil and pressed into a copper-clad laminate. This technology improves the compatibility of PTFE and the inorganic filler, greatly improves the dimensional stability of the copper-clad laminate, stabilizes the dielectric properties, and has low dielectric loss, but is still insufficient in terms of the thermal expansion coefficient. Summary of the invention

[0004] In order to overcome the problem of high thermal expansion coefficient of PTFE-based copper-clad laminates in the prior art, the present invention provides a preparation method of PTFE-based high-frequency copper-clad laminates. The preparation method improves the interfacial force between PTFE and inorganic fillers, reduces the thermal expansion coefficient of the PTFE-based copper-clad laminates, and takes into account high-frequency dielectric properties.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing a PTFE-based high-frequency copper-clad laminate comprises the following steps: (1) adding PTFE powder activated by tert-butyl lithium, cyclohexane and vinyl silane coupling agent in an anhydrous and oxygen-free atmosphere, heating for reaction, washing and drying to obtain PTFE powder grafted with silane coupling agent; (2) adding PTFE powder grafted with a silane coupling agent and an inorganic filler to an ethanol aqueous solution in sequence, heating for reaction, filtering, washing, and drying to obtain a PTFE-inorganic filler composite powder; (3) Dispersing PTFE-inorganic filler composite powder in PTFE emulsion to obtain slurry, coating the slurry on copper foil, removing the solvent, covering the other dielectric surface with copper foil, and pressing under high temperature and high pressure to obtain a PTFE-based copper clad laminate.

[0006] The present invention utilizes carbon free radicals in the chain of PTFE macromolecules activated by tert-butyl lithium to initiate a grafting reaction of double bonds of a vinyl silane coupling agent, thereby realizing the functional modification of PTFE; the obtained PTFE powder grafted with a silane coupling agent is stirred and mixed with an inorganic filler in a solvent, and the alkoxy group is hydrolyzed to form a hydroxyl group, which undergoes a dehydration condensation reaction with the hydroxyl group on the surface of the inorganic filler, thereby realizing the chemical bond connection between PTFE and the inorganic filler; the prepared PTFE-inorganic filler composite powder is dispersed in a PTFE emulsion, thereby greatly enhancing the compatibility and interfacial force of PTFE and the inorganic filler, improving the ability of the inorganic filler to inhibit the thermal motion of the PTFE macromolecular chain, and solving the problem of a high thermal expansion coefficient of a PTFE-based copper-clad laminate, wherein the thermal expansion coefficients of the pressed copper-clad laminate in the X-axis, the Y-axis and the Z-axis are all lower than 20 ppm / °C; and at the same time, the dielectric loss is lower than 0.001, thereby being able to meet the application requirements of high-frequency circuits.

[0007] Preferably, the mass ratio of the PTFE powder activated with tert-butyl lithium, cyclohexane and vinyl silane coupling agent in (1) is (1-2):10:(0.2-0.4).

[0008] Preferably, the vinyl silane coupling agent in (1) is vinyl trimethoxy silane and / or dimethoxy methyl vinyl silane.

[0009] Preferably, the cyclohexane in (1) is obtained by dehydrating with calcium hydride and then distilling.

[0010] Preferably, the (1) is to add PTFE powder activated by tert-butyl lithium, cyclohexane and vinyl silane coupling agent in an anhydrous and oxygen-free atmosphere, stir and react at 71-75° C. for 9-15 hours, and then wash and dry to obtain PTFE powder grafted with silane coupling agent.

[0011] Preferably, in said (1), an inert gas is used to create an anhydrous and oxygen-free atmosphere.

[0012] Preferably, the mass ratio of the PTFE powder grafted with the silane coupling agent to the inorganic filler in (2) is 1:(2-4).

[0013] Preferably, the inorganic filler in (2) is one or more of silicon dioxide, silicon nitride, aluminum oxide, titanium dioxide and hollow glass microspheres.

[0014] Preferably, the (2) is to add PTFE powder grafted with a silane coupling agent to a 90-95wt% ethanol aqueous solution, ultrasonically mix for 11-15 minutes, then add an inorganic filler, stir at high speed at 71-75°C for 12-15 hours, and obtain a PTFE-inorganic filler composite powder after filtering, washing and drying.

[0015] Preferably, the mass ratio of the PTFE-inorganic filler composite powder to the PTFE emulsion in (3) is 1:(0.5-1); and the solid content of the PTFE emulsion is 60%.

[0016] Preferably, the coating thickness of the slurry in (3) is 100 to 1500 μm.

[0017] Therefore, the present invention has the following beneficial effects: the ability of inorganic fillers to inhibit the thermal motion of PTFE macromolecular chains is improved, the thermal expansion coefficient of PTFE-based copper-clad laminates is reduced, the dielectric loss is low, and the PTFE-based high-frequency copper-clad laminates can meet the application requirements of high-frequency circuits. DETAILED DESCRIPTION

[0018] The present invention is further described below in conjunction with specific implementation methods.

[0019] The experimental materials used in the following specific implementation method are as follows: Vinyltrimethoxysilane, dimethoxymethylvinylsilane, and γ-aminopropyltriethoxysilane were purchased from Beijing Inokai Technology Co., Ltd.; Polytetrafluoroethylene (PTFE) emulsion was purchased from Chemours Fluoroplastics, brand DISP-30, solid content 60%; Silicon dioxide was purchased from Lianrui New Materials Co., Ltd. with an average particle size of 10 μm; Titanium dioxide was purchased from Suzhou Jinyi New Materials Technology Co., Ltd. with a particle size of 7.5 μm; Silicon nitride was purchased from Foshan Qingli New Materials Co., Ltd. with a particle size of 5 μm; PTFE powder activated by tert-butyl lithium: After the reaction bottle was flame-baked and nitrogen-exhausted three times, a mixed solution of tert-butyl lithium and triethylamine in a molar ratio of 1:1 was added in an anhydrous, oxygen-free and nitrogen atmosphere, and 0.1 g of PTFE powder (Zonyl MP1100, average particle size 4 μm) was added for every 5 mmol of tert-butyl lithium. After reacting at 0°C for 1 hour, the mixture was washed with THF and hexane at 0°C to obtain PTFE powder activated by tert-butyl lithium, which was stored in a glass bottle in an anhydrous, oxygen-free and nitrogen atmosphere.

[0020] Hereinafter, unless otherwise specified, "part" means part by weight, and "%" means "% by weight".

[0021] Example 1 A PTFE-based high-frequency copper-clad laminate is prepared by the following steps: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, ultrasonically mixing for 12 minutes, and then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0022] Example 2 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that the grafting rate of the PTFE powder obtained in step (1) is different; The details are as follows: (1) After the reaction bottle was flame-baked and nitrogen-evacuated three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.2 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and stirred for reaction at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 6.5% calculated by a weighing method. (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, ultrasonically mixing for 12 minutes, and then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0023] Example 3 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that the grafting rate of the PTFE powder obtained in step (1) is different; The details are as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.4 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 9% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, ultrasonically mixing for 12 minutes, and then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0024] Example 4 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that different inorganic fillers are added in step (2); specifically, as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, and ultrasonically mixing for 12 minutes, then adding 2.5 parts of silicon dioxide and 0.5 parts of titanium dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0025] Example 5 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that different inorganic fillers are added in step (2); specifically, as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, and ultrasonically mixing for 12 minutes, then adding 2 parts of silicon dioxide and 1 part of silicon nitride, and stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0026] Example 6 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that the grafting rates of the silane coupling agent and the obtained PTFE powder in step (1) are different; The details are as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of dimethoxymethylvinylsilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8.5% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, ultrasonically mixing for 12 minutes, and then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0027] Example 7 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that different inorganic fillers are added in step (2); specifically, as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, and ultrasonically mixing for 12 minutes, and then adding 2 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0028] Example 8 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that the inorganic filler added in step (2) is different, and the PTFE emulsion in step (3) is different; The details are as follows: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours. The mixture was washed with cyclohexane and ethanol and dried to obtain PTFE powder grafted with a silane coupling agent. The grafting rate of the PTFE powder was 8% calculated by a weighing method; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder grafted with a silane coupling agent, ultrasonically mixing for 12 minutes, then adding 4 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 1 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper clad laminate.

[0029] Comparative Example 1 A PTFE-based high-frequency copper-clad laminate, the preparation steps of which are different from those of Example 1 in that the PTFE powder in step (1) is not grafted with a vinyl silane coupling agent; The details are as follows: (1) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder activated by tert-butyl lithium, and ultrasonically dispersing for 12 minutes, then adding 2 parts of silicon dioxide and 1 part of silicon nitride, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (2) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0030] Comparative Example 2 A PTFE-based high-frequency copper-clad laminate is prepared by the following steps: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder and 0.3 parts of vinyltrimethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours, and then washed with cyclohexane and ethanol and dried to obtain PTFE powder treated with a silane coupling agent; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder treated with a silane coupling agent, ultrasonically mixing for 12 minutes, then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0031] Comparative Example 3 A PTFE-based high-frequency copper-clad laminate is prepared by the following steps: (1) After the reaction bottle was flame-baked and nitrogen-exhausted three times, 10 parts of cyclohexane treated by calcium hydride dehydration and rectification, 1.5 parts of PTFE powder activated by tert-butyl lithium and 0.3 parts of γ-aminopropyltriethoxysilane were added in an anhydrous, oxygen-free and nitrogen atmosphere, and the mixture was stirred and reacted at 72° C. for 12 hours, and then washed with cyclohexane and ethanol and dried to obtain PTFE powder treated with a silane coupling agent; (2) adding 50 parts of 95% ethanol aqueous solution into a high-speed stirring reactor, adding 1 part of PTFE powder treated with a silane coupling agent, ultrasonically mixing for 12 minutes, then adding 3 parts of silicon dioxide, stirring at high speed for 13 hours at 72° C., filtering, washing with ethanol, and drying to obtain a PTFE-inorganic filler composite powder; (3) Disperse 1 part of PTFE-inorganic filler composite powder in 0.5 part of PTFE emulsion, stir at high speed for 8 hours, coat the obtained slurry on copper foil, control the coating thickness to 180 μm, remove the solvent through heat treatment, cover the other medium surface with copper foil, and press at 370°C and 7 MPa for 5 hours to obtain a PTFE-based copper-clad laminate.

[0032] According to the IPC-TM650 testing method, the dielectric constant (D k ), dielectric loss (D f ) and thermal expansion coefficient were tested, and the test results are shown in Table 1: Table 1. Dielectric properties and thermal expansion coefficients of Examples 1 to 8 and Comparative Examples 1 to 3 It can be seen from Table 1 that the dielectric loss of the PTFE-based high-frequency copper-clad laminates prepared by the method of the present invention in Examples 1 to 8 is lower than 0.001, and the thermal expansion coefficients of the X-axis, Y-axis and Z-axis are all lower than 20ppm / °C. It can be seen that the method of the present invention can greatly enhance the compatibility and interfacial force between PTFE and inorganic fillers, enhance the ability of inorganic fillers to inhibit the thermal motion of PTFE macromolecular chains, solve the problem of high thermal expansion coefficient of PTFE-based copper-clad laminates in the prior art, and have extremely low dielectric loss, which can meet the use requirements of high-frequency circuits.

[0033] The types and contents of inorganic fillers added in Examples 1, 4-5 and 7-8 are different. From the data of dielectric properties and thermal expansion coefficients, it can be seen that the present invention can improve the ability of various types of inorganic fillers to inhibit the thermal motion of PTFE macromolecular chains.

[0034] In Comparative Example 1, the PTFE powder activated by tert-butyl lithium was not grafted with a vinyl silane coupling agent, and the PTFE could not be chemically bonded with the inorganic filler, and the thermal expansion coefficient of the pressed PTFE-based copper-clad laminate was significantly higher. In Comparative Example 2, the PTFE powder was directly mixed with vinyl trimethoxy silane without activation treatment, resulting in the inability of vinyl trimethoxy silane to graft with the PTFE powder; γ-aminopropyl triethoxy silane did not contain double bonds, and in Comparative Example 3, the activated PTFE powder was treated with γ-aminopropyl triethoxy silane, and the two could not undergo a free radical grafting reaction, and the thermal expansion coefficient of the pressed PTFE-based copper-clad laminate was significantly higher.

Claims

1. A method for preparing a PTFE-based high-frequency copper-clad laminate, characterized in that: The steps include: (1) In an anhydrous and oxygen-free atmosphere, PTFE powder activated by tert-butyl lithium, cyclohexane and vinyl silane coupling agent are added, and after heating reaction, washing and drying are performed to obtain PTFE powder grafted with silane coupling agent; (2) adding PTFE powder grafted with a silane coupling agent and an inorganic filler to an ethanol aqueous solution in sequence, heating the mixture for reaction, filtering, washing, and drying the mixture to obtain a PTFE-inorganic filler composite powder; (3) Dispersing PTFE-inorganic filler composite powder in PTFE emulsion to obtain slurry, coating the slurry on copper foil, removing the solvent, covering the other dielectric surface with copper foil, and pressing under high temperature and high pressure to obtain a PTFE-based copper clad laminate.

2. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, wherein: The mass ratio of the PTFE powder activated with tert-butyl lithium, cyclohexane and vinyl silane coupling agent in (1) is (1-2):10:(0.2-0.4).

3. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, wherein: The vinyl silane coupling agent in (1) is vinyl trimethoxy silane and / or dimethoxy methyl vinyl silane.

4. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, wherein: The cyclohexane in (1) is obtained by distillation after dehydration with calcium hydride.

5. A method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, 2, 3 or 4, characterized in that: The method (1) is to add PTFE powder activated by tert-butyl lithium, cyclohexane and vinyl silane coupling agent in an anhydrous and oxygen-free atmosphere, stir and react at 71-75° C. for 9-15 hours, and then wash and dry to obtain PTFE powder grafted with silane coupling agent.

6. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, wherein: The mass ratio of the PTFE powder grafted with the silane coupling agent to the inorganic filler in (2) is 1:(2-4).

7. A method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1 or 6, characterized in that: The inorganic filler in (2) is one or more of silicon dioxide, silicon nitride, aluminum oxide, titanium dioxide and hollow glass microspheres.

8. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 7, characterized in that: The (2) is to add PTFE powder grafted with a silane coupling agent to a 90-95wt% ethanol aqueous solution, ultrasonically mix for 11-15 minutes, then add an inorganic filler, stir at high speed at 71-75°C for 12-15 hours, and obtain a PTFE-inorganic filler composite powder after filtering, washing and drying.

9. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, wherein: The mass ratio of the PTFE-inorganic filler composite powder to the PTFE emulsion in (3) is 1: (0.5-1); the solid content of the PTFE emulsion is 60%.

10. The method for preparing a PTFE-based high-frequency copper-clad laminate according to claim 1, characterized in that: The coating thickness of the slurry in (3) is 100 to 1500 μm.

Citation Information

Cited By

  • A fluorine-containing resin composition, a fluorine-containing resin die sheet, a metal-clad plate, and a printed circuit board

    CN122686040A