Preparation method of air gap structure of resistive random access memory array

By optimizing the etching and deposition steps in the CMOS process, the periodic groove structure is designed to form an air gap, which solves the problem of capacitive coupling effect in CMOS hybrid integrated circuits, improves memory performance and simplifies the process flow.

CN118890904AActive Publication Date: 2024-11-01PEKING UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411012267.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-01
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In CMOS hybrid integrated circuits, it is difficult for traditional methods to effectively introduce air gap structures in the back-end process, resulting in a significant increase in capacitive coupling effect, affecting the performance and stability of the memory, and complex process flows increase cost and stability problems.

Method used

By optimizing the etching and deposition steps, the periodic groove structure is designed to form an air gap in the dielectric layer, and combined with specific materials and process technologies such as PVD, ALD, CVD, the aspect ratio and edge characteristics of the groove are accurately controlled to form a high depth The aspect ratio groove structure is used to reduce capacitive coupling.

Benefits of technology

It effectively reduces signal delay problems, improves the performance of integrated circuits, provides technical support for the commercialization of new high-density memory, simplifies process flow and improves stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890904A_ABST
    Figure CN118890904A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an air gap structure of a resistive random access memory array, and belongs to the technical field of semiconductors and CMOS hybrid integrated circuits. In the preparation process of the rear-end resistive random access memory array, a periodic air gap structure is formed between adjacent resistive random access memory units by utilizing the design of a groove structure with a high aspect ratio. According to the invention, the problem of signal delay caused by capacitive coupling can be effectively relieved, and the method has important significance for improving the performance of a novel memory technology in the aspects of large-scale integration and production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of semiconductor and CMOS hybrid integrated circuits, and in particular relates to a method for preparing an air gap structure between resistive memory cells. Background Art

[0002] With the advent of the intelligent era, Moore's Law has gradually become invalid; the limitations of the traditional von Neumann architecture in the separation of data storage and processing have promoted the research and attention of new non-volatile storage technologies. In order to achieve compatibility with the current CMOS platform, emerging storage technologies such as resistive RAM (RRAM), magnetoresistive RAM (MRAM) and phase-change resistive RAM (PCRAM) usually adopt a back-end integration method to ensure the coordination with the traditional metal interconnect layer.

[0003] With the development of VLSI technology, the continuous reduction of feature size has led to a significant increase in the capacitive coupling effect between interconnects. Faced with this challenge, although traditional methods have used low dielectric constant materials such as silicon dioxide (SiO2) to reduce the parasitic capacitance between interconnects, the effectiveness of these methods has been limited. Therefore, the introduction of air gap technology with extremely low dielectric constant (about 1) is considered to be an effective strategy to reduce RC delay and improve performance. However, how to integrate air gap technology into existing production processes while ensuring process stability and reliability remains a challenge.

[0004] In the development of 3D flash memory technology, the introduction of air gaps through self-alignment, double patterning and wet etching techniques, and by sacrificing specific layer materials, have demonstrated potential optimization strategies for back-end wiring issues. Similarly, the introduction of air gaps using XeF2 dry etching has also been explored. Although these methods have been successful in reducing coupling capacitance and increasing speed, the additional process steps and thermal and mechanical stability issues caused by multiple process cycles are still key factors restricting their widespread application.

[0005] In summary, although the existing air gap technology provides an effective solution for reducing the RC delay problem in integrated circuits, especially in the back-end metal wiring, the introduction of complex process flows and the thermal and mechanical stability of new structures have not been fully resolved. Therefore, how to effectively introduce air gaps in a very small area during the CMOS back-end process integration without adding additional costs is of vital theoretical and practical significance for promoting the development of new storage technologies and CMOS hybrid integration. Summary of the invention

[0006] In response to the above technical challenges, the present invention proposes a method for preparing an air gap structure of a resistive memory array. This method is innovative based on the traditional CMOS process. By optimizing and adjusting the etching and deposition steps in the back-end manufacturing process, the periodic introduction of air gaps in high-density storage structures is achieved, thereby effectively reducing capacitive coupling and providing a technical basis for the commercialization of high-density new memory.

[0007] The technical solution provided by the present invention is as follows:

[0008] A method for preparing an air gap structure of a resistive memory array, the specific steps comprising:

[0009] 1) Based on the CMOS process, a first insulating dielectric layer is deposited after the front-end process is completed, a plurality of first interconnect metal layers are arranged in the first insulating dielectric layer, the first interconnect metal layers correspond to the resistive memory cells of the resistive memory array, and a first barrier layer is deposited above the first interconnect metal layer and the first insulating dielectric layer;

[0010] 2) etching a first through hole in the first barrier layer, and depositing an interconnection metal in the first through hole to form a connection end of the first interconnection metal layer;

[0011] 3) depositing a bottom electrode layer, a resistive material layer, a top electrode layer and a protective layer in sequence above the connection end of the first barrier layer and the first interconnect metal layer by physical vapor deposition (PVD), atomic layer deposition (ALD) or chemical vapor deposition (CVD) technology to form a stacked structure;

[0012] 4) etching the stacked structure to form a resistive switching memory unit;

[0013] 5) depositing a second barrier layer on the resistive memory unit, and etching a periodic groove structure between adjacent resistive memory units, wherein the sidewall of the groove is perpendicular to the bottom, and the depth-to-width ratio of the groove is 10:1 to 10:1000;

[0014] 6) then depositing a second insulating dielectric layer to form an air gap structure in the groove structure;

[0015] 7) Etching a second through hole in the second insulating dielectric layer, the second barrier layer and the protective layer, the second through hole being located above the top electrode of the resistive memory cell, and depositing a second interconnect metal layer in the second through hole to complete the preparation of the resistive memory array.

[0016] Through the above steps, the present invention not only optimizes the back-end process flow, but also significantly improves the performance of the integrated circuit by periodically self-forming an air gap structure, providing strong technical support for the commercialization of high-density new memory.

[0017] Furthermore, the material of the resistive layer is selected from AlOx, HfOx, TaOx, ZrOx, SiOx, VO x , MnOx, TiOx, CuOx, ZnOx, WOx, AgOx, SrTiOx, CaTiOx or one or more combinations of organic materials.

[0018] Furthermore, the first insulating dielectric layer and the second insulating dielectric layer include but are not limited to SiCOH, SiO2, SiLK, FOx, MSQ, porous materials, Nanoglass, HOSP, organic polymers and porous materials, carbon nanotubes and graphene, etc.

[0019] Furthermore, the first interconnection metal and the second interconnection metal are made of metal copper or metal aluminum.

[0020] Furthermore, the first barrier layer and the second barrier layer are made of silicon carbide thin films, and the protective layer is made of metal, metal nitride or conductive metal oxide.

[0021] The bottom electrode and the top electrode are made of metal, metal nitride or conductive metal oxide.

[0022] Furthermore, the first through hole is etched by using photolithography technology, and the second through hole is formed by using dual damascene process.

[0023] Beneficial effects of the present invention:

[0024] In the deposition process of the back-end resistive memory array, the present invention forms a periodic air gap in the dielectric layer by following specific design principles (such as accurately defining the device size and the spacing between cells) and fine-tuning the lateral and longitudinal etching depth-to-width ratio and etching rate, and utilizing a groove structure design with a high depth-to-width ratio and sharp edges (the junction of the sidewall and the horizontal plane). This technology effectively alleviates the signal delay problem caused by capacitive coupling and is of great significance for improving the performance of new memory technology in large-scale integration and production. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 A schematic diagram of an air gap structure of a resistive memory array prepared by the present invention;

[0026] Figure 2-10 Corresponding to the implementation steps of each embodiment.

[0027] Fig.11 for Figure 1-10 Legend for . DETAILED DESCRIPTION

[0028] In order to make the above features and advantages of the present invention more obvious and easy to understand, the following is a detailed description of the implementation examples with reference to the accompanying drawings.

[0029] The present invention provides a method for preparing an air gap structure of a resistive memory array, wherein the resistive memory cell in the resistive memory array uses TiN as the bottom electrode material and TaO x (or other chemically matched oxides) as the resistive layer material, and TiN as the top electrode material. The specific preparation method is as follows:

[0030] S1: Based on the CMOS process, the front-end process is completed, a first insulating dielectric layer is deposited, and a plurality of first interconnect metal layers are arranged in the insulating dielectric layer, each of which corresponds to a resistive memory cell, and a first barrier layer is deposited on the first interconnect metal and the first insulating dielectric layer. Figure 2 shown.

[0031] The interconnect metal layer may be made of metal copper or metal aluminum, the first insulating dielectric layer may be made of silicon oxide, and the barrier layer may be made of silicon carbide film.

[0032] S2: etching a first through hole in the first barrier layer, and depositing interconnection metal in the first through hole to form a connection end of the first interconnection metal layer, such as Figure 3 shown.

[0033] The through hole is etched using photolithography technology, and the interconnection metal deposited in the through hole is copper using a PVD process.

[0034] S3: by physical vapor deposition PVD, atomic layer deposition ALD or chemical vapor deposition CVD technology, a bottom electrode layer, a resistive material layer, a top electrode layer and a protective layer are sequentially deposited on the connection end of the first insulating dielectric layer and the first interconnect metal layer to form a stacked structure, such as Figure 4 shown.

[0035] The bottom electrode layer and the top electrode layer may be made of TiN, the protective layer may be made of TaN, the resistive material layer may be made of TaOx or HfOx, each layer may be deposited by PVD, the thickness of each layer may be 1 to 300 nm, and the stacked structure may be patterned by photolithography.

[0036] The resistive material layer can be a single layer or two or more layers of material, and the materials used are AlOx, HfOx, TaOx, ZrOx, SiOx, VO x , MnOx, TiOx, CuOx, ZnOx, WOx, AgOx, SrTiOx, CaTiOx or organic materials or a combination of multiple materials.

[0037] The material of the protective layer can also be metal (W, Cu, Al, Ta, Hf, Ti, Pt, Ir, Ru, Pd, etc.) or metal nitride (TiN, TaN, AlN) or conductive metal oxide (IrO, RuO, SrTiO).

[0038] S4: etching the stacked structure to form a resistive switching memory cell, thereby forming a resistive switching memory array, such as Figure 5 As shown;

[0039] S5: depositing a second barrier layer on the resistive memory array; Figure 6 As shown, the second barrier layer is then etched to form a periodic groove structure between adjacent resistive memory cells, the sidewall of the groove is perpendicular to the bottom, and the depth-to-width ratio of the groove is 10:1 to 10:1000.

[0040] The second barrier layer may include a silicon carbide film with a thickness of 1 to 100 nm, which is mainly used to protect the resistive memory array; after the second barrier layer is deposited, the lateral and longitudinal etching aspect ratios and etching rates are adjusted to form a groove with a higher aspect ratio and a steep area (the sidewall of the groove is perpendicular to the bottom), such as Figure 7 shown.

[0041] S6: Deposit a second insulating dielectric layer to form a periodic air gap, such as Figure 8 shown.

[0042] The groove has a high aspect ratio and a steep area structure, which results in different deposition rates at the bottom and sidewalls of the groove during the PVD dielectric layer process, thereby forming a periodic air gap in the dielectric layer, which mitigates the speed drop caused by capacitive coupling.

[0043] S7: etching a second through hole in the second insulating dielectric layer, the second barrier layer and the protective layer, wherein the second through hole is located above the top electrode of the resistive memory cell. Fig. 9 As shown, by depositing the second interconnect metal, the preparation of the resistive switching memory array is completed, such as Fig.10 shown.

[0044] The second through hole is etched using a dual damascene process and filled with metal copper or aluminum as interconnection metal.

[0045] In this embodiment, after each layer is deposited, a CMP (Chemical Mechanical Polishing) process is used to perform a planarization process.

[0046] As described above, the resistive random access memory and the method for preparing the same according to the present invention are described by way of example with reference to the accompanying drawings. However, it should be understood by those skilled in the art that various improvements can be made to the resistive random access memory and the method for preparing the same according to the present invention without departing from the content of the present invention. Therefore, the protection scope of the present invention should be determined by the content of the attached claims.

Claims

1. A method for preparing an air gap structure of a resistive memory array, characterized in that: The specific steps include: 1) Based on the CMOS process, a first insulating dielectric layer is deposited after the front-end process is completed, a plurality of first interconnect metal layers are arranged in the first insulating dielectric layer, the first interconnect metal layers correspond to the resistive memory cells of the resistive memory array, and a first barrier layer is deposited above the first interconnect metal layer and the first insulating dielectric layer; 2) etching a first through hole in the first barrier layer, and depositing an interconnection metal in the first through hole to form a connection end of the first interconnection metal layer; 3) depositing a bottom electrode layer, a resistive material layer, a top electrode layer and a protective layer in sequence above the connection end of the first barrier layer and the first interconnect metal layer by physical vapor deposition (PVD), atomic layer deposition (ALD) or chemical vapor deposition (CVD) technology to form a stacked structure; 4) etching the stacked structure to form a resistive switching memory unit; 5) depositing a second barrier layer on the resistive memory unit, and etching a periodic groove structure between adjacent resistive memory units, wherein the sidewall of the groove is perpendicular to the bottom, and the depth-to-width ratio of the groove is 10:1 to 10:1000; 6) then depositing a second insulating dielectric layer to form an air gap structure in the groove structure; 7) Etching a second through hole in the second insulating dielectric layer, the second barrier layer and the protective layer, the second through hole being located above the top electrode of the resistive memory cell, and depositing a second interconnect metal layer in the second through hole to complete the preparation of the resistive memory array.

2. The preparation method according to claim 1, characterized in that The resistive material layer is selected from AlOx, HfOx, TaOx, ZrOx, SiOx, VO x , MnOx, TiOx, CuOx, ZnOx, WOx, AgOx, SrTiOx, CaTiOx or a combination of one or more organic materials.

3. The preparation method according to claim 1, characterized in that: The first insulating dielectric layer and the second insulating dielectric layer are made of SiCOH, SiO2, SiLK, Fox, MSQ, or porous materials, Nanoglass, HOSP, organic polymers or pore materials, and carbon nanotubes or graphene.

4. The preparation method according to claim 1, characterized in that: The first interconnection metal or the second interconnection metal is made of metal copper or metal aluminum.

5. The preparation method according to claim 1, characterized in that: The first barrier layer or the second barrier layer is made of a silicon carbide film.

6. The preparation method according to claim 1, characterized in that: The protective layer is made of metal, metal nitride or conductive metal oxide.

7. The preparation method according to claim 1, characterized in that: The bottom electrode or the top electrode is made of metal, metal nitride or conductive metal oxide.

Citation Information

Patent Citations

  • Three-dimensional nonvolatile memory array and preparation method thereof

    CN101976676A

  • Preparation method of three-dimensional resistive random access memory retaining air layer

    CN105405972A

  • Preparation method of metal interlayer dielectric layer in electrically induced resistive random access memory

    CN117202669A

  • Method and Apparatus for Composing Image by using Image and Thermal Image

    KR102003475B1

  • Resistive memory and preparation method therefor

    WO2022143886A1