Piezoelectric stack structure, micro electro mechanical system and preparation method of piezoelectric stack structure
By introducing a repair layer with a lower concentration of doped elements into the piezoelectric stack structure, the problem of unevenness of the second piezoelectric thin film is solved, the film formation quality and piezoelectric performance are improved, and higher sensitivity is achieved.
Patent Information
- Application Number
- CN202411366736.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing piezoelectric stack structure, the second piezoelectric film is uneven due to lattice mismatch caused by scandium doped aluminum nitride, which affects the film formation quality and is transferred to the top electrode, thereby affecting the quality of the piezoelectric device.
The repair layer with a lower concentration of doped elements is introduced into the piezoelectric stack structure. The repair layer is the same as the piezoelectric layer material and is located on the side of the electrode layer farthest away from the substrate layer to mitigate the bits caused by lattice mismatch Faults and hollow defects improve the flatness of the upper film layer.
The flatness of the film layer above the repair layer is significantly improved, the number of abnormal grains is reduced, the film formation quality is improved, and the piezoelectric performance and sensitivity of the piezoelectric stack structure are improved.
Smart Images

Figure CN118890952A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a piezoelectric stack structure, a micro-electromechanical system, and a method for preparing the piezoelectric stack structure. Background Art
[0002] Piezoelectric stack structure is an important component of micro-electromechanical system, please refer to Figure 1 The existing piezoelectric stack structure 10 includes a bottom electrode 11, a first piezoelectric film 12, an intermediate electrode 13, a second piezoelectric film 14 and a top electrode 15 stacked sequentially on the bottom electrode 11. Compared with the conventional sandwich piezoelectric structure having a single piezoelectric film sandwiched between two layers of electrodes, the existing piezoelectric stack structure 10 has better piezoelectric performance and higher sensitivity.
[0003] However, please refer to Figure 2 and Figure 3 In the actual growth process, the second piezoelectric film 14 is usually extremely uneven. The reason is that after the scandium atoms are doped into the first piezoelectric film 12 and the second piezoelectric film 14, the scandium-doped aluminum nitride (AlScN) will cause defects such as dislocations and voids due to lattice mismatch, especially at high-energy grain boundaries. Abnormally oriented grains will be formed, and the number of abnormal grains increases with the increase of scandium content and film thickness. Macroscopically, it is reflected in the fact that the surface of the second piezoelectric film 14 of the existing piezoelectric stack structure 10 generally has the phenomenon of uneven growth. The unevenness of the second piezoelectric film 14 will not only directly affect the performance of the second piezoelectric film 14, but also transfer these defects to the top electrode 15, thereby affecting the film quality of the top electrode 15, and further affecting the quality of the piezoelectric device. In addition, this unevenness can easily lead to uneven thickness of subsequent films, and the unevenness will accumulate and amplify, causing greater impact on subsequent processes, including but not limited to causing changes in the depth of the lithography focus during lithography, affecting the quality of the lithography pattern; increasing the difficulty of etching, resulting in distortion of the etched pattern or increased residue, etc. Summary of the invention
[0004] The purpose of the present application is to provide a piezoelectric stack structure, a micro-electromechanical system and a method for preparing a piezoelectric stack structure in response to the deficiencies in the above-mentioned prior art, which can greatly improve the unevenness of the upper film layer and improve the film formation quality of the upper film layer.
[0005] To achieve the above purpose, the technical solution adopted in the embodiment of the present application is as follows: According to a first aspect of an embodiment of the present application, a piezoelectric stack structure is provided, which is configured on a substrate layer and includes: at least three electrode layers stacked together, with at least one piezoelectric layer provided between two adjacent electrode layers; the piezoelectric stack structure also includes at least one repair layer, which is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer, the repair layer and the piezoelectric layer are made of the same material, and the concentration of the doped element in the material of the repair layer is lower than the concentration of the doped element in the material of the piezoelectric layer.
[0006] Optionally, the piezoelectric stack structure includes a first electrode layer, a second electrode layer and a third electrode layer stacked in sequence, a first piezoelectric layer is arranged between the first electrode layer and the second electrode layer, and a second piezoelectric layer is arranged between the second electrode layer and the third electrode layer; the repair layer is located between the second electrode layer and the first piezoelectric layer, or the repair layer is located between the second electrode layer and the second piezoelectric layer.
[0007] Optionally, one surface of the repair layer is in contact with the second electrode layer.
[0008] Optionally, when the repair layer is located between the second electrode layer and the first piezoelectric layer, the other surface of the repair layer is in contact with the first piezoelectric layer; when the repair layer is located between the second electrode layer and the second piezoelectric layer, the other surface of the repair layer is in contact with the second piezoelectric layer.
[0009] Optionally, the materials of the piezoelectric layer and the repair layer are both scandium-doped aluminum nitride, and the scandium doping concentration of the repair layer is lower than the scandium doping concentration of the piezoelectric layer.
[0010] Optionally, the thickness of the repair layer is smaller than the thickness of the piezoelectric layer.
[0011] Optionally, when the number of the repair layers is at least two, at least two repair layers are stacked and arranged, and two adjacent repair layers are arranged with an interval therebetween.
[0012] A second aspect of an embodiment of the present application provides another piezoelectric stack structure, which is configured on a substrate layer and includes: at least three electrode layers stacked together, with at least one piezoelectric layer provided between two adjacent electrode layers; the piezoelectric stack structure also includes at least one repair layer, the repair layer is located on the side of the piezoelectric layer closest to the substrate layer facing away from the substrate layer, the material of the piezoelectric layer is a preset piezoelectric material doped with doping elements, and the material of the repair layer is a preset piezoelectric material not doped with doping elements.
[0013] According to a third aspect of the embodiments of the present application, a micro-electromechanical system is provided, comprising a substrate and a piezoelectric stack structure as described above and arranged on the substrate.
[0014] According to a fourth aspect of an embodiment of the present application, a method for preparing a piezoelectric stack structure is provided, comprising: providing a substrate layer, and forming at least three electrode layers, at least two piezoelectric layers and at least one repair layer stacked on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, the repair layer is located on a side of the electrode layer farthest from the substrate layer facing the substrate layer, the materials of the repair layer and the piezoelectric layer are the same, and the concentration of the doped elements in the material of the repair layer is lower than the concentration of the doped elements in the material of the piezoelectric layer.
[0015] Optionally, the preparation method of the piezoelectric stack structure includes: providing a substrate layer, and sequentially forming a first electrode layer, a first piezoelectric layer, a second electrode layer, a second piezoelectric layer and a third electrode layer in a stacked arrangement on the substrate, and forming a repair layer between the second electrode layer and the first piezoelectric layer, and / or between the second electrode layer and the second piezoelectric layer, wherein the material of the repair layer and the piezoelectric layer is the same, and the concentration of the doped element in the material of the repair layer is lower than the concentration of the doped element in the material of the piezoelectric layer.
[0016] Optionally, the preparation method of the piezoelectric stack structure includes: providing a substrate layer, and forming at least three electrode layers, at least two piezoelectric layers and at least two repair layers in a stacked arrangement on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, the repair layer is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer, the two adjacent repair layers are spaced apart, the materials of the repair layer and the piezoelectric layer are the same, and the concentration of the doped elements in the material of the repair layer is lower than the concentration of the doped elements in the material of the piezoelectric layer.
[0017] A fifth aspect of an embodiment of the present application provides another method for preparing a piezoelectric stack structure, comprising: providing a substrate layer, and forming at least three electrode layers, at least two piezoelectric layers and at least one repair layer stacked on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, the repair layer is located on the side of the piezoelectric layer closest to the substrate layer facing away from the substrate layer, the material of the piezoelectric layer is a preset piezoelectric material doped with an impurity element, and the material of the repair layer is a preset piezoelectric material not doped with an impurity element.
[0018] The beneficial effects of this application include: The present application provides a piezoelectric stack structure, which is configured on a substrate layer. The piezoelectric stack structure includes: at least three electrode layers stacked together, at least one piezoelectric layer is provided between two adjacent electrode layers; the piezoelectric stack structure also includes at least one repair layer, the repair layer is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer, the repair layer and the piezoelectric layer are made of the same material, and the concentration of doping elements in the material of the repair layer is lower than the concentration of doping elements in the material of the piezoelectric layer. The piezoelectric stack structure greatly improves the unevenness of the film layer above the repair layer by introducing a repair layer with a lower concentration of doping elements, thereby improving the film forming quality of the upper film layer. It can be observed from the morphology image under a microscope that the flatness of the piezoelectric layer and the electrode layer above the repair layer has been greatly improved, and the number of abnormal grains in the piezoelectric layer has been significantly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A schematic diagram of film formation of an existing piezoelectric stack structure; Figure 2 The morphology of the cross section of the existing piezoelectric stack structure under a microscope; Figure 3 The figure is a morphology diagram of the second piezoelectric film in the existing piezoelectric stack structure under a microscope; Figure 4 One of the structural schematic diagrams of the piezoelectric stack structure provided in the embodiment of the present application; Figure 5 The second structural schematic diagram of the piezoelectric stack structure provided in the embodiment of the present application; Figure 6 The third structural schematic diagram of the piezoelectric stack structure provided in the embodiment of the present application; Figure 7 A fourth structural schematic diagram of a piezoelectric stack structure provided in an embodiment of the present application; Figure 8 A morphological diagram of a cross section of a piezoelectric stack structure provided in an embodiment of the present application under a microscope; Fig. 9 A morphology image of the second piezoelectric layer in the piezoelectric stack structure provided in an embodiment of the present application under a microscope; Fig.10 The morphology comparison diagram of the second piezoelectric layer on the repair layer with different scandium doping concentrations when the repair layer thickness is 100 nm; Fig.11 A comparison of the piezoelectric responses of an existing piezoelectric stack structure and a piezoelectric stack structure provided in an embodiment of the present application; Fig.12 This is a comparison diagram of the morphologies of the second piezoelectric layer on the repair layer with different thicknesses when the scandium doping concentration of the repair layer is 10%; Fig.13 Piezoelectric response of the piezoelectric stack structure corresponding to the repair layer of different thicknesses under a certain pressure.
[0021] Icon: 10-existing piezoelectric stack structure; 11-bottom electrode; 12-first piezoelectric film; 13-middle electrode; 14-second piezoelectric film; 15-top electrode; 100-piezoelectric stack structure; 110-electrode layer; 120-piezoelectric layer; 130-repair layer; 140-other film layers; A-preset direction. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0023] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. It should be noted that, in the absence of conflict, the various features in the embodiments of the present application can be combined with each other, and the combined embodiments are still within the scope of protection of the present application.
[0024] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0025] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, or the positions or positional relationships in which the product of the application is usually placed when in use. They are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific position, be constructed and operated in a specific position, and therefore cannot be understood as a limitation on the present application. In addition, the terms "first", "second", "third", etc. are only used to distinguish the description, and cannot be understood as indicating or implying relative importance.
[0026] In the description of this application, it should also be noted that, unless otherwise clearly specified and limited, the terms "set", "install", "connect", and "connect" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0027] For the first aspect of the embodiment of the present application, please refer to Figure 4 and Figure 5 , a piezoelectric stack structure 100 is provided, which is configured on a substrate layer. The piezoelectric stack structure 100 includes: at least three electrode layers 110 are stacked, and at least one piezoelectric layer 120 is arranged between two adjacent electrode layers 110; the piezoelectric stack structure 100 also includes at least one repair layer 130, the repair layer 130 is located on the side of the electrode layer 110 farthest from the substrate layer facing the substrate layer, the repair layer 130 and the piezoelectric layer 120 are made of the same material, and the concentration of the doping element in the material of the repair layer 130 is lower than the concentration of the doping element in the material of the piezoelectric layer 120.
[0028] Please refer to Figure 6 The piezoelectric stack structure 100 has a plurality of film layers, which at least include an electrode layer 110, a piezoelectric layer 120 and a repair layer 130, and may also include other film layers 140. The plurality of film layers are stacked on the substrate layer along a preset direction A, wherein the preset direction A is preferably perpendicular to the surface of the substrate layer.
[0029] Please refer to Figure 7 , the number of electrode layers 110 is at least three, and may also be four, five or more layers. The multiple electrode layers 110 are arranged in parallel, and at least one piezoelectric layer 120 is provided between two adjacent electrode layers 110. In other words, the number of piezoelectric layers 120 between two adjacent electrode layers 110 may be one, or two or more layers. When the number of piezoelectric layers 120 between two adjacent electrode layers 110 is two or more layers, preferably, the two adjacent piezoelectric layers 120 are arranged at intervals, and a repair layer 130 may be provided between the two adjacent piezoelectric layers 120, or other film layers 140 may be provided.
[0030] The repair layer 130 is located on the side of the electrode layer 110 farthest from the substrate layer toward the substrate layer, that is, the repair layer 130 is located between the substrate layer and the electrode layer 110 farthest from the substrate layer. The number of the repair layer 130 can be one, two, or more layers, and the setting position can be between any adjacent electrode layer 110 and piezoelectric layer 120, or between two adjacent piezoelectric layers 120. When the number of the repair layer 130 is two or more layers, preferably, at least two layers of the repair layer 130 are stacked, and the two adjacent layers of the repair layer 130 are spaced apart, so as to achieve a better repair effect.
[0031] It should be noted that the adjacent electrode layers 110 and piezoelectric layers 120 , the electrode layers 110 and the repairing layers 130 , and the piezoelectric layers 120 and the repairing layers 130 can be directly bonded together, or other film layers 140 can be provided.
[0032] The repair layer 130 and the piezoelectric layer 120 are made of the same material, and the concentration of the doping element in the material of the repair layer 130 is lower than the concentration of the doping element in the material of the piezoelectric layer 120. That is, the materials used in the repair layer 130 and the piezoelectric layer 120 have the same constituent elements, and at least one of the constituent elements is a doping element used to improve the piezoelectric properties of the material, and the concentration of the doping element in the material used in the repair layer 130 is lower than the concentration of the doping element in the material used in the piezoelectric layer 120. For example, if the material of the piezoelectric layer 120 is composed of three elements, B, C, and D, and D is a doping element, then the material of the repair layer 130 is also composed of three elements, B, C, and D, and D is a doping element, and the concentration of D in the repair layer 130 is lower than the concentration of D in the piezoelectric layer 120.
[0033] The repair layer 130 and the piezoelectric layer 120 are made of the same material, which can reduce the effect of the repair layer 130 on the piezoelectric performance of the piezoelectric stack structure 100. If the concentration of the doping element in the repair layer 130 is lower than that in the piezoelectric layer 120, the repair layer 130 can play a good transition role, gradually alleviating defects such as dislocations and voids caused by lattice mismatch, and inhibiting the formation of abnormally oriented grains at high-energy grain boundaries, thereby improving the flatness and film quality of other film layers 140 (such as the piezoelectric layer 120 and the electrode layer 110) above the repair layer 130.
[0034] It should be noted that, when the number of piezoelectric layers 120 is two or more, if the concentrations of doping elements in the materials of the two or more piezoelectric layers 120 are different, the concentration of doping elements in the material of the repair layer 130 should at least be lower than the concentration of doping elements in the material of the piezoelectric layer 120 above the repair layer 130 and closest to the repair layer 130. More preferably, the concentration of doping elements in the material of the repair layer 130 is lower than the concentration of doping elements in the materials of all piezoelectric layers 120.
[0035] Please refer to Figure 4 , Figure 8 and Fig. 9 The piezoelectric stack structure 100 introduces a repair layer 130 with a low concentration of doping elements between the substrate layer and the electrode layer 110 farthest from the substrate layer, which greatly improves the unevenness of the film layer above the repair layer 130, thereby improving the film quality of the upper film layer. It can be observed from the morphology under a microscope that the flatness of the piezoelectric layer 120 and the electrode layer 110 located above the repair layer 130 has been greatly improved, and the number of abnormal grains in the piezoelectric layer 120 has been significantly reduced.
[0036] Optionally, the materials of the piezoelectric layer 120 and the repairing layer 130 are both scandium-doped aluminum nitride (ScAlN), and the scandium doping concentration of the repairing layer 130 is lower than the scandium doping concentration of the piezoelectric layer 120 .
[0037] At this time, the constituent elements of the piezoelectric layer 120 and the repair layer 130 are scandium, nitrogen and aluminum, among which scandium is a doping element. The piezoelectric layer 120 prepared using ScAlN has the advantages of high acoustic velocity, good thermal stability and wide band gap. It can still maintain stable performance under high temperature and harsh environment, and is very suitable for application scenarios that require high stability. Moreover, ScAlN is compatible with CMOS process, which means that it can be easily integrated into micro-electromechanical systems, which is of great significance for improving system performance and reducing costs. In addition, through scandium doping modification, the piezoelectric constant of the ScAlN film is more than twice that of the aluminum nitride (AlN) film, which greatly improves its performance as a piezoelectric material.
[0038] Optionally, the scandium doping concentration of the piezoelectric layer 120 is 18%-22%.
[0039] Theoretically, when the atomic fraction of Sc in AlScN is in the range of 0-40%, the greater the atomic fraction of Sc doped, the higher the piezoelectric response of the material. However, in the actual thin film growth process, as the atomic fraction of Sc gradually increases, the defects of the piezoelectric layer 120 located at the upper position in the piezoelectric stack structure 100 will become more and more obvious, and these defects will reduce the piezoelectric performance of the piezoelectric stack structure 100. Therefore, by limiting the scandium doping concentration of the piezoelectric layer 120 to the range of 18%-22%, and combining it with a repair layer 130 with a lower scandium doping concentration, a balance can be found between the piezoelectric response and the influence of defects, so that the piezoelectric stack structure 100 has both good piezoelectric performance and film quality.
[0040] Optionally, the scandium doping concentration of the repair layer 130 is 8%-12%.
[0041] Please refer to Fig.10When the scandium doping concentration of the repair layer 130 is 8%-12%, only a few pyramid-shaped precipitation particles appear on the surface of the second piezoelectric layer. At this time, the film quality of the second piezoelectric layer has reached a relatively high level. The repair layer 130 plays a good repairing role, and the piezoelectric response of the piezoelectric stack structure 100 is also greatly improved. When the scandium doping concentration of the repair layer 130 is less than 8% and gradually decreases, the quality of the second piezoelectric layer is not significantly improved, but the piezoelectric response of the piezoelectric stack structure 100 will be significantly reduced. When the scandium doping concentration of the repair layer 130 is greater than 12% and gradually increases, the piezoelectric response of the piezoelectric stack structure 100 will be improved to a certain extent, but the film quality of the second piezoelectric layer will be significantly deteriorated.
[0042] Therefore, the scandium doping concentration of the repair layer 130 is preferably 8%-12%. Furthermore, the scandium doping concentration of the repair layer 130 is 10%. At this time, a better balance can be achieved between the repair effect of the repair layer 130 and the piezoelectric performance of the piezoelectric stack structure 100.
[0043] Optionally, please refer again to Figure 4 and Figure 5 The piezoelectric stack structure 100 includes a first electrode layer, a second electrode layer and a third electrode layer stacked in sequence, a first piezoelectric layer is arranged between the first electrode layer and the second electrode layer, and a second piezoelectric layer is arranged between the second electrode layer and the third electrode layer; the repair layer 130 is located between the second electrode layer and the first piezoelectric layer, or the repair layer 130 is located between the second electrode layer and the second piezoelectric layer.
[0044] The piezoelectric stack structure 100 includes three electrode layers 110 and two piezoelectric layers 120, which are the first electrode layer, the first piezoelectric layer, the second electrode layer, the second piezoelectric layer and the third electrode layer in sequence along the preset direction A, wherein the first electrode layer is the electrode layer 110 closest to the substrate layer, and the third electrode layer is the electrode layer 110 farthest from the substrate layer. The number of repair layers 130 is not limited. When the number of repair layers 130 is one layer, the repair layer 130 is located between the second electrode layer and the first piezoelectric layer, or the repair layer 130 is located between the second electrode layer and the second piezoelectric layer; when the number of repair layers 130 is at least two layers, at least two repair layers 130 can be located between the second electrode layer and the first piezoelectric layer, or can be located between the second electrode layer and the second piezoelectric layer, or part of the repair layer 130 is located between the second electrode layer and the first piezoelectric layer, and another part of the repair layer 130 is located between the second electrode layer and the second piezoelectric layer.
[0045] The above-mentioned piezoelectric stack structure 100 greatly improves the unevenness of the second piezoelectric layer and the third electrode layer by introducing at least one repair layer 130 with a lower doping element concentration between the first piezoelectric layer and the second piezoelectric layer with a higher doping element concentration, thereby improving the film forming quality of the second piezoelectric layer and the third electrode layer, so that the piezoelectric stack structure 100 has better piezoelectric performance and higher sensitivity.
[0046] Optionally, one surface of the repair layer 130 is in contact with the second electrode layer.
[0047] When the piezoelectric stack structure 100 is subjected to external force, the positions of the third electrode layer and the first electrode layer are the positions with the maximum compressive stress and tensile stress, respectively. The position of the second electrode layer coincides with the neutral layer of the piezoelectric stack structure 100. When the piezoelectric stack structure 100 is subjected to external force, the second electrode layer and its surroundings are the areas with the minimum strain. The piezoelectric material in this area contributes the least to the piezoelectric response of the overall piezoelectric stack structure 100. Therefore, setting the repair layer 130 to fit the second electrode layer can minimize the influence of the repair layer 130 on the overall piezoelectric performance of the piezoelectric stack structure 100.
[0048] Fig.11 The simulation was compared Figure 1 Existing piezoelectric stack structure 10, Figure 5 The piezoelectric response of the piezoelectric stack structure 100 with the repair layer 130 deposited on the second electrode layer. Fig.11 It can be seen that the introduction of the repair layer 130 has little effect on the piezoelectric response of the piezoelectric stack structure 100. Therefore, the introduction of the repair layer 130 close to the second electrode layer can not only play a significant role in repairing the second piezoelectric layer of the piezoelectric stack structure 100, but also minimize the impact of the repair layer 130 on the piezoelectric performance of the piezoelectric stack structure 100.
[0049] Optionally, when the repair layer 130 is located between the second electrode layer and the first piezoelectric layer, the other surface of the repair layer 130 is in contact with the first piezoelectric layer; when the repair layer 130 is located between the second electrode layer and the second piezoelectric layer, the other surface of the repair layer 130 is in contact with the second piezoelectric layer. This arrangement can further reduce the influence of the repair layer 130 on the overall piezoelectric performance of the piezoelectric stack structure 100.
[0050] Optionally, see Figure 4 and Figure 5 , the thickness of the repair layer 130 is less than the thickness of the piezoelectric layer 120. In this way, the piezoelectric performance of the piezoelectric stack structure 100 can be improved.
[0051] It should be noted that the thickness of the film layer refers to the size of the film layer in the preset direction A. Therefore, the thickness of the repair layer 130 refers to the size of the repair layer 130 in the preset direction A, and the thickness of the piezoelectric layer 120 refers to the size of the piezoelectric layer 120 in the preset direction A. Given that the number of the piezoelectric layers 120 is at least two, the thickness of the repair layer 130 is less than the thickness of any one of the piezoelectric layers 120.
[0052] Optionally, the repair layer 130 has a thickness of 80 nm-100 nm.
[0053] Please refer to Fig.12 , comparing the repair effects of the repair layer 130 with different thicknesses at the same scandium doping concentration, it can be seen that when the thickness of the repair layer 130 gradually increases from 0 nm to 200 nm, its repair effect is initially significantly improved, but when the thickness of the repair layer 130 exceeds 100 nm, the improvement of its repair effect gradually slows down and reaches a certain limit. However, please refer to Fig.13 , when the thickness of the repair layer 130 gradually increases, the overall piezoelectric response of the piezoelectric stack structure 100 will drop linearly. Therefore, when the thickness of the repair layer 130 is 80nm-100nm, the repair effect of the repair layer 130 is better and the piezoelectric performance of the piezoelectric stack structure 100 is also better. More preferably, the thickness of the repair layer 130 is 100 nm. At this time, a better balance can be achieved between the repair effect of the repair layer 130 and the piezoelectric performance of the piezoelectric stack structure 100.
[0054] For the second aspect of the embodiment of the present application, please refer to Figure 4 and Figure 5 , another piezoelectric stack structure 100 is provided, which is configured on a substrate layer. The piezoelectric stack structure 100 includes: at least three electrode layers 110 are stacked, and at least one piezoelectric layer 120 is arranged between two adjacent electrode layers 110; the piezoelectric stack structure 100 also includes at least one repair layer 130, the repair layer 130 is located on the side of the piezoelectric layer 120 closest to the substrate layer away from the substrate layer, the material of the piezoelectric layer 120 is a preset piezoelectric material doped with a doping element, and the material of the repair layer 130 is a preset piezoelectric material not doped with a doping element.
[0055] The main differences between this embodiment and the previous embodiment are: first, the location of the repair layer 130 is different. In this embodiment, the repair layer 130 is located between the piezoelectric layer 120 closest to the substrate layer and the electrode layer 110 farthest from the substrate layer; second, the concentration of the doping element in the repair layer 130 is different. In this embodiment, the material of the repair layer 130 is still the same as that of the piezoelectric layer 120, but no doping element is added to the repair layer 130. For example, if the material of the piezoelectric layer 120 is composed of three elements, B, C and D, and D is the doping element, then the material of the repair layer 130 is composed of two elements, B and C, and does not contain D.
[0056] By way of example, the material of the piezoelectric layer 120 is scandium-doped aluminum nitride (ScAlN), and the material of the repair layer 130 is aluminum nitride (AlN).
[0057] The above-mentioned piezoelectric stack structure 100 can also improve the unevenness of the film layer above the repair layer 130 by introducing a repair layer 130 without doping elements between the piezoelectric layer 120 closest to the substrate layer and the electrode layer 110 farthest from the substrate layer, thereby improving the film formation quality of the upper film layer.
[0058] According to a third aspect of the embodiments of the present application, a micro-electromechanical system is provided, comprising a substrate and a piezoelectric stack structure 100 as described above and arranged on the substrate.
[0059] The micro-electromechanical system includes the same structure and beneficial effects as the piezoelectric stack structure 100 in the aforementioned embodiment. The structure and beneficial effects of the piezoelectric stack structure 100 have been described in detail in the aforementioned embodiment and will not be repeated here.
[0060] In a fourth aspect of the present application, a method for preparing a piezoelectric stack structure 100 is provided. Figure 7 ,include: A substrate layer is provided, and at least three electrode layers 110, at least two piezoelectric layers 120 and at least one repair layer 130 are stacked on the substrate layer, wherein at least one piezoelectric layer 120 is provided between two adjacent electrode layers 110, and the repair layer 130 is located on the side of the electrode layer 110 that is farthest from the substrate layer and faces the substrate layer. The materials of the repair layer 130 and the piezoelectric layer 120 are the same, and the concentration of the doped elements in the material of the repair layer 130 is lower than the concentration of the doped elements in the material of the piezoelectric layer 120.
[0061] The preparation method of the piezoelectric stack structure 100 introduces a repair layer 130 with a lower doping element concentration between the substrate layer and the electrode layer 110 farthest from the substrate layer, thereby greatly improving the unevenness of the film layer above the repair layer 130 and thus improving the film formation quality of the upper film layer.
[0062] Optionally, the preparation method of the piezoelectric stack structure 100 includes: providing a substrate layer, and forming at least three electrode layers 110, at least two piezoelectric layers 120 and at least two repair layers 130 stacked on the substrate layer, wherein there is at least one piezoelectric layer 120 between two adjacent electrode layers 110, the repair layer 130 is located on the side of the electrode layer 110 farthest from the substrate layer facing the substrate layer, the two adjacent repair layers 130 are spaced apart, the materials of the repair layer 130 and the piezoelectric layer 120 are the same, and the concentration of the doped elements in the material of the repair layer 130 is lower than the concentration of the doped elements in the material of the piezoelectric layer 120.
[0063] The method for preparing the piezoelectric stack structure 100 can further improve the unevenness of the film layer above the repair layer 130 by arranging at least two repair layers 130 at intervals, thereby improving the film formation quality of the upper film layer.
[0064] Optionally, see Figure 4 and Figure 5 , the preparation method of the piezoelectric stack structure 100 includes: A substrate layer is provided, and a first electrode layer, a first piezoelectric layer, a second electrode layer, a second piezoelectric layer and a third electrode layer are stacked in sequence on the substrate, and a repair layer 130 is formed between the second electrode layer and the first piezoelectric layer, and / or between the second electrode layer and the second piezoelectric layer, wherein the material of the repair layer 130 and the piezoelectric layer 120 is the same, and the concentration of the doped element in the material of the repair layer 130 is lower than the concentration of the doped element in the material of the piezoelectric layer 120.
[0065] The preparation method of the above-mentioned piezoelectric stack structure 100 greatly improves the unevenness of the second piezoelectric layer and the third electrode layer by introducing at least one repair layer 130 with a lower doping element concentration between the first piezoelectric layer and the second piezoelectric layer with a higher doping element concentration, thereby improving the film forming quality of the second piezoelectric layer and the third electrode layer, so that the prepared piezoelectric stack structure 100 has better piezoelectric performance and higher sensitivity.
[0066] According to a fifth aspect of an embodiment of the present application, another method for preparing a piezoelectric stack structure 100 is provided, comprising: providing a substrate layer, and forming at least three electrode layers 110, at least two piezoelectric layers 120 and at least one repair layer 130 stacked on the substrate layer, wherein at least one piezoelectric layer 120 is provided between two adjacent electrode layers 110, the repair layer 130 is located on the side of the piezoelectric layer 120 closest to the substrate layer facing away from the substrate layer, the material of the piezoelectric layer 120 is a preset piezoelectric material doped with an impurity element, and the material of the repair layer 130 is a preset piezoelectric material not doped with an impurity element.
[0067] The preparation method of the above-mentioned piezoelectric stack structure 100 greatly improves the unevenness of the film layer above the repair layer 130 by introducing a repair layer 130 without doping elements between the piezoelectric layer 120 closest to the substrate layer and the electrode layer 110 farthest from the substrate layer, thereby improving the film formation quality of the upper film layer.
[0068] In the embodiment of the method for preparing the piezoelectric stack structure 100 , the preparation methods of the electrode layer 110 , the piezoelectric layer 120 and the repair layer 130 are not limited.
[0069] For example, a layer of electrode material is deposited on the surface of the lower film layer by metal sputtering process, and the electrode material is patterned by photolithography and etching process to form electrode layer 110. The electrode material can be molybdenum, and the deposition thickness of the electrode material can be between 30nm and 60nm.
[0070] For example, a layer of ScAlN is deposited on the surface of the lower film layer by using a reactive sputtering process in a nitrogen atmosphere and a high-purity Al-Sc alloy target, wherein the scandium doping concentration (i.e., the atomic fraction of Sc) of the ScAlN is determined by the content of Sc in the Al-Sc alloy target; and the ScAlN film layer is patterned by using a photolithography and etching process to form the piezoelectric layer 120. The thickness of the piezoelectric layer 120 may be between 300 nm and 500 nm.
[0071] For example, a layer of ScAlN is deposited on the surface of the lower film layer by using a reactive sputtering process in a nitrogen atmosphere and a high-purity Al-Sc alloy target, wherein the scandium doping concentration (i.e., the atomic fraction of Sc) of the ScAlN is determined by the content of Sc in the Al-Sc alloy target; and the ScAlN film layer is patterned by using a photolithography and etching process to form a repair layer 130. The thickness of the repair layer 130 may be between 80nm and 100nm.
[0072] Please note that, please refer to Figure 6 and Figure 7 , the lower film layer refers to the film layer located below the film layer to be prepared. When preparing the electrode layer 110, the lower film layer may be the substrate layer, the piezoelectric layer 120, the repair layer 130 or other film layers 140; when preparing the piezoelectric layer 120, the lower film layer may be the electrode layer 110, the repair layer 130 or other film layers 140; when preparing the repair layer 130, the lower film layer may be the substrate layer, the piezoelectric layer 120, the electrode layer 110 or other film layers 140.
[0073] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A piezoelectric stack structure, arranged on a substrate layer, characterized in that: include: At least three electrode layers are stacked, and at least one piezoelectric layer is provided between two adjacent electrode layers; The piezoelectric stack structure also includes at least one repair layer, which is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer. The repair layer and the piezoelectric layer are made of the same material, and the concentration of the doping element in the material of the repair layer is lower than the concentration of the doping element in the material of the piezoelectric layer.
2. The piezoelectric stack structure according to claim 1, wherein: It comprises a first electrode layer, a second electrode layer and a third electrode layer which are stacked in sequence, a first piezoelectric layer is arranged between the first electrode layer and the second electrode layer, and a second piezoelectric layer is arranged between the second electrode layer and the third electrode layer; The repair layer is located between the second electrode layer and the first piezoelectric layer, or the repair layer is located between the second electrode layer and the second piezoelectric layer.
3. The piezoelectric stack structure according to claim 2, wherein: One surface of the repair layer is in contact with the second electrode layer.
4. The piezoelectric stack structure according to claim 3, wherein: When the repair layer is located between the second electrode layer and the first piezoelectric layer, the other surface of the repair layer is in contact with the first piezoelectric layer; when the repair layer is located between the second electrode layer and the second piezoelectric layer, the other surface of the repair layer is in contact with the second piezoelectric layer.
5. The piezoelectric stack structure according to claim 1, wherein: The materials of the piezoelectric layer and the repair layer are both scandium-doped aluminum nitride, and the scandium-doped concentration of the repair layer is lower than the scandium-doped concentration of the piezoelectric layer.
6. The piezoelectric stack structure according to claim 1, wherein: The thickness of the repair layer is smaller than the thickness of the piezoelectric layer.
7. The piezoelectric stack structure according to claim 1, wherein: When the number of the repair layers is at least two, at least two repair layers are stacked, and two adjacent repair layers are spaced apart.
8. A piezoelectric stack structure, arranged on a substrate layer, characterized in that: include: At least three electrode layers are stacked, and at least one piezoelectric layer is provided between two adjacent electrode layers; The piezoelectric stack structure also includes at least one repair layer, which is located on the side of the piezoelectric layer closest to the substrate layer away from the substrate layer. The material of the piezoelectric layer is a preset piezoelectric material doped with doping elements, and the material of the repair layer is the preset piezoelectric material not doped with the doping elements.
9. A micro-electromechanical system, characterized in that: The invention comprises a substrate and the piezoelectric stack structure according to any one of claims 1 to 7 or the piezoelectric stack structure according to claim 8 arranged on the substrate.
10. A method for preparing a piezoelectric stack structure, characterized in that: include: A substrate layer is provided, and at least three electrode layers, at least two piezoelectric layers and at least one repair layer are stacked on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, and the repair layer is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer. The repair layer and the piezoelectric layer are made of the same material, and the concentration of the doped element in the material of the repair layer is lower than the concentration of the doped element in the material of the piezoelectric layer.
11. The method for preparing a piezoelectric stack structure according to claim 10, wherein: include: A substrate layer is provided, and a first electrode layer, a first piezoelectric layer, a second electrode layer, a second piezoelectric layer and a third electrode layer are sequentially stacked on the substrate, and a repair layer is formed between the second electrode layer and the first piezoelectric layer, and / or between the second electrode layer and the second piezoelectric layer, wherein the repair layer and the piezoelectric layer are made of the same material, and the concentration of the doping element in the material of the repair layer is lower than the concentration of the doping element in the material of the piezoelectric layer.
12. The method for preparing a piezoelectric stack structure according to claim 10, wherein: include: A substrate layer is provided, and at least three electrode layers, at least two piezoelectric layers and at least two repair layers are stacked on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, the repair layer is located on the side of the electrode layer farthest from the substrate layer facing the substrate layer, two adjacent repair layers are spaced apart, the repair layer and the piezoelectric layer are made of the same material, and the concentration of the doping element in the material of the repair layer is lower than the concentration of the doping element in the material of the piezoelectric layer.
13. A method for preparing a piezoelectric stack structure, characterized in that: include: A substrate layer is provided, and at least three electrode layers, at least two piezoelectric layers and at least one repair layer are stacked on the substrate layer, wherein at least one piezoelectric layer is provided between two adjacent electrode layers, the repair layer is located on the side of the piezoelectric layer closest to the substrate layer facing away from the substrate layer, the material of the piezoelectric layer is a preset piezoelectric material doped with an impurity element, and the material of the repair layer is the preset piezoelectric material without the impurity element being added.
Citation Information
Patent Citations
Aluminum nitride-based thin film structure and preparation method thereof, and semiconductor device and preparation method thereof
CN111740004A
Bulk acoustic wave resonator with stacked piezoelectric layers
CN115987240A
Piezoelectric thin film, piezoelectric material, and fabrication method of piezoelectric thin film and piezoelectric material, and piezoelectric resonator, actuator element, and physical sensor using piezoelectric thin film
US20080296529A1
Piezoelectric element, and resonator using piezoelectric element
US20190280181A1