Ultralow temperature and thermochromic roof and wallboard coatings

By applying a glassy enamel coating impregnated with highly reflective nanoparticles to roofs and wall panels, the problems of poor radiative cooling effect and insufficient durability of existing coatings within the solar sky's atmospheric window are solved, achieving a highly efficient and durable radiative cooling effect suitable for a variety of substrate surfaces.

CN118891236APending Publication Date: 2024-11-01EAGLE EYE RESEARCH INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380022784.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing roof and wall panel coatings have limited radiative cooling effects within solar sky windows and lack durability, failing to effectively meet the radiation absorption and radiative cooling requirements under different temperature environments.

Method used

The glass enamel coating, impregnated with high-reflectivity nanoparticles, provides high reflectivity within the solar sky atmospheric window. Combined with the size distribution and chemical properties of multi-scale nanoparticles, it ensures that the coating maintains high optical emissivity and reflectivity at different temperatures, and enhances durability through a multi-stage firing technique.

Benefits of technology

It achieves efficient radiative cooling within the solar sky atmospheric window, and the coating has a service life of 40 to 50 years, significantly improving durability and adaptability, and is suitable for a variety of substrate surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891236A_ABST
    Figure CN118891236A_ABST
Patent Text Reader

Abstract

The present invention provides a nanoparticle impregnated coating for roofs and wallboards that provides efficient radiant cooling for buildings. The coating may be a vitreous enamel coating. Multi-scale nanoparticles including one or more of titanium dioxide, barium sulfate, zirconium silicate, hexagonal boron nitride, calcium carbonate, zinc sulfide, silicon dioxide, magnesium oxide, yttrium orthoaluminate, calcium oxide, magnesium aluminate, lanthanum aluminate are used to provide one or more of very high optical reflectance and optical emissivity, and spans the entire frequency band of ground solar radiation. These substrate surfaces include metallic roof and wall panel materials such as steel, corrugated iron, cast iron, aluminum, zinc, tin, copper and metal blends, and further include metallic substrates with metallic coatings, or non-metallic roofs of clays, terra cotta, tiles, bricks, fiber cement, concrete and stones such as slate, and blends of these materials.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims one or more inventions disclosed in provisional application No. 63 / 313,860, entitled “ULTRA-COOL AND THERMOCHROMIC ROOF AND SIDING COATINGS,” filed on February 25, 2022. The benefits of the U.S. provisional application under 35 USC §119(e) are hereby claimed, and the aforementioned application is incorporated herein by reference. Background Art

[0003] The present invention relates to roof and siding coatings and, more particularly, to ultra low temperature and thermochromic roof and siding coatings.

[0004] In developed countries, large amounts of electrical energy are used to cool buildings through air conditioning systems. In underdeveloped countries, the lack of cooling in buildings has a significant impact on the health and well-being of a large number of individuals, as well as worker productivity. Passive cooling technologies have been developed to cool buildings without using energy, but developing affordable, efficient, and durable passive cooling technologies remains a major challenge.

[0005] Radiative cooling is a type of passive cooling in which a building cools itself by radiating the solar energy it emits to the sky through its roof and siding. Radiative cooling can allow the passively cooled exterior surfaces of the roof and siding to reach below-ambient air temperatures, even during periods of direct sunlight.

[0006] The solar sky window is the band of solar radiation at a given altitude on Earth. At sea level, most of the solar sky window is in the ultraviolet (UV) range from about 300nm to the infrared (IR) range of about 2,500nm, with most of the solar energy in the IR range. A key challenge is to develop coatings for roofs and sidings of buildings that provide a high degree of radiative cooling across the entire solar sky window from UV to IR at the height of the building. Within the solar sky window, the composition of total solar radiation is 48% in the near IR (NIR) spectrum, 45% in the visible spectral region, and 7% from UV radiation.

[0007] Note that the terms optical emissivity and optical reflectivity used in this application refer to the emissivity and reflectivity across the entire solar sky atmospheric window, not just the visible spectrum. Emissivity is the ratio of the thermal radiation of a surface to the radiation of the absolute back body at the same temperature, which is between 0 and 1, where an emissivity of 0 indicates that the material is a perfect reflector, and an emissivity of 1 indicates a perfect emitter. Solar reflectivity is the ratio between the solar energy reflected by the surface as a whole and the total incident solar energy. The key criteria for radiative cooling coatings are emissivity and solar reflectivity within the terrestrial solar radiation band, as well as the cost, durability and toxicity of the coating.

[0008] Ultra-low temperature radiative cooling coatings should have both very high optical emissivity and very high optical reflectivity across the entire solar sky atmospheric window. Various coatings, such as paints, epoxies, and polyethylene aerogels, have been proposed for ultra-low temperature radiative cooling of roofs and sidings, but their durability is limited.

[0009] Some geographic locations experience significant daily and seasonal variations in solar radiation and ambient temperature. Particularly in the summer and during the day, the location may experience high temperatures due to solar radiation and benefit from radiative cooling from the roof and siding. However, particularly in the winter and during the night, the location may experience low temperatures and benefit from radiative absorption from the roof and siding. Providing roof and siding coatings that have radiative cooling and radiative absorption properties that vary with temperature is a challenge.

[0010] Vitreous enamel (also called porcelain enamel) is a highly durable material. Its advantages include high weather resistance, high wear resistance, high chemical resistance and high mechanical hardness. The thickness of traditional vitreous enamel usually ranges from 0.3 mm to 1.3 mm. Vitreous enamel can be made by fusing a powder (called frit) composed mainly of silica (silicon dioxide) and other materials to a substrate through firing at high temperatures of 730°C and 870°C.

[0011] Typically, the frit is composed of various oxides; these oxides include adhesion oxides, refractory materials, and fluxes. Adhesion oxides such as cobalt oxide (CoO), nickel oxide (NiO), and copper (II) oxide (CuO) provide adhesion to the substrate surface. Refractory materials such as silicon dioxide (SiO2) and aluminum oxide (Al2O3) are acidic glass-forming oxides that provide a body for vitreous enamels; the refractory materials also enhance viscosity and chemical resistance. Fluxes such as boron oxide (B2O3), sodium oxide (Na2O), potassium oxide (K2O), lithium oxide (Li2O), and zinc oxide (ZnO) are alkaline oxides that react with the refractory materials and also reduce the softening temperature of the glass, thereby aiding in the production of the vitreous enamel matrix and enhancing surface hardness. Both refractory materials and fluxes also reduce the coefficient of expansion, thereby reducing cracking.

[0012] All content percentages described herein are relative to weight; the composition percentages of the frit are relative to the total weight of the frit; and the composition percentages of the substrate are relative to the weight of the substrate.

[0013] In practice, the frit composition depends on the substrate surface and whether the enamel is an undercoat or a topcoat on the substrate surface. As described below, for frits free of opacifiers and colored oxides, a variety of acceptable frit compositions are commonly used in practice.

[0014] For the steel plate undercoat, the frit batch material may be 25% feldspar, 35% borax, 20% quartz, 6.5% soda ash, 4% sodium nitre, 7% fluorite, 0.5% cobalt oxide, 0.5% nickel oxide and 1.5% tin oxide. Alternatively, also for the steel plate undercoat, the frit batch material may be 20.4% feldspar, 35.8% borax, 17.7% quartz, 5.3% soda ash, 4.5% sodium nitre, 4.9% fluorite, 6.5% barium carbonate, 2.4% sodium fluorosilicate, 0.5% cobalt oxide, 0.5% nickel oxide and 1.5% tin oxide.

[0015] For steel plate topcoat, the frit batch material may be 27% feldspar, 25% borax, 24% quartz, 4.1% soda ash, 6% sodium nitrate, 4.4% fluorite, 11% cryolite and 6% antimony oxide. Alternatively, also for steel plate topcoat, the frit batch material may be 22.8% feldspar, 23.1% borax, 21.1% quartz, 6.3% soda ash, 3% sodium nitrate, 3.4% fluorite, 10.1% cryolite and 6.8% sodium antimonate, and 3.4% zinc oxide.

[0016] The substrate surface to which the vitreous enamel may be applied may be a metal such as steel, corrugated iron, cast iron, aluminium, zinc, tin, copper and metal blends, and may also be a metal substrate with a metallic paint.

[0017] Steels used for enameling typically contain less than 0.20% carbon, which reduces blistering of the enamel. Special steel substrate surfaces developed as substrates for vitreous enamels include: decarburized enameled steel (for one-stage enamel coatings), interstitial enameled steel (medium low carbon steel, but with higher strength), cold rolled rimmed steel (low carbon steel), and cold rolled rimmed steel (low quality steel resulting in lower quality vitreous enamels).

[0018] Enameled iron is a high quality, nearly pure iron with a very low carbon content, but it requires a two-stage enameling firing. Cast iron has a carbon content of at least 2.06%, and its carbon content is usually between 3.25% and 3.60%, and to facilitate enameling, additional chemicals are usually provided, including carbon, silicon, phosphorus, manganese and sulfur.

[0019] Alternatively, the substrate surface may not be metal, but clay, clay, pottery, stoneware, terracotta, tile, brick, fiber cement, concrete, or a stone such as slate. In these cases, the coating applied to the substrate surface is generally referred to as a ceramic glaze. The composition of a standard ceramic glaze frit may vary greatly; an exemplary frit composition is 24.03% basalt, 14.68% albite, 2.89% sodium carbonate (Na2CO3), 10.26% boric acid, 5.97% ZnO, 4.42% calcium carbonate (CaCO3), 14.43% zirconium (IV) silicate (ZrSiO4), 20.32% opal, 2.80% barium sulfate (BaSO4), 0.96% potassium nitrate (KNO3).

[0020] The production of vitreous enamel can be done in several stages, some of which are optional.

[0021] The substrate surface is first prepared, usually by applying various substances (such as degreasers in the case of metal substrate surfaces), pickling (etching the metal substrate surface to provide anchoring points for the vitreous enamel), pH neutralization, and rinsing. The primer (also called undercoat) may also be pre-fired to further promote adhesion to the substrate.

[0022] After this preparation of the substrate surface, the primer frit can be applied to the substrate surface by a variety of dry and wet techniques, each requiring a specific frit composition. The dry application technique is electrostatic deposition, in which an organosilane that can hold an electrical charge encapsulates the dry frit, allowing electrostatic attachment to the substrate surface. The wet application technique is flow coating, in which a slurry of frit flows over the surface of the substrate surface.

[0023] For dry process cast iron over enamel coating, the frit batch material may be 34.3% feldspar, 19.3% borax, 7.7% soda ash, 2.6% sodium nitre, 7.3% fluorite, 3.4% cryolite, 9.2% zinc oxide, 8.1% red lead, 8.1% tin oxide.

[0024] For wet process cast iron over enamel coating, the frit batch may be 23% feldspar, 24% borax, 12% quartz, 8% sodium nitre, 2% fluorite, 6% cryolite, 10% barium carbonate, 4% sodium fluorosilicate, 6% zinc oxide, 10% boric acid and 8% antimony oxide.

[0025] After the frit is applied to the surface of the substrate, primary firing is performed at a temperature of about 750° C. to 850° C. to fuse the frit to the substrate to form a primary coating.

[0026] The duration and temperature of the undercoat firing depends on the substrate surface. Aluminum enamel is fired at 538°C to 593°C for 10 minutes. Dry process cast iron is fired at 816°C to 927°C for 5 minutes. Wet process cast iron is fired at 732°C to 816°C for 10 minutes to 20 minutes. Iron plate undercoat is fired at 760°C to 871°C for 1 minute to 4 minutes.

[0027] After this primer firing to fuse the frit to the substrate, subsequent firings can be performed using additional frits to assemble a vitreous enamel layer of different composition on the primer coating. For example, after the iron plate primer coating is fired, the iron plate top coating is fired at 816°C to 927°C for 1 minute to 3 minutes. Summary of the invention

[0028] In the present invention, a vitreous enamel coating impregnated with highly reflective nanoparticles is applied to a substrate surface to provide high reflectivity within the solar radiation range within the solar sky atmospheric window. Highly reflective nanoparticles (HRNPs) have a high melting point and reflectivity, allowing them to be fired without significantly changing their reflectivity.

[0029] In one embodiment, the HRNPs include one or more of the following: barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium aluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3).

[0030] The reflectivity of HRNPs depends on the size and chemical properties of the specific nanoparticle mixture. In an embodiment of the present invention, the HRNPs are multi-scale, with a size distribution to provide high reflectivity over the full range of solar radiation. For example, a larger size provides reflectivity of IR, while a smaller size provides reflectivity of UV. The present invention employs a selection of distributions of multiple sizes of HRNPs, wherein the selection of HRNPs and their sizes is optimized to ensure a distribution of high reflectivity over the frequency range of solar radiation.

[0031] In one embodiment of the present invention, the size range of the multi-scale HRNPs is continuous from smallest to largest. In other embodiments of the present invention, the size range of the multi-scale HRNPs is discrete; the mixture of multi-scale HRNPs is formed from two or more batches of HRNPs of uniform size.

[0032] In the present invention, the frit includes multi-scale HRNPs to produce a specialized vitreous enamel. The frit is fired at a temperature below the melting temperature of the HRNPs, thereby retaining high optical emissivity and reflectivity in the resulting HRNP-impregnated vitreous enamel coating. The vitreous enamel coating is highly durable, with a service life of approximately 40 to 50 years, far exceeding the service life of other roof and siding coatings (such as paints, epoxies, and polyethylene aerogels) that can be used for radiative cooling.

[0033] Embodiments of the HRNP-impregnated vitreous enamels of the present invention can be fired on metal substrate surfaces including steel, corrugated iron, cast iron, aluminum, zinc, tin, copper, and metal blends, and also metal substrates with metallic coatings. Embodiments of the HRNP-impregnated vitreous enamels of the present invention can also be fired on non-metal roofing and siding materials such as clay, terracotta, tile, brick, fiber cement, concrete, and stone such as slate, and blends of these materials.

[0034] The vitreous enamel coating includes from 2% to 40% of one or more highly reflective multi-scale nanoparticles, based on the total weight of the vitreous enamel coating, depending on the thickness of the coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Shown is the solar radiation onto the roof with reflection.

[0036] Figure 2 Shown is a cross section of a vitreous enamel comprising multi-scale size-distributed highly reflective nanoparticles.

[0037] Figure 3 A method or flow chart of applying an enamel coating to a substrate surface is shown. DETAILED DESCRIPTION

[0038] The terms used herein are only used for the purpose of describing specific embodiments and are not intended to limit the present invention. As used herein, the singular forms "a", "an", and "the" are intended to include plural forms as well as singular forms, unless the context clearly indicates otherwise. It should be further understood that when used in this specification, the terms "include" and "comprise" specify the presence of stated features, steps, operations, elements, and components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components, and groups thereof.

[0039] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. It should be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and in this disclosure, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such herein.

[0040] When describing the present invention, it should be understood that many techniques and steps are disclosed. Each of these techniques and steps has a separate benefit, and each technique and step can also be used in combination with one or more of other disclosed techniques, or in some cases all. Therefore, for the sake of clarity, this specification will avoid repeating each possible combination of the various steps in an unnecessary manner. However, the specification and claims should be understood as such combinations are fully within the scope of the present invention and claims.

[0041] All content percentages described herein are relative to weight; the composition percentages of the frit are relative to the total weight of the frit; and the composition percentages of the substrate are relative to the weight of the substrate.

[0042] This article discusses new vitreous enamel. In the following description, for the purpose of explanation, many specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to those skilled in the art that the present invention can be practiced without these specific details.

[0043] The present disclosure is to be considered as exemplification of the invention; it is not intended to limit the invention to the specific embodiments illustrated by the following drawings or description.

[0044] Embodiments of the present invention describe novel vitreous enamels containing multi-scale highly reflective nanoparticles. Such vitreous enamels can be fired on many metal substrate surfaces, including steel, corrugated iron, cast iron, aluminum, zinc, tin, copper, and metal blends, and also include metal substrates with metallic coatings. In addition, such vitreous enamels can be fired on many non-metal roofing and siding materials, such as clay, terracotta, tile, brick, fiber cement, concrete, and stone such as slate, and blends of these materials.

[0045] Figure 1 Solar radiation with reflection onto a roof is shown. The roof 1 preferably has a vitreous enamel paint 10 according to an embodiment of the invention. The vitreous enamel paint 10 receives solar radiation 3 from the sun 2. Due to the vitreous enamel paint 10, the solar radiation is reflected 4.

[0046] Embodiments of the present invention employ highly reflective nanoparticles (HRNPs) having a sufficiently high melting point that the reflectivity of the HRNPs is not compromised during the firing associated with applying the vitreous enamel coating to a substrate surface.

[0047] The HRNPs included in the vitreous enamel coating preferably comprise a size distribution of nanoparticles. The size distribution of the nanoparticles used provides high reflectivity over the full range of solar radiation from IR to UV.

[0048] The size of the nanoparticles used in embodiments of the present invention is less than 2000nm. In many cases, the nanoparticles of specific size and composition will have emission and reflection spectra limited to restricted bands. In embodiments of the present invention, single-sized nanoparticles are not used exclusively. The term "multi-scale nanoparticles" used herein refers to nanoparticles with size distribution or the collection of nanoparticles with multiple sizes.

[0049] In one embodiment, the HRNPs include one or more of the following: barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium aluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3).

[0050] The size distribution associated with exemplary HRNPs is shown in Table 1 below. Figure 2 A cross section of a vitreous enamel 10 comprising multi-scale size-distributed highly reflective nanoparticles 5-8 is shown.

[0051]

[0052]

[0053] Table 1

[0054] These materials are not hazardous under the existing OSHA Hazard Communication Standard and have very low toxicity compared to other nanoparticles, such as carbon nanotube nanoparticles.

[0055] In one embodiment, the one or more multi-scale HRNPs have a nanoparticle distribution ranging from 10 nm to 900 nm.

[0056] It should also be noted that multi-scale nanoparticles with a wide particle size distribution can provide a wider optical emission and reflection band spectrum. For example, the barium sulfate (BaSO4) nanoparticle size distribution between 170nm and 530nm provides a phonon resonance at 9μm, which produces very high optical emissivity (about 96%) and optical reflectivity (about 97.6%) in the full band of the solar sky atmospheric window of terrestrial solar radiation. The hexagonal boron nitride (h-BN) nanoparticle size distribution between 140nm and 525nm provides optical emissivity (about 83%) and optical reflectivity (about 97.9%) in the full band of the solar sky atmospheric window of terrestrial solar radiation. The titanium dioxide (TiO2) nanoparticle size distribution between 140nm and 600nm provides optical emissivity (about 92%) and optical reflectivity (about 95%) in the full band of the solar sky atmospheric window of terrestrial solar radiation. Zirconium silicate (ZrSiO4) nanoparticle size distribution between 160 nm and 550 nm provides optical emissivity (approximately 95%) and optical reflectivity (approximately 97%) across the full band of the solar sky atmospheric window of terrestrial solar radiation.

[0057] In some embodiments, a thermochromic material is added. Thermochromic materials exhibit phase changes in optical properties due to changes in temperature. Vanadium dioxide (VO2) is a thermochromic material that is IR transparent at temperatures below 68°C and has a phase change that reflects IR at temperatures at or above 68°C. Vanadium dioxide nanoparticles provide particularly advantageous thermochromic properties. The phase transition temperature of vanadium dioxide can be reduced by doping the material with various materials, including tungsten, magnesium, and molybdenum. For example, 1.9% tungsten can reduce the phase transition temperature to 29°C.

[0058] Figure 3 A method or flow chart of applying an enamel coating to a substrate surface is shown.

[0059] In the first step, a substrate surface is prepared (step 100). The substrate surface can be a metal, such as steel, corrugated iron, cast iron, aluminum, zinc, tin, copper and metal admixtures, and can also be a metal substrate with a metallic coating. Alternatively, the substrate surface can be clay, pottery, ceramics, stoneware, terracotta, ceramic tile, brick, fiber cement, concrete or a stone such as slate instead of a metal. Depending on the substrate surface, various substances (such as a degreasing agent applied in the case of a metal substrate surface), pickling (etching the metal substrate surface to provide an anchor point for the vitreous enamel), pH neutralization and rinsing are applied. The primer (also referred to as a topcoat undercoat) can also be preliminarily fired to further promote adhesion to the substrate.

[0060] Next, determine the thickness of the coating on the substrate surface and whether the coating will be a primer / finish coat, a top coat or a primer (step 102). A top coat is a coating that cannot be applied directly to the substrate surface but needs to be applied to the primer. The primer is the first coating that is applied directly to the substrate surface and promotes the adhesion of subsequent coatings. Some primers do not require additional coatings.

[0061] The type of coating determines the composition of the frit, the temperature of the prime firing, and the temperature and need for any additional firings. In general, the type of coating does not determine whether the frit is applied using a wet or dry technique, although in a wet process clay may be added to the prime frit.

[0062] The thickness of the coating determines the percentage of nanoparticles to be added to the frit in a subsequent step. Traditionally, the thickness of vitreous enamel is 0.3 mm to 1.33 mm, with an average thickness of 0.8 mm. In an embodiment of the present invention, for an enamel coating thickness range of 0.3 mm to 1.33 mm, 5% to 15% of nanoparticles are added to the frit.

[0063] If the thickness of the enamel coating is to be increased, the percentage of nanoparticles of the frit decreases linearly. For example, for a thickness of 1.2 mm, 3.3% to 10% nanoparticles are required.

[0064] If the thickness of the enamel paint is to be reduced, the percentage of nanoparticles of the frit increases linearly. Thus, for a thickness of 0.4 mm, the percentage of nanoparticles required would be 10% to 30%.

[0065] The thicknesses and percentages of multi-scale HRNPs described above may vary beyond the examples given above. In one embodiment, the vitreous enamel coating includes 2% to 40% of one or more highly reflective multi-scale nanoparticles, based on the total weight of the vitreous enamel coating.

[0066] A primer frit comprising multi-scale HRNPs is then prepared (step 104). It should be noted that single-sized nanoparticles are not used exclusively. Nanoparticles with a size distribution preferably in the range of 170 nm to 530 nm are blended into the primer frit. The primer frit is prepared by melting a variety of minerals in a furnace, and then rapidly quenching the molten material to obtain fine particles, which are then dried.

[0067] In one embodiment, the frit is composed of a variety of oxides; these oxides include adhesion oxides, refractory materials, fluxes, opacifiers, pigments, and multi-scale HNRPs. Adhesion oxides such as CoO, NiO, and CuO provide adhesion to the substrate surface. Refractory materials such as SiO2 and Al2O3 are acidic glass-forming oxides that provide a body for vitreous enamels; the refractory materials also enhance viscosity and chemical resistance. Fluxes such as B2O3, Na2O, K2O, Li2O, and ZnO are alkaline oxides that react with refractory materials and also reduce the softening temperature of glass, thereby contributing to the production of vitreous enamel matrices; the fluxes also enhance surface hardness. Both refractory materials and fluxes also reduce the coefficient of expansion, thereby reducing cracks. Opacifiers such as ZIO2, Sb2O3, TiO3, and P2O5 can be added to produce opacity (increased whiteness) and improve acid resistance.

[0068] The multi-scale HNRP added to the frit may include, but is not limited to, blends of barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium orthoaluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3). The total percentage of multi-scale HNRP in the frit composition is between 5% and 30% of the total weight of the vitreous enamel.

[0069] In one embodiment, the multiscale HNRP consists entirely of nanoparticles of one type selected from the group consisting of barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium orthoaluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3).

[0070] In another embodiment, the multi-scale HNRP in the frit is two types of nanoparticles, in relative percentages to optimize the total reflectivity across the solar atmospheric window, wherein the two types of nanoparticles are selected from barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium aluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3).

[0071] In a first example, if the substrate surface is a steel plate and the coating to be applied is a primer with a thickness of 0.8 mm, the frit includes: 25% feldspar, 35% borax, 20% quartz, 6.5% soda ash, 4% sodium nitre, 7% fluorite, 0.5% cobalt oxide, 0.5% nickel oxide, 1.5% tin oxide and 5% to 15% multi-scale HNRP.

[0072] In another example, if the substrate surface is a steel plate and the coating to be applied is a primer, the frit composition includes: 20.4% feldspar, 35.8% borax, 17.7% quartz, 5.3% soda ash, 4.5% sodium nitre, 4.9% fluorite, 6.5% barium carbonate, 2.4% sodium fluorosilicate, 0.5% cobalt oxide, 0.5% nickel oxide, 1.5% tin oxide and 5% to 15% multi-scale HNRP.

[0073] In another example, if the substrate surface is a steel plate and the coating to be applied is a topcoat, the frit composition includes: a topcoat having a thickness of 0.8 mm, the frit including: 22.8% feldspar, 23.1% borax, 21.1% quartz, 6.3% soda ash, 3% sodium nitre, 3.4% fluorite, 10.1% cryolite, 6.8% sodium antimonate and 3.4% zinc oxide, and 5% to 15% multi-scale HNRP.

[0074] The percentages of the components of the frit are examples only, and in practice the frit composition depends on the substrate surface, and also on whether it is an undercoat or a topcoat.

[0075] The primer frit may be applied to the substrate surface using a dry process or a wet process (step 106).

[0076] In the wet process, the primer frit is mixed with water to form an aqueous suspension. Additional floating agents, such as clay, are then added. The primer frit is then applied to the substrate surface by dipping or spraying. The application of the wet frit can be by dip coating, flow coating, spraying, electrostatic wet spraying or electrophoretic coating. For example, in a wet process cast iron overlay enamel coating, the frit batch can be 23% feldspar, 24% borax, 12% quartz, 8% sodium nitre, 2% fluorite, 6% cryolite, 10% barium carbonate, 4% sodium fluorosilicate, 6% zinc oxide, 10% boric acid, 8% antimony oxide and multi-scale HRNP.

[0077] In a dry process, the frit is ground in the absence of water and then applied to the substrate surface, for example, by an electrostatic dry powder process. The frit is enclosed in one or more organic compounds such as organosilanes, so that the particles of the organic compound acquire an electric charge and enclose the dried frit, so that the frit can be "sprayed" on the substrate surface, thereby allowing electrostatic attachment to the substrate surface. For example, in a dry process cast iron overlay enamel coating, the frit batch can be 34.3% feldspar, 19.3% borax, 7.7% soda ash, 2.6% sodium nitre, 7.3% fluorite, 3.4% cryolite, 9.2% zinc oxide, 8.1% red lead, 8.1% tin oxide, and multi-scale HRNPs.

[0078] The substrate surface then undergoes a primer firing (step 108). The duration and temperature of the firing depends on the substrate surface type. Aluminum enamel is fired at 538°C to 593°C for about 10 minutes. Dry process cast iron is fired at 816°C to 927°C for about 5 minutes. Wet process cast iron is fired at 732°C to 816°C for about 10 minutes to 20 minutes. Iron plate primer is fired at 760°C to 871°C for about 1 minute to 4 minutes.

[0079] Optionally, depending on the desired thickness and other properties, an additional firing may be performed after the bottom firing (step 110) at a similar temperature and time.

[0080] A coating is then placed over the enamel covering the substrate surface (step 112). The coating may be one or more of a resin / epoxy coating or a clear coating. Other coatings may also be used.

[0081] After all coating is complete, the substrate surface is cured (step 114) and the method ends. Curing is performed at a temperature of 230°C to 250°C.

[0082] It should be noted that the firing temperature of the frit of the embodiments of the present invention is much lower than the melting temperature of the included nanoparticles. For example, the melting point of barium sulfate is 1,345°C, the melting point of titanium dioxide is 1,855°C, and the melting point of zirconium silicate is 1,540°C, which are much lower than the firing temperature of less than 1000°C. In addition, the melting point of the nanoparticles is higher than that of the enamel coating, and the high reflectivity and emissivity of the nanoparticles are retained in the resulting nanoparticle-impregnated vitreous enamel coating.

[0083] Embodiments of the present invention include multi-scale nanoparticle impregnated vitreous enamel coatings that include a blend of conventional frit materials and frits of multi-scale HRNPs. Additional thermochromic materials may be added, such as vanadium dioxide.

[0084] The HRNP-impregnated vitreous enamel coatings of the present invention can be fired on a variety of substrates, including commonly used roofing and siding materials, including metal materials such as corrugated iron, zinc, tin, steel, copper, or aluminum; and other materials such as clay, terracotta, tile, brick, fiber cement, concrete, or stone such as slate.

[0085] In other embodiments of the invention, various techniques may be employed to improve the properties of the resulting vitreous enamel coating, including the use of high purity silica sand (99.5% to 99.9%) in the primer frit to optimize one or more of optical reflectivity and optical emittance.

[0086] In other embodiments of the invention, the underlying vitreous enamel paint comprising multi-scale nanoparticles has an additional overlying protective coating that is transparent to the solar sky window frequency band of solar radiation as defined in the Background section above.

[0087] It should therefore be understood that the embodiments of the invention described herein are merely illustrative of the application of the principles of the invention. Reference herein to details of the illustrated embodiments is not intended to limit the scope of the claims, which themselves recite those features regarded as essential to the invention.

Claims

1. A coating for application to roof surfaces and siding surfaces to promote radiative cooling, the coating comprising: One or more multi-scale highly reflective nanoparticles, wherein the coating is a vitreous enamel coating and the vitreous enamel coating comprises 2% to 40% of the one or more multi-scale highly reflective nanoparticles based on the total weight of the vitreous enamel coating.

2. The coating of claim 1, wherein one or more of the roof surface and the side surface is a metal material.

3. The coating of claim 2, wherein the metallic material is selected from the group consisting of steel, corrugated iron, cast iron, aluminum, zinc, tin, copper, metal blends, and metallic coatings.

4. The coating of claim 1, wherein one or more of the roof surface and the side surface is a non-metallic material.

5. The coating of claim 4, wherein the non-metallic material is selected from the group consisting of clay, terracotta, tile, brick, fiber cement, concrete, stone, and blends of non-metallic materials.

6. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are barium sulfate (BaSO4).

7. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are hexagonal boron nitride (h-BN).

8. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are zirconium silicate.

9. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are titanium dioxide.

10. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are: barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4) and titanium dioxide (TiO2).

11. The coating according to claim 1, wherein the one or more multi-scale highly reflective nanoparticles are one or more of the following: barium sulfate (BaSO4), hexagonal boron nitride (h-BN), zirconium silicate (ZrSiO4), titanium dioxide (TiO2), calcium carbonate (CaCO3), zinc sulfide (ZnS), silicon dioxide (SiO2), magnesium oxide (MgO), yttrium orthoaluminate (Al5O 12 Y3), calcium oxide (CaO), magnesium aluminate (Al2MgO4) and lanthanum aluminate (LaAlO3).

12. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles of the coating increase reflectivity in the solar radiation range from infrared to ultraviolet.

13. The coating of claim 1, further comprising high purity silica sand, such that the high purity silica sand improves one or more of the emissivity or reflectivity of the coating.

14. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles have a nanoparticle distribution ranging from 10 nm to 900 nm.

15. The coating according to claim 1, wherein the coating is a topcoat undercoat.

16. The coating of claim 1, wherein the vitreous enamel coating has a baking temperature below the melting point of the one or more highly reflective multi-scale nanoparticles.

17. The coating of claim 1, wherein the one or more multi-scale highly reflective nanoparticles are barium sulfate (BaSO4) and hexagonal boron nitride (h-BN).

18. The coating of claim 1, wherein the coating further comprises a thermochromic material of vanadium dioxide (VO2).

19. The coating of claim 1, wherein the coating is a topcoat.

20. The coating according to claim 1, wherein the coating is a primer coating.

21. A method of applying a vitreous enamel coating to a roof and / or siding substrate surface, the method comprising: determining the type of coating to be applied and the thickness of said coating; preparing a primer frit comprising one or more multi-scale highly reflective nanoparticles, wherein the primer frit comprises 2% to 40% of the one or more highly reflective multi-scale nanoparticles based on the total weight of the vitreous enamel coating to be applied; Applying the primer frit to the surface of the substrate using a wet process or a dry process; Firing the substrate surface with the applied primer frit at least once at a temperature below the melting point of the one or more multi-scale highly reflective nanoparticles to apply a first coating to the substrate surface; applying a second coating over the first coating; and The substrate surface having the first coating and the second coating is cured.

22. The method of claim 21, wherein prior to forming the frit, the substrate surface is prepared to receive the first coating.

23. The method of claim 21, wherein the first coating is a primer coating.

24. The method of claim 21, wherein the first coating is a topcoat.

25. The method of claim 21, wherein the second coating is a clear coating.

Citation Information

Cited By

  • Radiation refrigeration coating based on particle size regulation and spectrum complementation as well as preparation method and application of radiation refrigeration coating

    CN122502954A