C1 symmetric 5-OMe-6-alkyl substituted metallocene

By introducing 5-OMe-6-tBu on the C1 symmetric framework to replace the structure and optimize the support material, a new metallocene catalyst was developed, which solved the high production cost and complex process of high molecular weight EP copolymers and high crystalline iPP in the prior art. The problem of this problem has achieved efficient and low-cost catalytic effect and expanded its application potential in the fields of RCP and ICP.

CN118891293APending Publication Date: 2024-11-01EXXONMOBIL CHEMICAL PATENTS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028286.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-07
Filing Date
2023-01-30
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing C1 symmetric catalysts are costly and complex in the production of high molecular weight EP copolymers and high crystalline iPP, making them difficult to meet industrial needs, especially in the fields of RCP and ICP.

Method used

Using a new metallocene catalyst replaced by 5-OMe-6-tBu based on the C1 symmetrical backbone, the activity and molecular weight capacity of the catalyst are improved and the production cost is reduced by simplifying the synthesis process and selecting suitable support materials.

Benefits of technology

The production of EP copolymers and iPP with high activity and high molecular weight is achieved, which reduces production costs, expands the application potential of C1 symmetric catalytic system in the fields of RCP and ICP, and provides efficient impact copolymers and rubber properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005046931520000051
    Figure BDA0005046931520000051
  • Figure BDA0005046931520000071
    Figure BDA0005046931520000071
  • Figure BDA0005046931520000091
    Figure BDA0005046931520000091
Patent Text Reader

Abstract

The 5-OMe-6-tBu substitution of the indenyl fragment of the C1 symmetric catalyst is extremely important for improving the ability to improve the molecular weight of EP. The catalysts described in this document are also capable of producing other ordinary polyolefins, such as iPP, PE, and EO copolymers. The additional ability of high molecular weight EP copolymers can enlarge the potential of C1 symmetric systems in the RCP and ICP fields where this ability is necessary.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of and priority to U.S. Provisional Application No. 63 / 307,477, filed on February 7, 2022, the disclosure of which is incorporated herein by reference.

[0003] field

[0004] Exemplary embodiments described herein relate to polyolefin catalysts and methods of preparing polyolefins by using the catalysts.

[0005] background

[0006] Olefin polymerization catalysts are very useful in industry. There is therefore an interest in finding new catalytic systems (including catalyst activators) that increase the polymerization activity of the catalysts and allow the production of polymers with specific properties (eg high melting point and high molecular weight).

[0007] Catalysts for the polymerization of olefins are often based on metallocenes as catalyst precursors, which are activated either with the aid of aluminoxanes or by activators containing non-coordinating anions.

[0008] The vast majority of patent disclosures using the 4-Ar-5-OMe-6-tBu indene skeleton are based on C2 symmetric metallocene systems. The first example of the 4-Ar-5-OMe-6-tBu indene skeleton was described by Resconi in WO2007 / 116034 in the context of a C2 symmetric catalyst. Subsequently, patent disclosures by Borealis described the use of the 5-OMe-6-tBu indene skeleton in the context of symmetric (same substituted indene) and asymmetric (different indene substitution) metallocene catalysts of C2 symmetry (US2014 / 0221584, US2015 / 0259442, US2016 / 0002369). Relevant disclosures are EP3567061A1, WO2019 / 12110A1, WO2020 / 02349A1, WO2019 / 197383A1, and WO2020 / 157171A1.

[0009] Recent patent activity on C1 symmetric catalysts for PP (WO2020 / 184887, US2019 / 0270833, and KR2019 / 0064338) uses catalysts described in WO2014 / 099303, WO2017 / 069854, and US9266910B2. Other notable patent publications include KR2020 / 00041169, KR2020 / 2250792, KR2020 / 2250794, and WO2020 / 96250A1.

[0010] Other relevant references include U.S. Patent Nos. 5,416,177; 5,817,590; 8,202,958; 8,076,419; 7,531,605; 7,741,417, 6,355,747; 7,851,644; 7,081,543; 6,342,566; 6,960,676; 6,384,142; 6,472,474; U.S. Patent Publication Nos. 2011 / 0172375 and 2010 / 0152388; European Patent Publication Nos. 0 277 004, 0 405 201, 0 798 306, 0 630 910; PCT Publication Nos. WO 1991 / 002012, WO 2001 / 062764, WO 2001 / 068718, WO 2004 / 005360, WO 2001 / 048035, WO 2003 / 035708; MA Giardello et al. (1995) J. Am. Chem. Soc., Vol. 117, pp. 12114-12129; and EA Sanginov et al. (2006) Polymer Science, Series A, Vol. 48(2), pp. 99-106.

[0011] Overview

[0012] The 5-OMe-6-tBu substitution of the indenyl fragment of the C1 symmetric catalyst is extremely important for improving the EP molecular weight capability. The catalysts described in this document are also capable of producing other common polyolefins such as iPP, PE and EO copolymers. The additional capability of high molecular weight EP copolymers can expand the potential of C1 symmetric systems in the RCP and ICP fields where such capability is essential.

[0013] Attached photos

[0014] Figure 1 Here is the X-ray structure of the catalyst that embodies this technological advance.

[0015] Figure 2 The average catalyst activity in propylene polymerization of conventional catalysts and catalysts embodying the present technological advances is illustrated.

[0016] Figure 3A and 3B The average melting point and molecular weight capabilities of polypropylene produced using conventional catalysts and catalysts embodying the present technical advances are illustrated.

[0017] Figure 4A and 4BThe average catalyst activity and molecular weight capabilities of PE / EO copolymers prepared using conventional catalysts and catalysts embodying the present technological advances are illustrated.

[0018] Figure 5A and 5B The average melting point and average octene content of EO copolymers prepared using conventional catalysts and catalysts embodying the present technological advances are illustrated.

[0019] Figure 6 Typical catalyst activities for EP copolymers prepared using conventional catalysts and catalysts embodying the present advances are illustrated.

[0020] Fig. 7A and 7B Representative ethylene incorporation and molecular weight capabilities of EP copolymers of various compositions using conventional catalysts and catalysts embodying the present advances are illustrated.

[0021] Figure 8 Slurry polymerizations in the presence of propylene (iPP) and ethylene propylene mixtures using conventional catalysts and catalysts embodying the present advances are described.

[0022] Fig.9A and 9B The molecular weight capabilities and compositions of EP copolymers prepared in slurry polymerizations using conventional catalysts and catalysts embodying the present advances in the art are illustrated.

[0023] Detailed Description

[0024] For purposes of this application and the claims thereto, the new numbering scheme for the Periodic Table of the Elements as described in Chemical and Engineering News, 63(5), p. 27 (1985) is used. Thus, a "Group 4 metal" is an element from Group 4 of the Periodic Table of the Elements, such as Hf, Ti, or Zr.

[0025] Unless otherwise indicated, "catalyst productivity" is a measure of how many grams of polymer (P) are produced in a period of time T hours using a catalyst (cat) containing W g; and can be represented by the following formula: P / (T×W) and expressed in units of gPgcat-1hr-1. Unless otherwise indicated, "conversion" is the amount of monomer converted to polymer product and is reported in mole % and calculated based on polymer yield and the amount of monomer fed to the reactor. Unless otherwise indicated, "catalyst activity" is a measure of how active the catalyst is and is reported as the mass of product polymer (P) produced per mole of catalyst (cat) used (kgP / molcat).

[0026] "Olefins", or "alkene", are linear, branched or cyclic compounds of carbon and hydrogen with at least one double bond. For the purposes of this specification and the claims thereto, when a polymer or copolymer is referred to as containing an olefin, the olefin present in such a polymer or copolymer is the polymerized form of the olefin. For example, when a copolymer is said to have an "ethylene" content of 35% to 55% by weight, it is understood that the monomer units in the copolymer are derived from ethylene in the polymerization reaction, and based on the weight of the copolymer, the derived units are present at 35% to 55% by weight. A "polymer" has two or more identical or different monomer units. A "homopolymer" is a polymer having the same monomer units. A "copolymer" is a polymer having two or more monomer units that are different from each other. A "terpolymer" is a polymer having three monomer units that are different from each other. "Different" used to refer to a monomer unit indicates that the monomer units are different from each other or isomerically different at least one atom. Therefore, the definition of copolymer used herein includes terpolymers, etc. Oligomers are generally polymers having a low molecular weight (e.g., a number average molecular weight of less than 25,000 g / mol, preferably less than 2,500 g / mol) or a low number of monomer units (e.g., 75 monomer units or less). An "ethylene polymer" or "ethylene copolymer" is a polymer or copolymer comprising at least 50 mole % of ethylene-derived units, a "propylene polymer" or "propylene copolymer" is a polymer or copolymer comprising at least 50 mole % of propylene-derived units, and the like.

[0027] For the purposes of this application, ethylene shall be considered an alpha-olefin.

[0028] For the purposes of this application and its claims, the term "substituted" means that a hydrogen group has been replaced by a heteroatom or a heteroatom-containing group. For example, a "substituted hydrocarbyl" is a group consisting of carbon and hydrogen in which at least one hydrogen is replaced by a heteroatom or a heteroatom-containing group.

[0029] The term "heteroatom" refers to any of the Groups 13-17 elements, excluding carbon. Heteroatoms may include B, Si, Ge, Sn, N, P, As, O, S, Se, Te, F, Cl, Br, and I. The term "heteroatom" may include the above-mentioned elements connected to hydrogen, such as BH, BH2, SiH2, OH, NH, NH2, etc. The term "substituted heteroatom" describes heteroatoms in which one or more of these hydrogen atoms are replaced by a hydrocarbyl or substituted hydrocarbyl group (one or more).

[0030] Unless otherwise indicated (e.g., the definitions of "substituted hydrocarbyl," "substituted aryl," etc.), the term "substituted" means that at least one hydrogen atom has been replaced by at least one non-hydrogen group, such as a hydrocarbyl group, a heteroatom or heteroatom-containing group, such as a halogen (e.g., Br, Cl, F, or I), or at least one functional group (e.g., -NR * 2. -OR * , -SeR * , -TeR * , -PR * 2. -AsR * 2. -SbR * 2. -SR * , -BR * 2. -SiR * 3. -GeR * 3. -SnR * 3. -PbR * 3, wherein q is 1 to 10 and each R* is independently a hydrocarbon group or a halogenated hydrocarbon group, and two or more R * The hydrocarbon groups may be joined together to form a substituted or unsubstituted fully saturated, partially unsaturated or aromatic cyclic or polycyclic ring structure), or wherein at least one heteroatom has been inserted into the hydrocarbon ring.

[0031] The term "substituted hydrocarbyl" means a hydrocarbyl group in which at least one of the hydrogen atoms of the hydrocarbyl group has been replaced by at least one heteroatom (e.g., a halogen, such as Br, Cl, F, or I) or a heteroatom-containing group (e.g., a functional group, such as -NR * 2. -OR * , -SeR * , -TeR * , -PR * 2. -AsR * 2. -SbR * 2. -SR * , -BR * 2. -SiR * 3. -GeR * 3. -SnR * 3. -PbR * 3 alternative, wherein q is 1 to 10 and each R * are independently a hydrocarbon group or a halogenated hydrocarbon group, and two or more R * The term "hydrocarbyl substituted phenyl" means a phenyl group having 1, 2, 3, 4 or 5 hydrogen groups replaced by hydrocarbyl or substituted hydrocarbyl groups. For example, a "hydrocarbyl substituted phenyl" group can be represented by the formula:

[0032]

[0033] Where R a , R b , R c , R d and R e Each of which can be selected from hydrogen, C1-C 40 Hydrocarbon or C1-C 40 Substituted hydrocarbon group, heteroatom or heteroatom-containing group (provided that R a , R b , R c , R d and R e At least one of them is not H), or R a , R b , R c , R d and R e Two or more of these may be joined together to form C4-C 62 Cyclic or polycyclic hydrocarbon ring structures, or combinations thereof.

[0034] As used herein, Mn is the number average molecular weight, Mw is the weight average molecular weight, and Mz is the z average molecular weight, wt% is the weight percent, and mol% is the mole percent. Molecular weight distribution (MWD), also known as polydispersity, is defined as Mw divided by Mn. Unless otherwise indicated, all molecular weight units (e.g., Mw, Mn, Mz) are g / mol.

[0035] The following abbreviations may be used herein: Me is methyl, Et is ethyl, Pr is propyl, cPR is cyclopropyl, nPr is n-propyl, iPr is isopropyl, Bu is butyl, nBu is n-butyl, iBu is isobutyl, sBu is sec-butyl, tBu is tert-butyl, Oct is octyl, Ph is phenyl, Bn is benzyl, MAO is methylaluminoxane, Ind is indenyl, Cp is cyclopentadienyl, Flu is fluorenyl, OTf is triflate, and RT is room temperature (23°C unless otherwise indicated).

[0036] A "catalytic system" is a combination of at least one catalyst compound, at least one activator, an optional co-activator, and an optional support material. For the purposes of this application and the claims thereto, when a catalytic system is described as comprising neutral, stable forms of the components, it is well understood by those of ordinary skill in the art that the ionic forms of the components are the forms that react with the monomers to produce the polymers.

[0037] In the description herein, metallocene catalysts may be described as catalyst precursors, pre-catalyst compounds, metallocene catalyst compounds or transition metal compounds, and these terms are used interchangeably. A polymerization catalyst system is a catalytic system that can polymerize monomers into polymers. An "anionic ligand" is a negatively charged ligand that provides one or more pairs of electrons to a metal ion. A "neutral donor ligand" is a neutrally charged ligand that provides one or more pairs of electrons to a metal ion.

[0038] Metallocene catalysts are defined as organometallic compounds having at least one π-bound cyclopentadienyl moiety (or substituted cyclopentadienyl moiety), and more often two π-bound cyclopentadienyl moieties or substituted cyclopentadienyl moieties.

[0039] For purposes of this application and the claims thereto, the term "substituted" in relation to metallocene catalyst compounds means that a hydrogen group has been replaced by a hydrocarbyl group, a heteroatom or a heteroatom-containing group. For example, methylcyclopentadiene (Cp) is a Cp group substituted by a methyl group, and ethanol is an ethyl group substituted by an -OH group.

[0040] The terms "hydrocarbyl radical", "hydrocarbyl" and "hydrocarbyl group" are used interchangeably throughout this document. Likewise, the terms "group", "radical" and "substituent" are used interchangeably in this document. For the purposes of this disclosure, a "hydrocarbyl radical" is defined as a radical containing hydrogen atoms and up to 100 carbon atoms, and which may be linear, branched or cyclic, and when cyclic, aromatic or non-aromatic. A "substituted hydrocarbyl radical" is a radical consisting of carbon and hydrogen in which at least one hydrogen is replaced by a heteroatom or a heteroatom-containing group.

[0041] The 5-OMe-6-tBu substitution of the indenyl fragment of the C1 symmetric catalyst is extremely important for improving the EP molecular weight capability. The catalysts described in this document are also capable of producing other common polyolefins such as iPP, PE and EO copolymers. The additional capability of high molecular weight EP copolymers can expand the potential of C1 symmetric systems in the RCP and ICP fields where such capability is essential.

[0042] Propylene-ethylene random copolymers and EP rubber impact copolymers are of interest. However, C1 metallocene catalysts generally do not achieve the high molecular weight capabilities of impact-modified phases (e.g., EP rubbers). More generally, metallocene catalysts with high molecular weight capabilities generally involve complex syntheses, as well as challenging racemate / mesomorph separations. Therefore, it is desirable to have a catalyst that is capable of producing both highly crystalline isotactic polypropylene and high molecular weight EP rubber with a cost-effective catalytic system. One such catalyst compound disclosed herein is based on 5-OMe-6-tBu substitution on a C1 symmetric backbone as shown in formula (I) below.

[0043]

[0044] in:

[0045] M is a Group 4 metal, preferably Hf, Ti or Zr;

[0046] X 1 and X 2 Each of X is a monovalent anionic ligand, or X 1 and X 2 joining to form a metal annular ring;

[0047] R 1 -R 4 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl;

[0048] R 5 is hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl;

[0049] R 6 -R 10 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl;

[0050] R 14 and R 15 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl;

[0051] R 12 and R 13 Each is independently unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C10 Alkyl or C6-C 10 Aryl;

[0052] Optionally, R 12 and R 13 can be joined; and

[0053] R 16 Is unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl.

[0054] In addition to providing high crystallinity iPP with minimal regio errors, these catalysts are also able to produce high molecular weight EP copolymers with high activity and excellent ethylene incorporation (up to 50 wt%). In addition, the ability of these catalysts is also demonstrated on EO plastomers in this document. The intended application of these materials may be in the production of random copolymers or impact copolymers with rigid (iPP) or flexible (RCP) matrices. The ability to produce these product compositions will be described in the future.

[0055] Examples of catalysts that embody the advances of this technology are as follows.

[0056]

[0057] In this document, several conventional C1 symmetric catalysts (C1-C6) are used as comparative examples of materials E1-E4 that embody the advances of the present technology.

[0058] Most commercially available metallocene catalysts for propylene are based on C2 symmetric metallocenes. These catalysts are highly active, but they are more expensive to use due to the need for complex ligand synthesis and isomer resolution, which generally results in lower yields. On the other hand, the use of C1 symmetric catalysts is advantageous due to the ease of preparation and overall lower cost. This approach could theoretically close the cost gap between Ziegler–Natta (ZN) and metallocene catalysts. The structures of the catalysts discussed in this document are shown below

[0059]

[0060] The novel catalysts E1-E4 were prepared according to the following synthetic scheme for the preparation of C1 symmetric 5-OMe-6-tBu substituted metallocenes.

[0061]

[0062] Slow evaporation of a dichloromethane solution of catalyst E2 provided X-ray quality crystals. The collected data confirmed the expected ligand attachment. The corresponding X-ray structure is Figure 1 (ellipsoid probability level is 50%).

[0063] Catalysts E1-E3 were evaluated for propylene polymerization using MAO activator under high throughput conditions of MAO activation (500 equiv.). Figure 2 The average catalyst activity in propylene polymerization is shown (conditions: [catalyst] = 30 nmol, [MAO] = 500 eq. Polymerizations were carried out at 70 and 100°C).

[0064] Figure 3A and 3B The average melting point and molecular weight capabilities of polypropylene produced using conventional catalysts and catalysts embodying the present technical advances are illustrated.

[0065] The activity of the catalysts embodying the present technical advances is generally lower compared to comparative catalysts from the same class. However, the observed activities of >100 kg / mmol·h are still considered quite high. In addition, the catalysts embodying the present technical advances provide relatively high iPP crystallinity, and melting points exceeding 150°C and similar Mw capabilities to other catalysts from the same class. The high crystallinity of the iPP is demonstrated by the following Table 1 13 C NMR data confirmed.

[0066] Table 1. iPP produced at 70℃ and 100℃ 13 C NMR results

[0067]

[0068] As shown in Table 1, most catalysts maintain a high level of catalyst stereoselectivity. For example, the 4-tBu series of catalysts (C1, C3 and E1) show a gradual increase in stereoselectivity from simple indene to more substituted 5-OMe-6-tBu indene. As with the previous systems, the choice of substituents on the 4-aryl moiety affects stereoregularity.

[0069] Ethylene and ethylene-octene (EO) copolymerization was carried out under high throughput conditions at a fixed ethylene pressure of 115 psi. Figure 4A and 4BIllustrated are average catalyst activity and molecular weight capabilities for PE / EO copolymers (conditions: [catalyst] = 20 nmol, 115 psi ethylene, 100°C). Figure 5A and 5B State the average melting point and average octene content in EO.

[0070] In most cases the catalysts embodying the present technical advances show slightly reduced activity and comparable Mw capabilities compared to other C1 symmetric catalysts. The octene content remains comparable to the other catalysts.

[0071] Ethylene propylene polymerizations were performed with varying amounts of propylene and balanced ethylene pressures (making the total pressure 140 psi). Based on AVIATO calculations, the ethylene component in the feed ranged from about 0.2-0.8 based on the mole fraction relative to propylene. This type of screening allows for a variety of compositions (semi-crystalline copolymers to pure EP rubber). The results are described below. Catalysts E1-E3 are capable of producing a variety of compositions at high activity (>200 kg / mmol·h). The advantage of using a 5-OMe-6-tBu substitution system over other catalysts used in this document is that the EP Mw capability is significantly improved. This is a major challenge for C1 symmetric catalytic systems, which are typically unable to achieve good Mw capabilities in ethylene copolymers. This energy management can expand the use of C1 symmetric catalytic systems in areas where previous C1 symmetric catalyst classes are generally not feasible. By carefully considering the carrier, this can expand the capabilities of C1 catalysts in specialty copolymer / impact copolymer systems. Preferred supports may include Al2O3, ZrO2, SiO2, SiO2 / Al2O3, SiO2 / TiO2, silica clay, silica / clay, or mixtures thereof. "Careful" consideration of the support influences the type of process for making a particular polymer. For example, if one wishes to make an impact copolymer, they would prefer a more porous support with a high surface area. On the other hand, if one wants to make a simple PP for fibers or molded articles, they would consider a smaller particle size support with a low pore content to help resolve volatiles.

[0072] Figure 6 The activity of representative catalysts on EP copolymers is illustrated (conditions: [catalyst] 20 nmol, 140 psi total pressure, 70°C).

[0073] Fig. 7A and 7B Representative ethylene incorporation and molecular weight capabilities for EP copolymers of various compositions are illustrated.

[0074] The catalysts embodying the present technological advances can also be supported on conventional porous materials (e.g., silica). Details on the supporting methods are described in the experimental section below. These supported catalysts show high activity and improved molecular weight capabilities of EP copolymers.

[0075] Figure 8 The slurry polymerization in the presence of propylene (iPP) and ethylene propylene mixture (EP) is described (condition iPP: 0.6 mg supported catalyst, 5 μmol TIBAL, 4 mL liquid propylene, 1 mL isohexane. Condition EP (250 psi) 0.6 mg supported catalyst, 5 μmol TIBAL, 2 mL liquid propylene, 3 mL isohexane, 70 psi ethylene. Condition EP (185 psi) 0.6 mg supported catalyst, 5 μmol TIBAL, 1 mL liquid propylene, 4 mL isohexane 70 psi ethylene).

[0076] Table 1 Average polydispersity index (PDI) of polymers produced in slurry polymerization using supported catalysts C3, C6, E1 and E4

[0077] catalyst PDI(iPP) PDI(EP 250psi) PDI (EP 185psi) C3 2.48 2.23 2.07 E1 2.05 2.10 1.95 C6 2.25 2.35 2.25 E4 1.98 2.20 2.00

[0078] Fig.9A and 9B The molecular weight capabilities and compositions of EP copolymers prepared in slurry polymerization are described.

[0079] The data shown in Figures 7-9 indicate that supported catalysts E1-E4, which embody the advances of the present technology, exhibit relatively high catalyst activity (>10000 g / mol) for the production of EP copolymers. The main advantage of using such systems is their improved molecular weight capabilities and narrower PDI in EP copolymers, which results in better quality rubbers that provide improved impact properties. Additionally, the narrow polydispersity index (PDI) provided by catalysts E1-E4 is an extremely useful property in the polypropylene fiber process.

[0080] The terms "co-catalyst" and "activator" are used interchangeably herein and are defined as any compound that can activate any of the above catalyst compounds by converting a neutral catalyst compound into a catalytically active catalyst compound cation. Non-limiting activators, for example, include aluminoxanes, alkyl aluminums, ionizing activators (which can be neutral or ionic), and conventional types of co-catalysts. Preferred activators typically include aluminoxane compounds, modified aluminoxane compounds, and ionizing anion precursor compounds that capture reactive, σ-bound metal ligands, making the metal complex cationic and providing a non-coordinating or weakly coordinating anion that balances the charge. Those of ordinary skill in the art will be able to select a suitable activator for use with a catalyst that embodies the present technological advancement. Activators that can be used with the present technological advancement can be found in U.S. Patent No. 9,266,910, which is incorporated herein by reference in its entirety. Preferred activators may include, wherein the activator is an aluminoxane or a non-coordinating (NCA) anion salt.

[0081] The term "non-coordinating anion" (NCA) means an anion that is either not coordinated to a cation or is only weakly coordinated to a cation, thereby remaining sufficiently labile to be displaced by a neutral Lewis base. "Compatible" non-coordinating anions are those that do not degrade to neutrality when the initially formed complex decomposes. Further, the anion does not transfer anionic substituents or fragments to the cation so that it forms a neutral transition metal compound and neutral byproducts from the anion. Useful non-coordinating anions according to the present application are those that are compatible, stabilize the transition metal cation in the sense of balancing its ionic charge with +1, and yet remain sufficiently labile to allow displacement during polymerization.

[0082] The minimum activator to catalyst compound ratio is a 1:1 molar ratio. Alternative preferred ranges include from 1:1 to 500:1, alternatively from 1:1 to 200:1, alternatively from 1:1 to 100:1, or alternatively from 1:1 to 50:1.

[0083] In the embodiments herein, the catalytic system may include an inert carrier material. Preferably, the loaded material is a porous carrier material, for example, talc and an inorganic oxide. Other carrier materials include zeolites, clays, organoclays or any other organic or inorganic carrier materials, etc. or mixtures thereof. One of ordinary skill in the art can select a suitable carrier for use with the catalyst embodying this technological advancement. Carriers that can be used together with this technological advancement can be found in U.S. Patent No. 9,266,910, which is incorporated herein by reference in its entirety. Preferred carriers may include Al2O3, ZrO2, SiO2, SiO2 / Al2O3, SiO2 / TiO2, silica clay, silicon oxide / clay, or mixtures thereof.

[0084] In embodiments herein, the present technology advancement relates to a polymerization process wherein a monomer (e.g., propylene) and optional comonomers are contacted with a catalytic system comprising an activator and at least one metallocene compound as described above. The catalyst compound and activator may be combined in any order and are typically combined prior to contact with the monomer. A polymerization process that may be used with the present technology advancement may be found in U.S. Pat. No. 9,266,910, which is incorporated herein by reference in its entirety.

[0085] The present technology advancement also relates to material compositions produced by the methods described herein. The methods of some embodiments of the present technology advancement produce olefin polymers, preferably polyethylene and polypropylene homopolymers and copolymers. In one embodiment, the polymer produced herein is an ethylene copolymer, preferably having from 0 to 25 mol % (alternatively from 0.5 to 20 mol %, alternatively from 1 to 15 mol %, preferably from 3 to 10 mol %) of C3 to C 20 One or more olefin comonomers (preferably C3 to C 12 α-olefins, preferably propylene, butene, hexene, octene, decene, dodecene, preferably propylene, butene, hexene, octene), or propylene copolymers, preferably having 0 to 25 mol% (alternatively from 0.5 to 20 mol%, alternatively from 1 to 15 mol%, preferably from 3 to 10 mol%) of C2 or C4 to C 20 One or more olefin comonomers (preferably ethylene or C4 to C 12 α-olefins, preferably ethylene, butene, hexene, octene, decene, dodecene, preferably ethylene, butene, hexene, octene).

[0086] Unless otherwise indicated, Mw, Mn, MWD are determined by GPC as described in US 2006 / 0173123, pages 24-25, paragraphs

[0334] to

[0341] .

[0087] In a preferred embodiment of this technological advance, the propylene polymer produced may be isotactic polypropylene, atactic polypropylene, and random, block or impact copolymers.

[0088] A method for preparing an alpha-olefin homopolymer or copolymer, comprising: reacting a C2-C olefin at a reactor pressure of 0.7 bar to 70 bar and a reactor temperature of 20° C. to 150° C. 40 One or more olefin monomers, and a catalytic system comprising a catalyst compound of formula (I), and optionally hydrogen are introduced into a reactor; and an α-olefin homopolymer or copolymer is obtained. 40The comonomers may include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 2-methyl-1-pentene, vinylcyclobutane, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1,5-hexadiene, 1,7-octadiene and 1,9-decadiene, norbornene, vinyl norbornene or ethylidene norbornene. The olefin polymer or copolymer may have an Mw value of 1000 to 1000000 g / mol, such as from 5000 to 500000, such as from 10000 to 250000, as measured by gel permeation chromatography. The olefin homopolymer or copolymer may have an Mw distribution with a polydispersity index of less than 10, more preferably less than 6 and even more preferably less than 3. Propylene homopolymers and copolymers may have a melting point greater than 120°C, more preferably greater than 140°C and even more preferably greater than 150°C. The ethylene-propylene copolymer may have a comonomer content of 0.1-99.9 wt%, such as from 1 to 50 wt%, such as from 2 to 20 wt%, such as from 3 to 10 wt%. The ethylene-linear α-olefin copolymer may have an α-olefin content comonomer content of 0.1-50 wt%, such as from 5 to 40 wt%, such as from 10 to 30 wt%.

[0089] experiment

[0090] Preparation of dimethylsilyl (6-tert-butyl-4-(4-tert-butylphenyl)-5-methoxy-2-methylindenyl) (2,3,4,5-tetramethylcyclopentadienyl) zirconium dichloride (catalyst E1)

[0091] 5-tert-butyl-7-(4-tert-butylphenyl)-6-methoxy-2-methylindene.

[0092] To a sealable flask, add 7-bromo-5-tert-butyl-6-methoxy-2-methylindene (0.791 g, 2.68 mmol), 4-tert-butylphenylboric acid (0.480 g, 2.70 mmol, 1.01 equivalents), potassium carbonate (0.830 g, 6.01 mmol, 2.24 equivalents), bis(dibenzylideneacetone)palladium (0.020 g, 0.035 mmol, 0.013 equivalents), 1,3,5,7-tetramethyl-6-phenyl-2,4,8-trioxa-6-phosphonoadamantane (0.030 g, 0.10 mmol, 0.038 equivalents), and tetrahydrofuran (30 mL). Subsequently, add nitrogen-bubbled water (10 mL). The sealable flask is placed under a nitrogen atmosphere for 30 minutes, and then the flask is sealed. Stir and heat the sealed flask to 75 ° C for 16 hours. The reaction was then cooled to room temperature. The contents of the flask were transferred to a separate flask and then concentrated in vacuo. The residue was distributed between water (50mL) and ether (50mL). The organic phase was separated, and the aqueous phase was further extracted with ether (50mL). The combined ether extracts were washed with saturated potassium carbonate aqueous solution (50mL) and subsequent brine (50mL). The organic extract was dried over anhydrous magnesium sulfate and filtered on a silica pad, and the product was washed through the pad with additional ether (3×50mL). The ether filtrate was concentrated in vacuo to provide a yellow solid. The yellow solid was then dissolved in pentane (50mL) and filtered again on a silica pad, and the product was washed through the pad with additional pentane (3×50mL). The pentane filtrate was concentrated in vacuo to provide a white solid product (0.544g, 58% yield). 1 H NMR (400MHz, C6D6): δ7.47 (d, 2H, J=8.4Hz), 7.41-7.33 (m, 3H), 6.43 (d, 1H, J=2.2Hz), 3.24(s, 3H), 2.98(s, 2H), 1.84(s, 3H), 1.59(s, 9H), 1.28(s, 9H).

[0093] (6-(tert-butyl)-4-(4-(tert-butyl)phenyl)-5-methoxy-2-methyl-1H-inden-1-yl)dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-dien-1-yl)silane

[0094] To a pre-cooled, stirred solution of 5-tert-butyl-7-(4-tert-butylphenyl)-6-methoxy-2-methylindene (0.544 g, 1.56 mmol) in diethyl ether was added n-butyllithium (0.60 mL, 2.74 M in hexane, 1.6 mmol, 1.05 equiv). The reaction was stirred at room temperature for 16 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a white solid lithiate. The lithiate was dissolved in diethyl ether (40 mL). The solution was then added to a stirred solution of tetramethylcyclopentadienyldimethylsilyl trifluoromethanesulfonate (0.425 g, 1.56 mmol, 1 equiv) in diethyl ether. The reaction was stirred at room temperature for 1 hour. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with pentane (3×20 mL) and filtered over Celite. The combined pentane extracts were concentrated under a stream of nitrogen and then concentrated under high vacuum to afford the product as a white foam (0.615 g, 75% yield). 1 HNMR (400MHz, C6D6): δ7.70 (d, 2H, J=8.4Hz), 7.61 (s, 1H), 7.43 (d, 2H, J=8.4Hz), 6.67 (s, 1H), 3.25 (s, 3H), 2.00 (s, 3H), 1.97 (s, 3H), 1.91 (s, 3H), 1.82 (s, 6H), 1.63 (s, 9H), 1.31 (s, 9H), -0.08 (s, 3H), -0.17 (s, 3H).

[0095] 6-(tert-butyl)-4-(4-(tert-butyl)phenyl)-1-(dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-dien-1-yl)silyl)-5-methoxy-2-methyl-1H-indene-1-lithium

[0096] To a stirred solution of (6-(tert-butyl)-4-(4-(tert-butyl)phenyl)-5-methoxy-2-methyl-1H-inden-1-yl)dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-dien-1-yl)silane (0.615 g, 1.17 mmol) in diethyl ether (50 mL) was added n-butyl lithium (0.90 mL, 2.74 M in hexanes, 2.5 mmol, 2.1 equiv). The reaction was stirred at room temperature for 2 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was washed with pentane (10 mL) and filtered on a plastic fritted funnel. The filtered solid was collected and then concentrated under high vacuum to provide the product as a light orange solid (0.366 g, 58% yield). 1HNMR (400MHz, THF-d8): δ7.58 (d, 2H, J=8.4Hz), 7.49 (s, 1H), 7.37 (d, 2H, J=8.4Hz), 5.74 (s, 1H ), 3.11(s, 3H), 2.31(s, 3H), 2.15(s, 6H), 1.93(s, 6H), 1.38(s, 9H), 1.37(s, 9H), 0.60(s, 6H).

[0097] Dimethylsilyl(6-tert-butyl-4-(4-tert-butylphenyl)-5-methoxy-2-methylindenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride (Catalyst E1)

[0098] Zirconium chloride (0.155 g, 0.665 mmol, 0.979 equiv) was added to a stirred solution of 6-(tert-butyl)-4-(4-(tert-butyl)phenyl)-1-(dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-diene-1-hexa-1-yl)silyl)-5-methoxy-2-methyl-1H-indene-1-hexalithium (0.366 g, 0.679 mmol) in diethyl ether (50 mL) and the remaining zirconium chloride was washed into the reaction with toluene (5 mL). The reaction was stirred at room temperature for 15 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with dichloromethane (2×20 mL) and filtered over celite. The combined dichloromethane extracts were concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a viscous orange foam (0.443 g). The foam was stirred in pentane (20 mL) for 1 hour to produce a yellow suspension. The suspension was filtered on a plastic fritted funnel. The filtered solid was collected and concentrated under high vacuum to provide a yellow solid product (0.253 g, 54% yield). 1 H NMR (400MHz, CD2Cl2): δ7.60-7.52(m, 2H), 7.52-7.46(m, 2H), 7.44(s, 1H), 6.62(s, 1H), 3.32(s, 3H), 2.20(s, 3H), 2.05(s, 3H), 1.98(s, 3H), 1.90(s, 3H), 1.89(s, 3H), 1.37(s, 9H), 1.35(s, 9H), 1.19(s, 3H), 1.08(s, 3H).

[0099] Preparation of dimethylsilyl(6-tert-butyl-5-methoxy-2-methyl-4-(o-tolyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride (catalyst E3)

[0100] 5-tert-Butyl-6-methoxy-2-methyl-7-(o-tolyl)-indene

[0101] 7-bromo-5-tert-butyl-6-methoxy-2-methylindene (0.776 g, 2.63 mmol), o-tolylboronic acid (0.357 g, 2.63 mmol, 1 equivalent), potassium carbonate (0.799 g, 5.78 mmol, 2.2 equivalents), bis(dibenzylideneacetone)palladium (0.015 g, 0.026 mmol, 0.01 equivalents), 1,3,5,7-tetramethyl-6-phenyl-2,4,8-trioxa-6-phosphonoadamantane (0.023 g, 0.079 mmol, 0.03 equivalents), and tetrahydrofuran (30 mL) were added to a sealable flask. Subsequently, nitrogen-bubbled water (10 mL) was added. The sealable flask was placed under a nitrogen atmosphere for 30 minutes, and then the flask was sealed. The sealed flask was stirred and heated to 80 ° C for 17 hours. The reaction was then cooled to room temperature. The contents of the flask are transferred to a separate flask and concentrated in vacuo. The residue is distributed between water (50mL) and pentane (100mL). The aqueous layer is discharged, and then the organic layer is washed with saturated potassium carbonate aqueous solution and subsequent brine. The organic extract is dried over anhydrous magnesium sulfate and filtered on a silica pad, and the product is washed through with additional pentane (3×50mL). The pentane filtrate is concentrated in vacuo to provide a white solid product (0.460g, 57% yield, a mixture of two isomers, 0.16:1 ratio). 1 H NMR (400 MHz, C6D6): major isomer δ 7.37 (s, 1H), 7.22-7.05 (m, 4H), 6.43 (q, 1H, J=1.5 Hz), 3.19 (s, 3H), 2.98 (dt, 1H, J=22.7, 1.1 Hz), 2.66 (dt, 1H, J=22.5, 1.3 Hz), 2.17 (s, 3H), 1.83 (d, 3H, J=1.5 Hz), 1.56 (s, 9H).

[0102] Lithium 6-tert-butyl-4-(o-tolyl)-5-methoxy-2-methylindenate

[0103] To a pre-cooled, stirred solution of 5-tert-butyl-6-methoxy-2-methyl-7-(o-tolyl)-indene (0.460 g, 1.50 mmol) in ether (50 mL) was added n-butyl lithium (0.60 mL, 2.74 M in hexane, 1.6 mmol, 1.1 equivalents). The reaction was stirred at room temperature for 16 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was washed with hexane (10 mL) and filtered on a porous funnel of plastic. The filtered solid was collected and concentrated under high vacuum to provide a white solid product (0.469 g, 64% yield). 1H NMR (400MHz, C4D8O): δ7.45-7.39 (m, 1H), 7.24-7.20 (m, 1H), 7.18 (s, 1H), 7.15-7.09 (m, 2H), 5. 70 (d, 1H, J=2.0Hz), 5.25 (d, 1H, J=2.1Hz), 3.16 (s.3H), 2.25 (s, 3H), 2.20 (s, 3H), 1.42 (s, 9H).

[0104] (6-(tert-butyl)-5-methoxy-2-methyl-4-(o-tolyl)-1H-inden-1-yl)dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-dien-1-yl)silane

[0105] To a stirred solution of 6-tert-butyl-5-methoxy-2-methyl-4-(o-tolyl)-indenyl lithium (0.298 g, 0.954 mmol) in diethyl ether (50 mL) was added tetramethylcyclopentadienyldimethylsilyl trifluoromethanesulfonate (0.313 g, 0.954 mmol, 1 eq.). The reaction was stirred at room temperature for 3 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with pentane (3×20 mL) and filtered over cinnamate. The combined pentane extracts were concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a white foam product (0.399 g, 86% yield, two isomers, 1:1.8 isomer ratio). 1 H NMR (400 MHz, C6D6): integrated as combined isomers δ 7.62 / 7.61 (s, 1H), 7.54-7.44 (m, 1H), 7.27-7.17 (m, 3H), 6.36 / 6.31 (s, 1H), 3.62 / 3.54 (s, 1H), 3.24 (br s, 1H), 3.20 / 3.19 (s, 3H), 2.30 / 2.29 (s, 3H), 1.98 / 1.97 (s, 6H), 1.90 (s, 3H), 1.83 (s, 6H), 1.600 / 1.596 (s, 9H), -0.10 / -0.16 (s, 3H), -0.19 / -0.22 (s, 3H).

[0106] Dimethylsilyl(6-tert-butyl-5-methoxy-2-methyl-4-(o-tolyl)-indenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride (Catalyst E3)

[0107] To a stirred solution of (6-(tert-butyl)-5-methoxy-2-methyl-4-(o-tolyl)-1H-inden-1-yl)dimethyl(2,3,4,5-tetramethylcyclopenta-2,4-diene-1-yl)silane (0.399 g, 0.823 mmol) in diethyl ether was added n-butyl lithium (0.61 mL, 2.74 M in hexane, 1.7 mmol, 2 eq.). The reaction was stirred at room temperature for 16 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was washed with pentane (10 mL) and filtered on a plastic porous funnel. The solid was collected and concentrated under high vacuum to provide a pink solid. The pink solid was dissolved in diethyl ether (50 mL), and zirconium chloride (0.192 g, 0.823 mmol, 1 eq.) was added to the solution under stirring, and the remaining zirconium chloride was washed into the reaction with toluene (5 mL). The reaction was stirred at room temperature overnight. The reaction was concentrated under a nitrogen stream and then concentrated under high vacuum. The residue was extracted with dichloromethane (3×20mL) and filtered on Yin's salt. The combined dichloromethane extracts were concentrated under a nitrogen stream and then concentrated under high vacuum. The residue was stirred in pentane (10mL) until a suspension was formed. The resulting suspension was filtered on a porous funnel of plastic. The filtered solid was collected and concentrated under high vacuum to provide a yellow solid product (0.181g, 34% yield, 1:1.7 isomer A and B ratio). 1 H NMR (400 MHz, CD2Cl2): overall integrated isomers δ 7.76-7.70 (m, 1H), 7.46 (s, 1H), 7.44 (s, 1H), 7.36-7.14 (m, 6H), 7.02 (dd, 1H, J = 7.6, 1.5 Hz), 6.47 (s, 1H, calculated for chlorine, isomer B), 6.36 (s, 1H, calculated for Lu, isomer A), 3.34 (s, 3H), 3.31 (s, 3H), 2.57 (s , 3H), 2.20(s, 3H), 2.18(s, 3H), 2.07(s, 3H), 2.044(s, 3H), 2.037(s, 3H), 1.98(s, 6H), 1.95(s, 3H), 1.92(s, 3H), 1.91(s, 3H), 1.90(s, 3H), 1.36(s, 9H), 1.35(s, 9H), 1.19(s, 3H), 1.18(s, 3H), 1.08(s, 3H), 1.07(s, 3H).

[0108] Preparation of dimethylsilyl (4-(o-biphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl) (2,3,4,5-tetramethylcyclopentadienyl) zirconium dichloride (catalyst E2)

[0109] 7-(o-Biphenyl)-5-tert-butyl-6-methoxy-2-methylindene

[0110] 7-bromo-5-tert-butyl-6-methoxy-2-methylindene (0.812g, 2.75mmol), o-biphenylboric acid (0.545g, 2.75mmol, 1 equivalent), potassium carbonate (0.836g, 6.05mmol, 2.2 equivalents), bis(dibenzylideneacetone)palladium (0.016g, 0.028mmol, 0.01 equivalents), 1,3,5,7-tetramethyl-6-phenyl-2,4,8-trioxa-6-phosphonoadamantane (0.024g, 0.083mmol, 0.03 equivalents), and tetrahydrofuran (30mL) are added to a sealable flask. Subsequently, nitrogen-bubbled water (10mL) is added. The sealable flask is placed under a nitrogen atmosphere for 30 minutes, and then the flask is sealed. Stir and heat the sealed flask to 80°C for 65 hours. The reaction is then cooled to room temperature. The contents of the flask are transferred to a separate flask and concentrated in vacuo. The residue is distributed between water (100mL) and ether (100mL). The aqueous layer is discharged, and the ether layer is collected. The aqueous layer is further extracted with ether (2×50mL). The combined ether extracts are washed with saturated potassium carbonate aqueous solution and subsequent brine. The organic extract is dried over anhydrous magnesium sulfate and concentrated in vacuo to provide an orange solid. The solid is dissolved in pentane (50mL) and filtered on a silica pad. The product is further washed through a silica pad with additional pentane (3×50mL) and subsequent ether-pentane mixtures (ether to pentane ratio is 1:5, using a mixture of 3×50mL). The combined filtrate is concentrated in vacuo to provide a pale to yellow solid product (0.964g, 95% yield, 1:20 isomer ratio). 1 H NMR (400 MHz, C6D6): major isomer δ 7.49-7.44 (m, 1H), 7.37-7.32 (m, 1H), 7.28-7.17 (m, 5H), 7.01-6.93 (m, 3H), 6.39 (q, 1H, J=1.6 Hz), 3.15 (s, 3H), 3.14 (d, 1H, J=22.2 Hz), 2.73 (d, 1H, J=22.8 Hz), 1.86-1.84 (m, 3H), 1.32 (s, 9H).

[0111] 7-(o-Biphenyl)-5-tert-butyl-6-methoxy-2-methylindenyl lithium

[0112] To a pre-cooled, stirred solution of 7-(o-biphenyl)-5-tert-butyl-6-methoxy-2-methylindene (0.964 g, 2.62 mmol) in ether (50 mL) was added n-butyl lithium (1.00 mL, 2.74 M in hexane, 2.74 mmol, 1.05 equiv). The reaction was stirred overnight at room temperature. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was washed with hexane (10 mL) and filtered on a porous funnel of plastic. The filtered solid was collected and concentrated under high vacuum to provide a white solid product (0.748 g, 76% yield). 1 H NMR (400MHz, C4D8O): δ7.72-7.65(m, 1H), 7.41-7.37(m, 1H), 7.33-7.27(m, 2H), 7.08(s, 1H), 7.07-7.02(m, 2H), 6.93-6.87 (m, 3H), 5.69 (d, 1H, J=6.0Hz), 5.51 (d, 1H, J=2.1Hz), 3.08 (s, 3H), 2.28 (s, 3H), 1.10 (s, 9H).

[0113] (4-(o-biphenyl)-6-(tert-butyl)-5-methoxy-2-methylindenyl)dimethyl(2,3,4,5-tetramethylcyclopentadienyl)silane

[0114] To a stirred solution of 7-(o-biphenyl)-5-tert-butyl-6-methoxy-2-methylindenyl lithium (0.748 g, 2.00 mmol) in diethyl ether (50 mL) was added tetramethylcyclopentadienyldimethylsilyl trifluoromethanesulfonate (0.656 g, 2.00 mmol, 1 eq.). The reaction was stirred at room temperature for 2 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with pentane (3×20 mL) and filtered over cinnamate. The combined pentane extracts were concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a white foam product (1.07 g, 98% yield). 1H NMR (400 MHz, C6D6): isomers combined, δ 7.68-7.63 (m, 1H), 7.59-7.54 (m, 1H), 7.53-7.46 (m, 4H), 7.32-7.23 (m, 8H), 7.10-6.93 (m, 6H), 6.59 (s, 1H), 6.49 (s, 1H), 3.60 (s, 1H), 3.53 (s, 1H), 3.25-3.17 (m, 5H), 3.11(s, 3H), 2.04(s, 3H), 2.02(s, 6H), 1.95(s, 6H), 1.88(s, 3H), 1.85(s, 3H), 1.84(s, 3H), 1.81(s, 6H), 1.36(s, 9H), 1.32(s, 9H), -0.13(s, 3H), -0.19(s, 3H), -0.21(s, 3H), -0.23(s, 3H).

[0115] Dimethylsilyl(4-(o-biphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl)(2,3,4,5-tetramethylcyclopentadienyl)zirconium dichloride (Catalyst E2)

[0116] To a stirred solution of (4-(o-biphenyl)-6-(tert-butyl)-5-methoxy-2-methylindenyl)dimethyl(2,3,4,5-tetramethylcyclopentadienyl)silane (1.07 g, 1.95 mmol) in diethyl ether (50 mL) was added n-butyl lithium (1.5 mL, 2.74 M in hexanes, 4.1 mmol, 2.1 eq). The reaction was stirred at room temperature for 70 minutes. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a tan solid. The solid was dissolved in diethyl ether (50 mL) and stirred, and zirconium chloride (0.455 g, 1.95 mmol, 1 eq) was added, and the remaining zirconium chloride was washed into the reaction with toluene (5 mL). The reaction was stirred at room temperature for 15 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with dichloromethane (50 mL, then 2×10 mL) and filtered over celite. The methylene chloride extracts combined were concentrated under a nitrogen stream and then concentrated under high vacuum. The residue was stirred in pentane (10 mL). The resulting suspension was filtered on a porous funnel of plastics. The filtered solid was collected and concentrated under high vacuum to provide a yellow solid product (0.962 g, 70% yield). 1H NMR (400MHz, CD2Cl2): δ7.94-7.87 (m, 1H), 7.49-7.40 (m, 3H), 7.31 (s, 1H), 7.09-7.01 (m, 3H), 6.95-6.89 (m, 2H), 6.60 (s, 1H), 3.26(s, 3H), 2.24(s, 3H), 2.06(s, 3H), 1.99(s, 3H), 1.90(s, 3H), 1.83(s, 3H), 1.18(s, 3H), 1.10(s, 3H), 0.99(s, 9H).

[0117] Preparation of dimethylsilyl (4-(3,5-di-tert-butyl-4-methoxyphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl) (2,3,4,5-tetramethylcyclopentadienyl) zirconium dichloride (catalyst E4)

[0118] 5-tert-butyl-7-(3,5-di-tert-butyl-4-methoxyphenyl)-6-methoxy-2-methylindene To a sealable flask were added 7-bromo-5-tert-butyl-6-methoxy-2-methylindene (0.916 g, 3.26 mmol), 3,5-di-tert-butyl-4-methoxyphenylboronic acid (0.870 g, 3.29 mmol, 1 eq), potassium carbonate (1.04 g, 7.50 mmol, 2.3 eq), bis(dibenzylideneacetone)palladium (0.020 g, 0.035 mmol, 0.01 eq), 1,3,5,7-tetramethyl-6-phenyl-2,4,8-trioxa-6-phosphonoadamantane (0.030 g, 0.10 mmol, 0.03 eq), and tetrahydrofuran (30 mL). Subsequently, nitrogen-bubbled water (10 mL) was added. The sealable flask was placed under a nitrogen atmosphere for 30 minutes, and then the flask was sealed. The sealed flask was stirred and heated to 80 ° C for 19 hours. The reaction was then cooled to room temperature. The contents of the flask were transferred to a separate flask and concentrated in a vacuum. The residue was distributed between water (50mL) and ether (50mL). The aqueous layer was discharged, and the ether layer was collected. The aqueous layer was further extracted with ether (50mL). The combined ether extracts were washed with brine (50mL). The organic extract was dried over anhydrous magnesium sulfate and concentrated in a vacuum to provide an orange solid. The solid was dissolved in isohexane (100mL) and filtered on a silica layer. The product was further washed through a silica pad with additional isohexane (2×50mL). The combined filtrate was concentrated in a vacuum to provide a white solid product (1.36g, 96% yield). 1H NMR (400MHz, C6D6): δ7.55 (s, 2H), 7.38 (s, 1H), 6.46 (q, 1H, J=1.5Hz), 3.47 (s, 3 H), 3.25 (s, 3H), 3.14 (s, 2H), 1.85 (d, 3H, J=1.5Hz), 1.60 (s, 9H), 1.49 (s, 18H).

[0119] Lithium 4-(3,5-di-tert-butyl-4-methoxyphenyl)-6-tert-butyl-5-methoxy-2-methylindenate

[0120] To a pre-cooled, stirred solution of 7-(3,5-di-tert-butyl-4-methoxyphenyl)-5-tert-butyl-6-methoxy-2-methylindene (1.36 g, 3.14 mmol) in ether (50 mL) was added n-butyl lithium (1.30 mL, 2.74 M in hexane, 3.56 mmol, 1.1 equiv). The reaction was stirred at room temperature for 30 minutes. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was washed with hexane (20 mL) and filtered on a plastic porous funnel. The filtered solid was collected and concentrated under high vacuum to provide a white solid product (1.30 g, 94% yield). 1 HNMR (400MHz, C4D8O): δ7.69 (s, 2H), 7.15 (s, 1H), 5.72 (dd, 1H, J=2.1, 0.7Hz), 5.65 (d, 1H, J = 2.1Hz), 3.72 (s, 3H), 3.15 (s, 3H), 2.30 (s, 3H), 1.48 (s, 18H), 1.42 (s, 9H).

[0121] (4-(3,5-di-tert-butyl-4-methoxyphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl)dimethyl(2,3,4,5-tetramethylcyclopentadienyl)silane

[0122] To a stirred solution of tetramethylcyclopentadienyldimethylsilyl trifluoromethanesulfonate (0.972g, 2.96mmol, 1 equivalent) in ether (20mL) was added a solution of 4-(3,5-di-tert-butyl-4-methoxyphenyl)-5-tert-butyl-6-methoxy-2-methylindenyl lithium (1.30g, 2.96mmol) in ether (50mL). The reaction was stirred at room temperature for 1 hour. The reaction was concentrated under a nitrogen stream and then concentrated under high vacuum. The residue was extracted with pentane (40mL, then 20mL) and filtered over cinnamate. The combined pentane extracts were concentrated under a nitrogen stream and then concentrated under high vacuum to provide a white foam product (1.79g, 98% yield). 1H NMR (400MHz, C6D6): δ7.77(s, 2H), 7.63(s, 1H), 6.79(s, 1H), 3.62(s, 1H), 3.49(s, 3H), 3.28(s, 3H), 3.21(br s, 1H), 2.03 (s, 3H), 1.98 (s, 3H), 1.90 (s, 3H), 1.82 (s, 6H), 1.64 (s, 9H), 1.54 (s, 18H), -0.08 (s, 3H), -0.18 (s, 3H).

[0123] Dimethylsilyl (4-(3,5-di-tert-butyl-4-methoxyphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl) (2,3,4,5-tetramethylcyclopentadienyl) zirconium dichloride (Catalyst E4)

[0124] To a stirred solution of (4-(3,5-di-tert-butyl-4-methoxyphenyl)-6-tert-butyl-5-methoxy-2-methylindenyl)dimethyl(2,3,4,5-tetramethylcyclopentadienyl)silane (1.79 g, 2.92 mmol) in diethyl ether (50 mL) was added n-butyl lithium (2.2 mL, 2.74 M in hexane, 6.0 mmol, 2.1 eq). The reaction was stirred at room temperature for 67 minutes. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum to provide a foam. The foam was dissolved in diethyl ether (50 mL) and stirred, and zirconium chloride (0.679 g, 2.91 mmol, 1 eq) was added, and the remaining zirconium chloride was washed into the reaction with toluene (5 mL). The reaction was stirred at room temperature for 15 hours. The reaction was concentrated under a stream of nitrogen and then concentrated under high vacuum. The residue was extracted with dichloromethane (50 mL, then 20 mL) and filtered over celite. The methylene chloride extracts combined were concentrated under nitrogen stream and then concentrated under high vacuum. The residue was stirred in hexane (40mL). The yellow suspension produced was filtered on a porous funnel of plastics. The filtered solid was collected and concentrated under high vacuum to provide a yellow solid product (1.589g, 70% yield). 1 HNMR (400MHz, CD2Cl2): δ7.88-7.11 (m, 3H), 6.61 (s, 1H), 3.72 (s, 3H), 3.30 (s, 3H), 2.21 (s, 3H), 2.05 (s, 3H), 1.99 (s, 3H), 1.90 (s, 3H), 1.88 (s, 3H), 1.44 (s, 18H), 1.36 (s, 9H), 1.19 (s, 3H), 1.08 (s, 3H).

[0125] High Throughput Polymerization Conditions: Unless otherwise indicated, propylene homopolymerization and ethylene-propylene copolymerization (if any) were conducted in parallel pressure reactors as generally described in U.S. Pat. Nos. 6,306,658; 6,455,316; 6,489,168; WO 2000 / 009255; and Murphy et al., (2003) J. Am. Chem. Soc., Vol. 125, pp. 4306-4317, each of which is fully incorporated herein by reference for U.S. purposes. Although specific quantities, temperatures, solvents, reactants, reactant ratios, pressures, and other variables may vary from one polymerization run to the next, a typical polymerization conducted in parallel pressure reactors is described below.

[0126] Polypropylene polymerization using metallocene: A pre-weighed glass bottle insert and a disposable stirring paddle are installed to each reaction vessel of the reactor, which contains 48 individual reaction vessels. The reactor is then closed and propylene is introduced into each reaction vessel in the form of a condensed gas liquid (usually 1 mL). Solvent (usually isohexane) is then added to bring the total reaction volume, including subsequent additions, to 5 mL, and the reaction vessels are heated to their set temperature (usually about 50°C to about 110°C). The contents of the container are stirred at 800 rpm. The activator solvent (usually 100-1000 molar equivalents of methylaluminoxane (MAO) in toluene) is injected into the reaction vessel together with 500 microliters of toluene, followed by a toluene solution of the catalyst (usually 0.50 mM in toluene, such as 20-40 nmol of catalyst) and an additional aliquot of toluene (500 microliters).

[0127] The equivalent value is determined based on the molar equivalent relative to the mole number of transition metals in the catalyst complex. The reaction is then allowed to proceed until the reaction takes up a predetermined amount of pressure. At this point, the reaction is quenched by pressurizing the container with compressed air. After the polymerization reaction, the glass bottle insert containing the polymer product and solvent is removed from the pressure chamber and the inert gas glove box, and the Genevac HT-12 centrifuge and Genevac VC3000D vacuum evaporator operating under the elevated temperature and reduced pressure are used to remove the volatile components. The bottle is then weighed to determine the output of the polymer product. The polymer produced is analyzed by fast GPC (see below) to determine the molecular weight, and the polymer produced is analyzed by DSC (see below) to determine the melting point.

[0128] Preparation of silica supported MAO (SMAO)

[0129] In a celstir, 10.0 g of calcined silica (DM-L403, AGC Chemicals) at 200° C. was suspended in approximately 100 mL of dry toluene and cooled to −20° C. in a refrigerator. After approximately 30 minutes of cooling, a 30% solution of MAO (15.8 g in toluene) was slowly added to the stirring silica mixture (10 minutes). The reaction was warmed to room temperature and stirred for 1.5 hours. After 1.5 hours, the temperature was increased to 100° C. and the reaction was stirred for an additional 2.5 hours. The temperature was then reduced to 55° C. and the mixture was then filtered on a frit. The collected SMAO was then washed with 2×50 mL of toluene and 2×50 mL of pentane and dried in a vacuum for 1 hour. Yield: 14.1 g of free-flowing powder, calculated MAO absorption = 7.1 mmol / g.

[0130] General procedure for catalyst loading

[0131] 0.51 g of SMAO was suspended in 10 mL of toluene. While stirring, TIBAL (0.260 mL of 1 M) solution was added. The mixture was further stirred at room temperature for 15 minutes. After 15 minutes, 8.2 μmol of the desired metallocene was slowly added in the form of a toluene solution (in approximately 1-2 mL of toluene). The mixture turned green and slowly turned dark red. Each mixture was stirred at room temperature for 2.5 hours. After 2.5 hours, the mixture was filtered, the supported catalyst was washed with toluene (2×5 mL) and pentane (2×5 mL) and dried in vacuo to provide the supported metallocene as a dark orange / red powder.

[0132] Test Method

[0133] 13 C-NMR spectroscopy

[0134] The polymer microstructure was determined by 13C-NMR spectroscopy, including the concentrations of isotactic and syndiotactic diads ([m] and [r]), trinitrogen atoms ([mm] and [rr]) and pentads ([mmmm] and [rrrr]). The sample was dissolved in d2-1,1,2,2-tetrachloroethane. The spectra were recorded at 125°C using a 75 or 100 MHz NMR spectrometer. The polymer resonance peaks were referenced to mmmm = 21.8 ppm. The calculations included in the characterization of polymers by NMR followed the work of FA Bovey in "Polymer Conformation and Configuration" Academic Press, New York 1969 and J. Randall in "Polymer Sequence Determination, 13C-NMR Method", Academic Press, New York, 1977. The percentage of methylene sequences of length 2, %(CH2)2, is calculated as follows: the integral of the methyl carbons between 14-18 ppm (whose concentration is equal to the number of methylenes in a sequence of length 2) divided by the sum of the integral of the methylene sequence of length 1 between 45-49 ppm and the integral of the methyl carbons between 14-18 ppm, multiplied by 100. Since methylene sequences greater than 2 have been excluded, this is the minimum calculated value for methylene groups contained in sequences of 2 or more. Attributes are based on HN Cheong and JA Ewen, Makromol. Chem. 1989, 190, 1931.

[0135] Fast GPC Procedure

[0136] To determine molecular weight related values ​​by GPC, high temperature size 5 exclusion chromatography was performed using an automated "fast GPC" system as generally described in U.S. Pat. Nos. 6,491,816; 6,491,823; 6,475,391; 6,461,515; 6,436,292; 6,406,632; 6,175,409; 6,454,947; 6,260,407 and 6,294,388 (each of which is fully incorporated herein by reference for U.S. purposes). The apparatus had a series of three 30 cm x 7.5 mm linear columns, each containing PLgel 10 μm, Mix B. The GPC system was calibrated using polystyrene standards ranging from 580-3390000 g / mol. The system was operated at an eluent rate of 2.0 mL / min and an oven temperature of 165°C. 1,2,4-trichlorobenzene was used as the eluent. The polymer sample was dissolved in 1,2,4-trichlorobenzene at a concentration of 0.1-0.9 mg / mL. 250 uL of the polymer solution was injected into the system. The concentration of the polymer in the eluent was monitored using an evaporative light scattering detector (as shown in the examples in Table 3) or a Polymer Char IR-4 detector. The molecular weights given are relative to linear polystyrene standards and are not corrected.

[0137] DSC Procedure

[0138] For high throughput samples, melting points (T) were measured using differential scanning calorimetry (DSC) using commercially available equipment such as the TA Instruments TA-Q200 DSC. m ). Typically, 5 to 10 mg of the molded polymer or plasticized polymer is sealed in an aluminum pan at about room temperature and loaded into the instrument. The sample is pre-annealed at about 220°C for about 15 minutes and then allowed to cool to about room temperature overnight. The sample is then heated to about 220°C at a heating rate of about 100°C / min, maintained at that temperature for at least about 5 minutes, and then cooled at a rate of about 50°C / min to a temperature that is typically at least about 50°C below the crystallization temperature. Melting points are collected during the heating period.

[0139] All documents described herein are incorporated herein by reference, including any priority documents and / or testing procedures, as long as they are not inconsistent with this text, but provided that any priority documents not specified in the application originally filed or the archived documents are not incorporated herein by reference. It will be apparent from the foregoing general description and specific embodiments that, although the form of the present technological advancement has been illustrated and described, various modifications can be made without departing from the spirit and scope of the invention. Therefore, it is not intended to limit the invention thereby. Similarly, for the purposes of Australian law, the term "comprising" is considered to be synonymous with the term "including". Similarly, whenever a composition, element or group of elements is preceded by the transition phrase "comprising", it is understood that we also consider the same composition or group of elements preceded by the transition phrase "essentially consisting of...", "consisting of...", "selected from the group consisting of..." or "is" in the recording of the composition, one or more elements, and vice versa.

[0140] Upper numerical limits and lower numerical limits have been used to describe certain embodiments and features. It should be understood that ranges including combinations of any two values, for example, combinations of any lower limit value with any upper limit value, combinations of any two lower limits, and / or combinations of any two upper limits are contemplated, unless otherwise indicated. Certain lower limits, upper limits, and ranges may appear in one or more claims below. All numerical values ​​are "approximately" or "approximately" indicated values, and experimental errors and variations that would be expected by a person of ordinary skill in the art are taken into account. Any value in the table may provide endpoints defining the range of its respective measurement or performance, with an additional + / - 10%.

[0141] All documents described herein are incorporated herein by reference, including any priority documents and / or test procedures, as long as they are not inconsistent with this text. It is apparent from the foregoing general description and specific embodiments that, although the form of the present disclosure has been illustrated and described, various modifications can be made without departing from the essence and scope of the present disclosure. Therefore, it is not intended to limit the present disclosure thereby.

[0142] While the disclosure has been described with respect to certain embodiments and examples, those skilled in the art, having benefit of this disclosure, will appreciate that other embodiments can be devised which do not depart from the scope and spirit of the disclosure.

Claims

1. A catalyst compound represented by formula (I): in, M is a Group 4 metal, preferably Hf, Ti, or Zr; X 1 and X 2 Each is a monovalent anionic ligand, or X 1 and X 2 joining to form a metal annular ring; R 1 -R 4 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl; R 5 is hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl; R 6 -R 10 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl; R 14 and R 15 are independently hydrogen, unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl; R 12 and R 13 Each is independently unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -NR'2, -SR', -OR, -SiR'3, -OSiR'3, -PR'2 or -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl; Optionally, R 12 and R 13 can be joined; and R 16 Is unsubstituted C1-C 40 Hydrocarbon, C1-C 40 Substituted hydrocarbon, unsubstituted C4-C 62 Aryl, substituted C4-C 62 Aryl, unsubstituted C4-C 62 Heteroaryl, substituted C4-C 62 heteroaryl, -R"-SiR'3, wherein R" is C1-C 10 alkyl and each R' is independently hydrogen, halogen, C1-C 10 Alkyl or C6-C 10 Aryl.

2. The catalyst compound according to claim 1, wherein the catalyst compound comprises one or more of the following:

3. A catalytic system comprising: the catalyst compound according to claim 1 or 2; and an activator.

4. The catalytic system of claim 3, wherein the activator comprises methylaluminoxane.

5. A method for preparing isotactic polypropylene, comprising contacting propylene with the catalyst system according to claim 3 and obtaining isotactic polypropylene.

6. A method for preparing a copolymer, comprising contacting ethylene and ethylene-octene with the catalyst system according to claim 3 and obtaining a polyethylene / ethylene-octene copolymer.

7. A method for preparing a copolymer, comprising contacting ethylene and propylene with the catalyst system according to claim 3 and obtaining an ethylene-propylene copolymer.

8. A process for preparing an alpha-olefin homopolymer or copolymer by: At a reactor pressure of 0.7 bar to 70 bar and a reactor temperature of 20° C. to 150° C., C2-C 40 One or more of olefin monomers, and the catalytic system according to claim 3, and optionally hydrogen are introduced into the reactor; and An α-olefin homopolymer or copolymer is obtained.

9. The method according to claim 8, wherein the C2-C 40The comonomers consist of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 2-methyl-1-pentene, vinylcyclobutane, 1-heptene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1,5-hexadiene, 1,7-octadiene and 1,9-decadiene, norbornene, vinyl norbornene or ethylidene norbornene.

10. A process according to any one of claims 8 or 9, wherein the olefin polymer or copolymer has a Mw value of 1000 to 1000000 g / mol, such as 5000 to 500000, such as 10000 to 250000, as measured by gel permeation chromatography.

11. The process according to any one of claims 8 to 9, wherein the olefin homopolymer or copolymer has a Mw distribution with a polydispersity index of less than 10, more preferably less than 6 and even more preferably less than 3.

12. The process according to any one of claims 8 to 11, wherein the olefin monomer is propylene.

13. The process according to any one of claims 8 to 11, wherein the propylene homopolymer and copolymer has a melting point of above 120°C, more preferably above 140°C and even more preferably above 150°C.

14. A process according to any one of claims 8 to 11, wherein the copolymer is an ethylene-propylene copolymer having a comonomer content of 0.1 to 99.9 wt%, such as 1 to 50 wt%, such as 2 to 20 wt%, such as 3 to 10 wt%.

15. The process according to any one of claims 8 to 11, wherein the copolymer is an ethylene-linear alpha-olefin copolymer having a linear alpha-olefin content comonomer content of 0.1 to 50 wt%, such as 5 to 40 wt%, such as 10 to 30 wt%.