Polyvinyl alcohol film, and polarizing film and polarizing plate using same
By controlling the crystallinity and dissolution residual crystallinity of the polyvinyl alcohol-based film, combined with the adjustment of the casting mold and drying conditions, the tensile and dissolution amount of the polyvinyl alcohol-based film in the manufacture of the polarizing film is solved, and high polarization is achieved Polarized film with performance and high yield.
Patent Information
- Application Number
- CN202380020006.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-22
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to simultaneously improve the tensile properties of the polarizing films and reduce the amount of resin dissolution when the polyvinyl alcohol-based film is produced, resulting in poor polarization performance and yield of the polarizing film.
By controlling the crystallinity of the polyvinyl alcohol-based film and the dissolved residual crystallization rate after immersion for 30 seconds within a specific range, combining the adjustment of the casting mold temperature and moisture evaporation rate, the drying state and stretching conditions of the film are controlled, and a high tension is prepared. Films with elongation and low dissolution amounts.
High tensile properties and low fracture rates when manufacturing polarized films are achieved, the amount of resin dissolution is reduced, the polarization performance and yield are improved, and equipment pollution is avoided.
Smart Images

Figure BDA0004975477340000151 
Figure BDA0004975477340000181
Abstract
Description
Technical Field
[0001] The present invention relates to a polyvinyl alcohol film, and more particularly to a polyvinyl alcohol film that can be manufactured with a high yield, has the effect of reducing the tension during stretching when manufacturing a polarizing film, suppresses the elution of impurities from the polyvinyl alcohol film, and a manufacturing method, as well as a polarizing film using the polyvinyl alcohol film. Background Art
[0002] Polyvinyl alcohol-based films have been used in various applications as films with excellent transparency, and one of the useful applications thereof is polarizing films. The polarizing films are used as basic components of liquid crystal displays, and in recent years, their application to devices requiring high quality and high reliability has been expanded.
[0003] Among these, as the screens of liquid crystal televisions, multifunctional portable terminals, etc., become higher in brightness, higher in definition, larger in area, and thinner, a polarizing film having further excellent optical properties and further reduced stretching force is required.
[0004] Generally, polyvinyl alcohol film is produced by continuous casting of aqueous solution of polyvinyl alcohol resin. Specifically, the aqueous solution of polyvinyl alcohol resin is cast on a casting mold such as a casting drum or an endless belt, and the obtained film is peeled off from the casting mold, and then transported along the flow direction (MD direction) by a roller or the like, and dried by a hot roller or a floating dryer, thereby producing the film. In the above-mentioned transporting process, the film is stretched along the flow direction (MD direction), so that the polyvinyl alcohol polymer is easily oriented along the MD direction.
[0005] On the other hand, generally, a polarizing film is produced by swelling a polyvinyl alcohol-based film as a raw material in water (including hot water), dyeing the film with a dichroic dye such as iodine, and stretching the film.
[0006] It is important to rapidly swell the polyvinyl alcohol film in the swelling step and to uniformly swell the polyvinyl alcohol film in the dyeing step so that the dye can smoothly penetrate into the film.
[0007] In addition, the above-mentioned stretching process is a process of stretching the dyed film along the flow direction (MD direction) to highly orient the dichroic dye in the film, but in order to improve the polarization performance of the polarizing film, it is important that the polyvinyl alcohol-based film that becomes the blank shows good stretchability in the flow direction (MD direction) during the stretching process.
[0008] In addition, in the swelling process of the above-mentioned manufacturing process of the polarizing film, when impurities are dissolved from the polyvinyl alcohol film and contaminate the swelling tank, the contamination becomes diffused to the entire subsequent process. In the dyeing process and the boric acid crosslinking process, when impurities are also dissolved from the polyvinyl alcohol film, not only the polarization performance of the obtained polarizing film is reduced, but also the filtration and replacement of the chemical solution used in each process requires huge labor. As the above-mentioned impurities, low molecular weight polyvinyl alcohol resins (including oligomers) present in the polyvinyl alcohol film can be cited, especially low molecular weight bodies with a molecular weight of less than 50,000 are easily dissolved into water, and there is a tendency to easily form low molecular weight iodine complexes that reduce the degree of polarization.
[0009] As methods for improving stretchability, for example, there have been proposed: a method of controlling the speed of the casting drum and the final winding speed (for example, see Patent Document 1); and a polyvinyl alcohol film in which the values of the birefringence in the length direction and the width direction averaged along the thickness direction of the polyvinyl alcohol film satisfy a specific relationship (for example, see Patent Document 2).
[0010] In addition, as a method for improving the contamination caused by the elution from the polyvinyl alcohol film in the swelling process, for example, a polyvinyl alcohol film is proposed, characterized in that the elution amount of the polyvinyl alcohol resin when immersed in water at 50° C. for 1 minute is 900 ppm / m 2 The curling angle in the short-side direction measured under specific conditions is 135° or less (see, for example, Patent Document 3).
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2001-315141
[0014] Patent Document 2: International Publication No. 2012 / 132984
[0015] Patent Document 3: International Publication No. 2017 / 204271 Summary of the invention
[0016] Problem that the invention aims to solve
[0017] However, the current situation is that even if the method of the above patent document is used, it is still impossible to achieve a technology that can simultaneously control the improvement of stretchability and the elution amount of the polyvinyl alcohol-based resin when producing a polarizing film.
[0018] Specifically, the above-mentioned Patent Document 1 specifies the degree of stretching (stretching condition) in the MD direction when manufacturing a polyvinyl alcohol film, but does not disclose the stretchability of the polyvinyl alcohol film when manufacturing a polarizing film. In addition, the polyvinyl alcohol film stretched in the flow direction (MD direction) with a ratio of the casting drum speed to the final winding speed greater than 1 tends to have reduced stretchability when manufacturing a polarizing film. On the other hand, when the ratio of the casting drum speed to the final winding speed is lowered than 0.9, there is a tendency for the transportation (manufacturing) stability to deteriorate due to the influence of wrinkles and slack.
[0019] The technology disclosed in Patent Document 2 can achieve high stretchability, but there is room for improvement in reducing the elution of the polyvinyl alcohol-based resin in the swelling step.
[0020] The technology disclosed in Patent Document 3 can obtain a polyvinyl alcohol-based film with a small amount of elution, but there is room for improvement in stretchability for obtaining a polarizing film that is required to have a high degree of polarization in recent years.
[0021] Therefore, in this context, the present invention provides: a polyvinyl alcohol film that has excellent stretchability during the manufacture of a polarizing film, can suppress breakage, can obtain a polarizing film with high polarization performance, can reduce the amount of polyvinyl alcohol resin eluted when immersed in water, and does not contaminate polarizing film manufacturing equipment; and a polarizing film using the polyvinyl alcohol film; and a polarizing plate.
[0022] Solutions for solving problems
[0023] Therefore, in view of the above-mentioned matters, the inventors of the present invention have repeatedly conducted in-depth research and found that by controlling both the crystallinity of the polyvinyl alcohol film and the dissolved residual crystallinity rate after immersion in water for 30 seconds within a specific range, the dissolution amount of the polyvinyl alcohol resin during the manufacture of the polarizing film can be reduced, and a polarizing film with less breakage and high polarizing performance can be obtained.
[0024] That is, the present invention provides the following [1] to [4]. [1]
[0026] A polyvinyl alcohol film having a crystallinity of 38% or more and a dissolved residual crystal ratio of 18% or less after immersion in water for 30 seconds. [2]
[0028] The polyvinyl alcohol film according to [1], wherein the polyvinyl alcohol film has a thickness of 10 to 70 μm. [3]
[0030] A polarizing film obtained by using the polyvinyl alcohol-based film described in [1] or [2]. [4]
[0032] A polarizing plate comprising: the polarizing film described in [3]; and a protective film provided on at least one surface of the polarizing film.
[0033] Effects of the Invention
[0034] The polyvinyl alcohol film of the present invention is a film that has good stretchability and is not easy to break when manufacturing a polarizing film. Therefore, it can be highly stretched to obtain a polarizing film with high polarization performance. The dissolution and precipitation of the polyvinyl alcohol resin when manufacturing the polarizing film can be suppressed. Therefore, the contamination of the polarizing film manufacturing equipment can be suppressed, and the film can be manufactured with a high yield. DETAILED DESCRIPTION
[0035] Hereinafter, although the form for implementing this invention is demonstrated concretely, this invention is not limited to these.
[0036] It should be noted that, when expressed as "X to Y" (X and Y are arbitrary numbers) in the present invention, unless otherwise specified, it also includes the meaning of "X or more and Y or less", and the meaning of "preferably greater than X" or "preferably less than Y".
[0037] Furthermore, when expressed as "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number), it also includes the meaning of "preferably greater than X" or "preferably less than Y".
[0038] The polyvinyl alcohol film of the present invention has a crystallinity of 38% or more, and a dissolved residual crystal ratio of 18% or less after immersion in water for 30 seconds.
[0039] The crystallinity of the polyvinyl alcohol film of the present invention must be 38% or more, preferably 40% or more, and particularly preferably 42% or more.
[0040] The upper limit of the crystallinity is usually 50% or less, preferably 47% or less.
[0041] When the crystallinity is 38% or more, the elution of low molecules is reduced, the contamination of polarizing film manufacturing equipment is suppressed, and the polarizing film can be made into a polyvinyl alcohol-based film with fewer defective pixels.
[0042] In other words, if the crystallinity is lower than the above lower limit, the elution of low molecules increases, which contaminates the polarizing film production equipment, increases the number of defective spots in the polarizing film, and does not produce the effects of the present invention.
[0043] The dissolved residual crystal ratio of the polyvinyl alcohol film of the present invention after immersion in water for 30 seconds must be 18% or less, preferably 17% or less, particularly preferably 16% or less, and further preferably 15% or less.
[0044] The lower limit is usually 5% or more, preferably 8% or more, and more preferably 10% or more.
[0045] When the dissolved residual crystal ratio after immersion in water for 30 seconds is 18% or less, even when high stretching is performed during the production of the polarizing film, less breakage occurs due to reduced tension, thereby achieving a polyvinyl alcohol-based film with excellent polarizing performance.
[0046] In other words, if the dissolved residual crystal ratio after immersion in water for 30 seconds exceeds the above upper limit, the effect of the present invention will not be exhibited.
[0047] As methods for controlling the above-mentioned crystallinity and the dissolved residual crystallinity after immersion in water for 30 seconds within a specified range, for example, the following methods can be cited: a method for adjusting the molecular weight and saponification degree of the polyvinyl alcohol-based resin used as a raw material; a method for introducing a trace amount of modified groups into the polyvinyl alcohol-based resin; a method for washing the polyvinyl alcohol-based resin to improve the purity; a method for controlling the crystallinity and orientation state of the polymer in the process of forming a film from an aqueous solution of the polyvinyl alcohol-based resin; a method for controlling the dry state of the film during and after film formation; etc., but in the present invention, the method of controlling the dry state of the film during and after film formation is preferred. In terms of facilitating the adjustment of the crystallinity and the dissolved residual crystallinity after immersion in water for 30 seconds, the method of adjusting the temperature on the casting mold, the evaporation rate of water, etc. is particularly preferred.
[0048] Generally, for polyvinyl alcohol-based films, it is preferred to increase the crystallinity in order to improve optical properties and reduce the amount of dissolution during production. However, if the crystallinity is increased, a block of a single crystal is likely to become larger, so that when immersed in water, the crystal structure becomes difficult to collapse, and there is a tendency for the stretchability during production to deteriorate. In contrast, the polyvinyl alcohol-based film defined in the present invention controls the blocks of individual crystals so that they do not become larger, and controls the overall crystallinity to a high level, so that it is highly crystalline, and can also achieve improved stretchability during production and reduced dissolution.
[0049] Hereinafter, the method for producing the polyvinyl alcohol film of the present invention will be described in more detail step by step, but the polyvinyl alcohol film of the present invention is not limited to these embodiments.
[0050] The polyvinyl alcohol film of the present invention is preferably produced through the following steps (A) to (C), and preferably further through the step (D) as necessary.
[0051] Step (A) A step of preparing an aqueous solution of a polyvinyl alcohol-based resin.
[0052] Step (B) A step of casting an aqueous solution of a polyvinyl alcohol-based resin on a casting mold to form a film.
[0053] Step (C) A step of heating and drying the formed film by bringing it into contact with a plurality of hot rolls.
[0054] Step (D): a step of heat-treating the obtained thin film with hot air.
[0055] <Process (A)>
[0056] The step (A) is a step of preparing an aqueous solution of a polyvinyl alcohol-based resin.
[0057] First, the polyvinyl alcohol-based resin and the polyvinyl alcohol-based resin aqueous solution, which are materials of the polyvinyl alcohol-based film, will be described.
[0058] In the present invention, as the polyvinyl alcohol resin constituting the polyvinyl alcohol film, an unmodified polyvinyl alcohol resin, that is, a resin produced by saponifying polyvinyl acetate obtained by polymerizing vinyl acetate. If necessary, a resin obtained by saponifying a copolymer of vinyl acetate and a small amount (usually less than 10 mol %, preferably less than 5 mol %) of a component copolymerizable with vinyl acetate may be used. As components copolymerizable with vinyl acetate, for example, unsaturated carboxylic acids (such as salts, esters, amides, nitriles, etc.), olefins having 2 to 30 carbon atoms (such as ethylene, propylene, n-butene, isobutylene, etc.), vinyl ethers, unsaturated sulfonates, etc. may be cited. In addition, a modified polyvinyl alcohol resin obtained by chemically modifying the hydroxyl group after saponification may also be used. These may be used alone or in combination of two or more.
[0059] In addition, as the polyvinyl alcohol-based resin, a polyvinyl alcohol-based resin having a 1,2-diol structure in the side chain can also be used. The polyvinyl alcohol-based resin having a 1,2-diol structure in the side chain can be obtained, for example, by the following methods: method (i), saponifying a copolymer of vinyl acetate and 3,4-diacetoxy-1-butene; method (ii), saponifying and decarboxylating a copolymer of vinyl acetate and vinyl ethylene carbonate; method (iii), saponifying and deketalizing a copolymer of vinyl acetate and 2,2-dialkyl-4-vinyl-1,3-dioxolane; method (iv), saponifying a copolymer of vinyl acetate and glycerol monoallyl ether.
[0060] The weight average molecular weight of the polyvinyl alcohol resin is preferably 100,000 to 300,000, particularly preferably 110,000 to 280,000, and further preferably 120,000 to 260,000. If the weight average molecular weight is too small, it is difficult to obtain sufficient optical properties when the polyvinyl alcohol resin is formed into an optical film. If the weight average molecular weight is too large, it is difficult to stretch the polarizing film using the polyvinyl alcohol film. It should be noted that the weight average molecular weight of the polyvinyl alcohol resin is a weight average molecular weight measured according to the GPC-MALS method.
[0061] The average saponification degree of the polyvinyl alcohol resin used in the present invention is usually preferably 98 mol% or more, particularly preferably 99 mol% or more, further preferably 99.5 mol% or more, and particularly preferably 99.8 mol% or more. If the average saponification degree is too small, when the polyvinyl alcohol film is formed into a polarizing film, there is a tendency that sufficient optical properties cannot be obtained.
[0062] Here, the average saponification degree in the present invention is measured in accordance with JIS K 6726.
[0063] As the polyvinyl alcohol-based resin used in the present invention, two or more types different in modification type, modification amount, weight average molecular weight, average saponification degree, etc. may be used in combination.
[0064] The polyvinyl alcohol resin is used to prepare a polyvinyl alcohol resin aqueous solution as a film-forming stock solution. The polyvinyl alcohol resin aqueous solution generally has a resin concentration of 5 to 70% by mass, preferably 10 to 60% by mass.
[0065] In terms of film-forming properties, it is more preferred that the polyvinyl alcohol resin aqueous solution contains, in addition to the polyvinyl alcohol resin, a commonly used plasticizer such as glycerol, diglycerol, triglycerol, ethylene glycol, triethylene glycol, polyethylene glycol, trimethylolpropane, and at least one surfactant selected from nonionic, anionic, and cationic surfactants as required. These surfactants may be used alone or in combination of two or more.
[0066] The resin concentration of the polyvinyl alcohol-based resin aqueous solution thus obtained is preferably 15 to 60% by mass, particularly preferably 17 to 55% by mass, and further preferably 20 to 50% by mass. If the resin concentration of the aqueous solution is too low, the drying load becomes large, thereby tending to reduce the production capacity, and if it is too high, the viscosity becomes excessively high, tending to make it difficult to dissolve uniformly.
[0067] Next, the obtained polyvinyl alcohol-based resin aqueous solution is subjected to a degassing treatment. As a degassing method, static degassing, degassing based on a multi-screw extruder and the like can be cited. As a multi-screw extruder, any multi-screw extruder with a vent is sufficient, and a twin-screw extruder with a vent is generally used.
[0068] <Process (B)>
[0069] The step (B) is a step of casting an aqueous solution of a polyvinyl alcohol-based resin on a casting mold to form a film.
[0070] After the degassing treatment, the polyvinyl alcohol-based resin aqueous solution was introduced into a T-slit die in a fixed amount, discharged onto a rotating casting die, and cast to form a film by a continuous casting method.
[0071] The resin temperature of the polyvinyl alcohol-based resin aqueous solution at the outlet of the T-slit die is preferably 80 to 100°C, particularly preferably 85 to 98°C.
[0072] If the resin temperature of the polyvinyl alcohol-based resin aqueous solution is too low, the fluidity tends to be poor, and if it is too high, foaming tends to occur.
[0073] The viscosity of the polyvinyl alcohol-based resin aqueous solution when discharged is preferably 50 to 200 Pa·s, particularly preferably 70 to 150 Pa·s.
[0074] If the viscosity of the aqueous solution is too high, the fluidity tends to be poor, and if it is too low, film casting tends to be difficult.
[0075] The discharge speed of the polyvinyl alcohol-based resin aqueous solution discharged from the T-slit die to the casting die is preferably 0.2 to 5 m / min, particularly preferably 0.4 to 4 m / min, and further preferably 0.6 to 3 m / min.
[0076] If the discharge speed is too slow, productivity tends to decrease, and if it is too fast, casting tends to become difficult.
[0077] When the casting mold is a casting drum, the diameter of the drum is preferably 2 to 5 m, particularly preferably 2.4 to 4.5 m, and further preferably 2.8 to 4 m.
[0078] If the diameter is too small, the drying zone on the casting drum becomes short, so the speed tends to be difficult to increase. If it is too large, the conveying performance tends to decrease.
[0079] The width of the casting mold is preferably 4 m or more, particularly preferably 4.5 m or more, further preferably 5 m or more, and particularly preferably 5 to 8 m.
[0080] If the width of the casting mold is too small, productivity tends to decrease.
[0081] The speed of the casting mold is preferably 3 to 50 m / min, particularly preferably 7 to 40 m / min, and further preferably 10 to 35 m / min.
[0082] If the speed is too slow, productivity tends to decrease, and if it is too fast, drying tends to be insufficient.
[0083] The upper limit of the surface temperature of the casting mold is preferably 100° C. or lower, particularly preferably 97° C. or lower, further preferably 95° C. or lower, and particularly preferably 92° C. or lower, in terms of suppressing foaming during drying and obtaining a film with excellent appearance. In terms of excellent releasability when the film obtained by film formation is peeled off from the casting mold, the lower limit is preferably 60° C. or higher, particularly preferably 65° C. or higher, further preferably 70° C. or higher, particularly preferably 75° C. or higher, and particularly preferably 80° C. or higher.
[0084] The moisture content of the film immediately after being peeled off from the casting mold is preferably 18% by mass or less, particularly preferably 17% by mass or less, further preferably 16% by mass or less, and particularly preferably 15% by mass or less. If the moisture content is too high, the dissolved residual crystal ratio tends to increase, and the tension during the manufacture of the polarizing film tends to be high, which tends to cause breakage.
[0085] The moisture content immediately after peeling is preferably 3% by mass or more, particularly preferably 5% by mass or more, and further preferably 7% by mass or more. If the moisture content is too low, the film tends to curl easily.
[0086] The lower limit of the evaporation rate of water on the casting mold is preferably 1.65% / sec or more, particularly preferably 1.7% / sec or more, further preferably 1.75% / sec or more, and particularly preferably 1.8% / sec or more.
[0087] The upper limit is preferably 3.0% / sec or less, particularly preferably 2.7% / sec or less, and further preferably 2.6% / sec or less.
[0088] If the evaporation rate of water on the casting mold is too slow, the dissolved residual crystal ratio tends to increase, and the tension during the production of the polarizing film tends to be high and breakage tends to occur easily. If it is too fast, it tends to cause poor appearance such as bending.
[0089] <Process (C)>
[0090] Step (C) is a step of heating and drying the film formed as described above.
[0091] The film (the film formed as described above) peeled from the casting mold is dried by conveying it in the flow direction (MD direction) with a nip roller or the like, and making the front and back of the film contact alternately with a plurality of hot rollers, thereby drying. The hot rollers are, for example, rollers with a diameter of 0.2 to 2 m, the surface of which is hard chrome plated or mirror-finished. Usually, 2 to 30 hot rollers, preferably 10 to 25 hot rollers, are used for drying.
[0092] The surface temperature of the heat roll is not particularly limited, but is usually preferably 60 to 150° C., more preferably 70 to 140° C. If the surface temperature is too low, drying tends to be poor, while if it is too high, drying tends to be excessive, resulting in poor appearance such as warping.
[0093] The upper limit of the hot roller drying time is preferably 60 seconds or less, particularly preferably 55 seconds or less, further preferably 50 seconds or less, and particularly preferably 45 seconds or less. In addition, the lower limit is preferably 20 seconds or more, particularly preferably 25 seconds or more, further preferably 27 seconds or more, and particularly preferably 30 seconds or more.
[0094] If the hot roll drying time is too long, the dyeability during the production of the polarizing film tends to be reduced. If it is too fast, wrinkles and folds are easily generated in the film during the swelling step during the production of the polarizing film, and the appearance of the polarizing film tends to be reduced.
[0095] <Process (D)>
[0096] Step (D) is a step of heat-treating the obtained thin film using hot air.
[0097] The film after the step (C) may be heat-treated using, for example, a floating dryer.
[0098] The upper limit of the heat treatment temperature is preferably 140°C or lower, particularly preferably 137°C or lower, further preferably 135°C or lower, and particularly preferably 130°C or lower. The lower limit is preferably 100°C or higher, particularly preferably 103°C or higher, further preferably 105°C or higher, and particularly preferably 110°C or higher.
[0099] If the heat treatment temperature is too high, the dyeability during the production of the polarizing film tends to be reduced, while if it is too low, wrinkles and creases are easily generated in the film during the swelling step during the production of the polarizing film, and the appearance of the polarizing film tends to be reduced.
[0100] The heat treatment time is preferably 20 to 100 seconds, particularly preferably 40 to 70 seconds.
[0101] 〔Polyvinyl alcohol film〕
[0102] In this way, a polyvinyl alcohol-based film is obtained through the above steps (A) to (D), and is finally wound into a roll to become a product.
[0103] The thickness of the polyvinyl alcohol film of the present invention thus obtained is preferably 10 μm or more, particularly 15 μm or more, further preferably 20 μm or more, and particularly preferably 25 μm or more in terms of the production stability of the polarizing film. In addition, in terms of reducing the warping of a liquid crystal display using a polarizing film made of the polyvinyl alcohol film, the upper limit is preferably 70 μm or less, particularly 60 μm or less, further preferably 50 μm or less, particularly preferably 45 μm or less, and more preferably 35 μm or less.
[0104] The length of the polyvinyl alcohol-based film is usually 1 km or longer, preferably 4 km or longer from the viewpoint of increasing the area of the polarizing film, and particularly preferably 5 to 50 km from the viewpoint of transport quality.
[0105] In terms of widening the width of the polarizing film, the width of the polyvinyl alcohol-based film is preferably 4 m or more, particularly preferably 5 m or more, and further preferably 5 to 6 m from the viewpoint of avoiding breakage during production of the polarizing film.
[0106] The polyvinyl alcohol-based film of the present invention is useful for optical applications, and is particularly useful as a raw film for a polarizing film. Hereinafter, a method for producing a polarizing film and a polarizing plate formed of the polyvinyl alcohol-based film will be described.
[0107] From the perspective of suppressing the pollution of polarizing film manufacturing equipment, the elution amount of polyvinyl alcohol resin from the polyvinyl alcohol film is preferably 40 ppm or less, particularly preferably 35 ppm or less, and further preferably 30 ppm or less. The most preferred lower limit is 0 ppm. The elution amount of polyvinyl alcohol resin can be measured, for example, by the method described in the examples described below.
[0108] From the perspective of suppressing breakage during the manufacture of the polarizing film, the tensile tension of the polyvinyl alcohol film is preferably 0.8 N / mm or less, particularly preferably 0.75 N / mm or less, and further preferably 0.7 N / mm or less. The lower limit is usually 0.30 N / mm. The tensile tension of the polyvinyl alcohol film can be measured, for example, by the method described in the examples described below.
[0109] [Polarizing film manufacturing method]
[0110] The polarizing film of the present invention is produced by unwinding the obtained polyvinyl alcohol-based film from a roll, conveying it in a horizontal direction, and subjecting it to steps such as swelling, dyeing, boric acid cross-linking, stretching, washing, and drying.
[0111] The swelling step is performed before the dyeing step. The swelling step can not only clean the dirt on the surface of the polyvinyl alcohol film, but also swell the polyvinyl alcohol film to prevent uneven dyeing.
[0112] In the swelling process, water is usually used as the treatment liquid. The treatment liquid may be water as the main component, and may also contain additives such as iodinated compounds, surfactants, alcohols, etc. The temperature of the swelling bath is usually about 10 to 45°C, and the immersion time in the swelling bath is usually about 0.1 to 10 minutes.
[0113] The dyeing process is carried out by bringing the film into contact with a liquid containing iodine or a dichroic dye. An aqueous solution of iodine-potassium iodide is usually used, and it is appropriate that the concentration of iodine is 0.1 to 2 g / L and the concentration of potassium iodide is 1 to 100 g / L. It is practical to dye for about 30 to 500 seconds. The temperature of the treatment bath is preferably 5 to 50°C. In addition to the water solvent, the aqueous solution may also contain a small amount of an organic solvent that is compatible with water.
[0114] The boric acid crosslinking process is carried out using a boron compound such as boric acid or borax. The boron compound is used in the form of an aqueous solution or a water-organic solvent mixture at a concentration of about 10 to 100 g / L. In terms of stabilizing the polarization performance, potassium iodide is preferably coexisted in the liquid. The preferred treatment temperature is about 30 to 70° C. and the treatment time is about 0.1 to 20 minutes. In addition, a stretching operation can be performed during the treatment as needed.
[0115] In the stretching process, the film is preferably stretched 3 to 10 times, preferably 3.5 to 7 times, along a uniaxial direction. At this time, some stretching may be performed in a direction perpendicular to the stretching direction (to prevent shrinkage in the width direction, or stretching above that). The temperature during stretching is preferably 40 to 170°C. Furthermore, as long as the stretching ratio is finally set to the aforementioned range, the stretching operation is not only one stage, but may also be performed multiple times in the manufacturing process.
[0116] The cleaning process is carried out, for example, by immersing the film in an aqueous iodide solution such as water or potassium iodide, so that the precipitate produced on the surface of the film can be removed. When using an aqueous potassium iodide solution, the potassium iodide concentration is preferably about 10 to 1000 g / L. The temperature during the cleaning treatment is usually 5 to 50° C., preferably 10 to 45° C. The treatment time is usually 1 to 300 seconds, preferably 10 to 240 seconds. It should be noted that water cleaning and cleaning based on an aqueous potassium iodide solution can be appropriately combined and carried out.
[0117] The drying step is performed, for example, by drying at 40 to 100° C. for 0.1 to 10 minutes using a dryer.
[0118] The polarizing film thus obtained preferably has a polarization degree of 99.90% or more, more preferably 99.99% or more, and the upper limit is 100%. If the polarization degree is too low, the contrast in a liquid crystal display tends to decrease.
[0119] The degree of polarization is generally calculated as follows: the transmittance (H) measured at a wavelength λ in a state where two polarizing films are stacked so that their orientation directions are in the same direction. 11 ), and the light transmittance (H1) measured at a wavelength λ in a state where two polarizing films are overlapped so that their orientation directions are orthogonal to each other, are calculated according to the following formula (1).
[0120] Polarization degree=〔(H 11 -H1) / (H 11 +H1)〕 1 / 2 ···(1)
[0121] Furthermore, the single transmittance of the polarizing film of the present invention is preferably 43% or more. If the single transmittance is too low, it tends to be impossible to achieve high brightness of a liquid crystal display.
[0122] The single-sheet transmittance is a value obtained by measuring the light transmittance of a polarizing film alone using a spectrophotometer.
[0123] Next, a method for producing the polarizing plate of the present invention using the polarizing film of the present invention will be described.
[0124] The polarizing film of the present invention is suitable for manufacturing a polarizing plate having less chromaticity unevenness and excellent polarization performance.
[0125] [Polarizing plate manufacturing method]
[0126] The polarizing plate of the present invention is prepared as follows: an optically isotropic resin film is bonded to one or both sides of the polarizing film of the present invention by means of an adhesive as a protective film. Examples of the protective film include films formed of acetyl cellulose resins such as triacetyl cellulose and diacetyl cellulose, films formed of polyester resins such as polyethylene terephthalate, polyethylene naphthalate and polybutylene terephthalate, polycarbonate resin films, cycloolefin resin films, acrylic resin films, and films formed of chain olefin resins such as polypropylene resins.
[0127] The lamination is performed by a known method, for example, by uniformly applying a liquid adhesive composition to the polarizing film, the protective film, or both, laminating and pressing the two, and then heating and irradiating them with active energy rays.
[0128] It should be noted that a polarizing plate can also be formed by coating a curable resin such as a urethane resin, an acrylic resin, or a urea resin on one or both sides of a polarizing film and curing the cured layer. In this way, the cured layer becomes a substitute for the protective film and can be made thinner.
[0129] The polarizing film and polarizing plate obtained using the polyvinyl alcohol-based film of the present invention have excellent polarizing properties and are preferably used in liquid crystal display devices such as portable information terminals, personal computers, televisions, projectors, signs, electronic desktop computers, electronic clocks, word processors, electronic paper, game consoles, video cameras, cameras, photo albums, thermometers, audio equipment, automobiles, mechanical instruments, etc., sunglasses, anti-glare glasses, stereo glasses, wearable displays, foldable displays, anti-reflection layers for display elements (CRT, LCD, organic EL, electronic paper, etc.), optical communication equipment, medical equipment, building materials, toys, etc.
[0130] Example
[0131] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples unless the gist of the invention is exceeded.
[0132] In addition, "part" and "%" in the examples are based on mass.
[0133] <Measurement conditions>
[0134] (1) Moisture content of the film immediately after peeling from the casting mold A [%]
[0135] For the film just peeled off from the casting mold, a sample was taken from the center of the width direction to measure the initial mass A0 (g). Then, the moisture content [%] of the film was calculated according to the following formula (i) from the mass A1 (g) of the film after drying in a vacuum dryer at 83°C for 20 minutes.
[0136] Moisture content A[%] = 100×(A0-A1) / A0···(i)
[0137] The average value of the results of sampling and measurement three times in total was defined as the moisture content A [%] of the film immediately after being peeled off from the casting mold.
[0138] (2) Crystallinity
[0139] A 50 mm × 50 mm test piece was cut out from the obtained polyvinyl alcohol film, and the test piece was vacuum dried in a vacuum dryer set at 83°C for 20 minutes, and then cooled in a desiccator for 10 minutes. The temperature was raised from -50°C to 250°C at a heating rate of 10°C / min using DSC (Q2000 manufactured by TA instruments, aluminum pan, 5 mg sample), and the heat of fusion ΔH (J / g) per 1 g of the sample was measured. The degree of crystallinity was calculated from the above heat of fusion (J / g) according to the following formula (X).
[0140] Crystallinity = △H (J / g) / 156 (J / g) × 100···(X)
[0141] (3) Dissolved residual crystallization rate after immersion in water for 30 seconds
[0142] The obtained polyvinyl alcohol film was immersed in water (water temperature 10° C.) for 30 seconds and then taken out to wipe off the water on the surface. Thereafter, the film was measured by NMR (Nuclear Magnetic Resonance) using a solid echo method. The measurement method was set as follows.
[0143] Device: Bruker AVANCEIII 400WB
[0144] Probe: 4mmΦCPMPS
[0145] ·Measurement temperature: 25℃
[0146] Test tube speed: 0Hz
[0147] Observation core: 1 H(400.3MHz)
[0148] Pulse sequence: Solid Echo
[0149] · 1 H H90℃ pulse: (2.0μs)×(-4.6dB)(224W / 300W)
[0150] Echo delay: 5μs
[0151] Acquisition time: 4ms
[0152] ·FID points: 8192
[0153] Pulse delay: 4s
[0154] Cumulative times: 1
[0155] The real part of the obtained FID was subjected to curve fitting using the following formula (Y) to calculate the first component (dissolved residual component) and the second component (soft component). 1 The spin-spin relaxation time (T 2H ) and its quantity (M(0)).
[0156]
[0157] Finally, the dissolved residual crystal ratio was calculated according to the following formula (Z).
[0158] Dissolved residual crystal ratio after immersion in water for 30 seconds (%) = 100 × M1(0) / {M1(0)+M2(0)}···(Z)
[0159] (4) Dissolution amount of polyvinyl alcohol resin (ppm)
[0160] The obtained polyvinyl alcohol film was subjected to humidity conditioning at 23°C and 50% RH for 24 hours, and five test pieces of 100 mm x 100 mm were cut out to make a total of 0.05 mm 2 ) was immersed in 1L of ion exchange water at 50°C for 1 minute to obtain an eluate. At room temperature (23°C), 10mL of a colorimetric reagent (500g of ion exchange water, 7.4g of potassium iodide, 0.65g of iodine, 10.6g of boric acid) was mixed in 10mL of the above eluate, and the absorbance at a wavelength of 690nm was measured using a spectrophotometer (UV-3100PC manufactured by Shimadzu Corporation), and the concentration (ppm) of the polyvinyl alcohol-based resin was calculated from a pre-prepared standard curve.
[0161] (Evaluation Criteria)
[0162] ○ (good): Dissolution amount 40ppm or less
[0163] × (bad): Dissolution amount exceeds 40 ppm
[0164] (5) Tensile tension
[0165] The obtained polyvinyl alcohol film was unwound from the roll, transported in the horizontal direction, immersed in a water tank at a water temperature of 25°C to swell, and stretched in the flow direction (MD direction) to 1.6 times the original blank. In the above swelling process, no creases or wrinkles were generated in the film. Next, it was immersed in an aqueous solution (liquid temperature 28°C) containing 30g / L of potassium iodide, and stretched in the flow direction (MD direction) while dyeing to 2.3 times the original blank. Furthermore, it was immersed in an aqueous solution (liquid temperature 59°C, the treatment tank was called a stretching tank) composed of 30g / L of boric acid and 30g / L of potassium iodide, and uniaxially stretched in the flow direction (MD direction) to 5.9 times the original blank. The tension (N) at this time was measured. The value obtained by dividing the tension by the width (mm) of the polarizing film being processed at the exit of the stretching tank was taken as the tension (N / mm) when stretched 5.9 times.
[0166] The tensile strength (N / mm) at 5.9 times stretching was evaluated according to the following evaluation criteria.
[0167] (Evaluation Criteria)
[0168] ○(Good): 0.8N / mm or less
[0169] ×(bad): greater than 0.8N / mm
[0170] (6) Number of breaks within 6 hours in manufacturing polarizing film
[0171] During the production of the polarizing film, the number of times the polarizing film was broken within 6 hours was measured.
[0172] (7) Polarization degree (%)
[0173] A sample of 4 cm in length×4 cm in width was cut out from the obtained polarizing film, and the degree of polarization (%) was measured using an automatic polarizing film measuring apparatus (VAP7070 manufactured by JASCO Corporation).
[0174] (Evaluation Criteria)
[0175] ○(Good): 99.993% or more
[0176] ×(Poor): Less than 99.993%
[0177] <Example 1>
[0178] (Production of polyvinyl alcohol film)
[0179] In a 500L dissolving tank, 100kg of a polyvinyl alcohol resin having a weight average molecular weight of 156,000 and a saponification degree of 99.8 mol%, 300kg of water, 11.5kg of glycerol as a plasticizer, and 0.03kg of sodium dodecyl sulfate as a surfactant were placed. The mixture was heated to 150°C while being stirred and pressurized to obtain a polyvinyl alcohol resin aqueous solution having a resin concentration of 26.0%.
[0180] Next, the polyvinyl alcohol resin aqueous solution was supplied to a twin-screw extruder with an exhaust port and degassed, and then the aqueous solution temperature was set to 95°C, and the solution was discharged from the T-slit die outlet on a rotating casting mold temperature of 88°C and cast, and retained on the casting mold for 34 seconds, and film-made at a water evaporation rate of 1.9% / second. The moisture content of the obtained film just after being peeled off from the casting mold was 10%. Next, the surface and back of the film were alternately contacted with a total of 10 hot rollers while drying for 34 seconds, and then, hot air of 125°C was blown from both sides of the film for heat treatment, and finally slit and wound to obtain a rolled polyvinyl alcohol film (film thickness 30μm, width 0.6m, length 1km). The properties of the obtained polyvinyl alcohol film are shown in Table 1.
[0181] (Production of polarizing film)
[0182] The obtained polyvinyl alcohol film is unwound from the roller, conveyed in the horizontal direction, immersed in a water tank at a water temperature of 25°C, and stretched in the flow direction (MD direction) to 1.6 times the original blank while swelling. In the above swelling process, no creases or wrinkles are generated in the film. Next, the iodine amount is adjusted in such a way that the single-piece transmittance of the polarizing film finally obtained becomes 43.5%, immersed in an aqueous solution (28°C) containing 30g / L of potassium iodide, and stretched in the flow direction (MD direction) to 2.3 times the original blank as a reference, and then immersed in an aqueous solution (59°C) composed of 30g / L of boric acid and 30g / L of potassium iodide, and uniaxially stretched in the flow direction (MD direction) to 5.9 times the original blank as a reference while performing boric acid crosslinking. Finally, it is washed with an aqueous potassium iodide solution and dried at 80°C for 40 seconds to obtain a polarizing film. The polarization properties of the polarizing film are shown in Table 1.
[0183] <Example 2>
[0184] A polyvinyl alcohol film was obtained in the same manner as in Example 1 except that the temperature of the casting mold was changed to 75°C, the evaporation rate of water was changed to 1.7% / sec, and the moisture content of the film immediately after peeling was changed to 16%. The properties of the obtained polyvinyl alcohol film and the properties of the polarizing film obtained in the same manner as in Example 1 are shown in Table 1.
[0185] <Comparative Example 1>
[0186] A polyvinyl alcohol film was obtained in the same manner as in Example 1 except that the temperature of the casting mold was changed to 70°C, the evaporation rate of water was changed to 1.6% / sec, and the moisture content of the film immediately after peeling was changed to 20%. The properties of the obtained polyvinyl alcohol film and the properties of the polarizing film obtained in the same manner as in Example 1 are shown in Table 1.
[0187] [Table 1]
[0188]
[0189] The crystallinity of the polyvinyl alcohol-based films of Examples 1 and 2 and the dissolved residual crystallinity rate after immersion in water for 30 seconds are within the specific range of the present invention. Therefore, the amount of dissolution from the film is low when manufacturing the polarizing film, and the stretching tension is low. As a result, there is no breakage in the manufactured polarizing film, and a polarizing film with high polarization performance is obtained.
[0190] On the other hand, since the tensile tension of the polyvinyl alcohol-based film of Comparative Example 1 was high when forming a polarizing film, many breaks occurred during the polarizing plate film formation, and the film forming property was deteriorated.
[0191] It is also found that the polarizing plate obtained by bonding the protective film to the polarizing film having high polarizing performance without breakage during the production of the polarizing film as in Examples 1 and 2 also has high polarizing performance.
[0192] The above embodiments show specific aspects of the present invention, but the above embodiments are merely examples and are not to be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention.
[0193] Industrial Applicability
[0194] The polarizing film using the polyvinyl alcohol-based film of the present invention has excellent polarizing properties and is preferably used in liquid crystal display devices such as portable information terminals, personal computers, televisions, projectors, signs, electronic desktop computers, electronic clocks, word processors, electronic paper, game consoles, video cameras, cameras, photo albums, thermometers, audio equipment, automobiles, mechanical instruments, etc., sunglasses, anti-glare glasses, stereo glasses, wearable displays, foldable displays, rollable televisions, rollable displays, anti-reflection films for display elements (CRT, LCD, organic EL, electronic paper, etc.), optical communication equipment, medical equipment, building materials, toys, etc.
Claims
1. A polyvinyl alcohol film, It is characterized in that The crystallinity is 38% or more, and the dissolved residual crystal ratio after immersion in water for 30 seconds is 18% or less.
2. The polyvinyl alcohol film according to claim 1, It is characterized in that The thickness of the polyvinyl alcohol-based film is 10 to 70 μm.
3. A polarizing film, It is characterized in that This is obtained by using the polyvinyl alcohol-based film according to claim 1 or 2.
4. A polarizing plate, It is characterized in that The invention comprises: the polarizing film according to claim 3, and a protective film provided on at least one surface of the polarizing film.