Transparent porous forming coating material and method for producing transparent porous forming coating material

By adjusting the particle concentration in the transparent porous forming coating and using a high boiling point dispersion medium, the problem of reducing transparency after spraying is solved, and a high-transparency and smooth transparent porous membrane suitable for multi-shaped optical components is achieved.

CN118891329APending Publication Date: 2024-11-01NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380031352.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-23
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing transparent porous membranes tend to reduce transparency during the spraying process, making it difficult to adapt to the diverse shapes of optical components, and the existing coatings lack transparency and surface smoothness after spraying.

Method used

Use transparent porous materials with a particle concentration of 0.1% to 6.0%, use a dispersion medium with a boiling point above 150°C, and adjust the particle distribution and medium replacement to ensure that the coating is suitable Spray and create excellent transparency and surface smoothness.

Benefits of technology

It realizes excellent transparency and surface smoothness of the transparent porous membrane, is suitable for multi-shaped optical components, and improves the optical characteristics and mechanical strength of the transparent porous membrane.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

Provided are: a transparent porous-forming coating material which can be suitably used for spray coating and is capable of producing a transparent porous film having excellent transparency; and a method for producing the transparent porous-forming coating material. A transparent porous forming coating material according to an embodiment of the present invention comprises particles and a dispersion medium in which the particles are dispersed, the concentration of the particles in the coating material being 0.1-6.0 mass%, and the dispersion medium comprising a first dispersion medium having a boiling point of 150 DEG C or higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent porous coating material and a method for producing the transparent porous coating material. Background Art

[0002] It is known that a transparent porous film having a refractive index smaller than that of the optical component is provided on various optical components to arbitrarily control the optical properties of the optical products containing them. Such a transparent porous film is manufactured, for example, by applying an organic silica sol coating containing a pulverized product of a gel-like silicon compound and a dispersion medium to a substrate (for example, refer to Patent Document 1). In the past, from the perspective of manufacturing efficiency, such a transparent porous film was manufactured by die coating on a long strip substrate and pasted to the optical component after being peeled off from the substrate. However, in recent years, the use of optical products has become more and more diverse, and the formation of transparent porous films directly on optical components has been explored. Since optical components may take various shapes (special shapes, small pieces, etc.) corresponding to the use, it is expected that the coating is sprayed on the object to form a transparent porous film. However, if the organic silica sol coating described in Patent Document 1 is used for spraying, the transparency of the transparent porous film is sometimes reduced.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2017-25277 Summary of the invention

[0006] Problems to be solved by the invention

[0007] The present invention has been made to solve the above-mentioned conventional problems, and its main object is to provide a transparent porous-forming coating material which can be suitably used for spray coating and can produce a transparent porous film having excellent transparency, and a method for producing the same.

[0008] Solutions to the problem

[0009] The transparent porous coating material according to an embodiment of the present invention comprises: particles; and a dispersion medium in which the particles are dispersed, wherein the concentration of the particles in the transparent porous coating material is 0.1 mass % to 6.0 mass %, and the dispersion medium comprises a first dispersion medium having a boiling point of 150° C. or higher.

[0010] In one embodiment, the content ratio of the first dispersion medium in the dispersion medium is 3 mass % to 100 mass %.

[0011] In one embodiment, the particles are porous particles of a silicon compound.

[0012] A method for producing a transparent porous coating material according to another aspect of the present invention includes: a step of pulverizing a pulverized material in a hydrophilic medium to prepare a sol solution in which particles are dispersed in the hydrophilic medium; and a step of replacing the hydrophilic medium contained in the sol solution with a dispersion medium containing a first dispersion medium having a boiling point of 150° C. or higher, and adjusting the concentration of particles in the transparent porous coating material to 0.1% by mass to 6.0% by mass.

[0013] Effects of the Invention

[0014] The transparent porous-forming coating material according to the embodiment of the present invention can be suitably used for spray coating, and can produce a transparent porous film having excellent transparency. DETAILED DESCRIPTION

[0015] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0016] A. Overview of transparent porous coating

[0017] The transparent porous coating in one embodiment comprises particles and a dispersion medium in which the particles are dispersed. The concentration of the particles in the transparent porous coating is 0.1% by mass or more, preferably 1.0% by mass or more, more preferably 2.0% by mass or more, 6.0% by mass or less, preferably 5.0% by mass or less. The dispersion medium comprises a first dispersion medium having a boiling point of 150° C. or more. The boiling point of the first dispersion medium is a boiling point at 1 atmosphere, preferably 155° C. or more, more preferably 165° C. or more, for example, 200° C. or less, preferably 190° C. or less. According to such a configuration, the concentration of the particles in the transparent porous coating is within the above range, and the boiling point of the first dispersion medium contained in the dispersion medium is above the above lower limit, so even if a transparent porous film is manufactured by spraying the transparent porous coating, excellent transparency can be imparted to the transparent porous film, and the surface smoothness of the transparent porous film can be improved.

[0018] In one embodiment, the content of the first dispersion medium in the dispersion medium is, for example, 3% by mass or more, preferably 5% by mass or more, more preferably 40% by mass or more, for example, 100% by mass or less, preferably 90% by mass or less, more preferably 60% by mass or less. If the content of the first dispersion medium is within the above range, the transparency of the transparent porous film manufactured by spraying can be further improved.

[0019] The dispersion medium may consist of only the first dispersion medium, or may contain a second dispersion medium in addition to the first dispersion medium.

[0020] Hereinafter, the particles and the dispersion medium contained in the transparent porous forming coating material will be described in detail.

[0021] B. Particles

[0022] The particles can be made of any material suitable for the manufacture of transparent porous films. As the material constituting the particles, for example, the materials described in International Publication No. 2004 / 113966, Japanese Patent Publication No. 2013-254183, Japanese Patent Publication No. 2012-189802, and Japanese Patent Publication No. 2017-25277 can be used. As the material, both inorganic and organic substances can be provided.

[0023] Examples of the inorganic substance constituting the particles include silicon compounds containing Si, magnesium compounds containing Mg, aluminum compounds containing Al, titanium compounds containing Ti, zinc compounds containing Zn, and zirconium compounds containing Zr.

[0024] Examples of the organic substance constituting the particles include organic polymers; polymerizable monomers (eg, (meth)acrylic monomers and styrene monomers); and curable resins (eg, (meth)acrylic resins, fluorine-containing resins, and urethane resins).

[0025] The materials constituting these particles may be used alone or in combination.

[0026] Among such materials, inorganic substances are preferred, and silicon compounds are more preferred. Specific examples of silicon compounds include: silicon dioxide compounds; hydrolyzable silanes, and partial hydrolyzates and dehydrated condensates thereof; silicon compounds containing silanol groups; and active silica obtained by contacting silicates with acids and ion exchange resins. Among silicon compounds, silicon compounds containing silanol groups are preferred.

[0027] In an embodiment of the present invention, the shape of the "particles" (for example, the porous particles described later) is not particularly limited, and may be, for example, spherical or other shapes. The particles may take any appropriate shape. Examples of the shape of the particles include: spherical, plate-like, needle-like, rope-like, and bunches of grapes. Examples of rope-like particles include: particles formed by connecting a plurality of particles having a spherical, plate-like or needle-like shape into a rosary shape, short-fiber particles (for example, short-fiber particles described in Japanese Patent Gazette No. 2001-188104), and combinations thereof. Rope-like particles may be linear or branched. Examples of bunches of grape-like particles include: particles formed by agglomerating a plurality of spherical, plate-like and needle-like particles into a bunch of grapes. The shape of the particles can be confirmed, for example, by observation using a transmission electron microscope.

[0028] The particles preferably have voids (pores). More preferred examples of the particles include hollow particles (hollow nano-silica / nano hollow sphere particles) and porous particles, and even more preferred examples include porous particles.

[0029] In one embodiment, the particles are porous particles of silicon compounds. According to such a configuration, a transparent porous film having desired optical properties can be stably manufactured. The porous particles of silicon compounds are preferably a pulverized body of a gel-like silicon compound obtained by pulverizing a gel-like silicon compound in a medium (representatively a hydrophilic medium). The pulverized body will be described in detail later.

[0030] In one embodiment, the volume average particle size of the particles (representatively pulverized body) is, for example, 0.05 μm or more, preferably 0.10 μm or more, more preferably 0.20 μm or more, and further preferably 0.40 μm or more, for example, 2.00 μm or less, preferably 1.50 μm or less, and more preferably 1.00 μm or less. The volume average particle size represents the particle size deviation of the particles (pulverized body) in the transparent porous forming coating, and can be measured, for example, by a particle size distribution evaluation device such as a dynamic light scattering method and a laser diffraction method, and an electron microscope such as a scanning electron microscope (SEM) and a transmission electron microscope (TEM).

[0031] In one embodiment, in the particle size distribution of particles (representatively pulverized bodies), particles with a particle size of 0.05 μm to 1 μm are, for example, 50% to 99.9% by mass, preferably 80% to 99.8% by mass, more preferably 90% to 99.7% by mass, and particles with a particle size of 1 μm to 2 μm are, for example, 0.1% to 50% by mass, preferably 0.2% to 20% by mass, more preferably 0.3% to 10% by mass. The particle size distribution represents the particle size deviation of the particles (pulverized bodies) in the transparent porous forming coating, and can be measured, for example, by a particle size distribution evaluation device or an electron microscope.

[0032] The content of such particles is adjusted so that the concentration of the particles in the transparent porous forming coating reaches the above range. The content of the particles is, for example, 0.1 parts by mass or more, preferably 0.5 parts by mass or more, for example, 50 parts by mass or less, preferably 30 parts by mass or less, relative to 100 parts by mass of the dispersion medium.

[0033] C. Dispersion medium

[0034] The dispersion medium includes a first dispersion medium having a boiling point greater than or equal to the above lower limit. Examples of the first dispersion medium include dimethyl sulfoxide (DMSO); esters such as ethylene glycol monoethyl ether acetate and ethyl lactate; ethers such as diethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, dipropylene glycol dimethyl ether, dipropylene glycol monomethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol butyl methyl ether, tripropylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol monobutyl ether, ethylene glycol monophenyl ether, triethylene glycol monomethyl ether, diethylene glycol dibutyl ether, triethylene glycol butyl methyl ether, polyethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and polyethylene glycol monomethyl ether.

[0035] These first dispersion media may be used alone or in combination. Among these first dispersion media, preferably, esters and ethers are used, and more preferably, diethylene glycol ethyl methyl ether and ethylene glycol monoethyl ether acetate are used.

[0036] In one embodiment, the dispersion medium further includes a second dispersion medium having a boiling point in the following range in addition to the first dispersion medium. The boiling point of the second dispersion medium is, for example, lower than 150°C, preferably lower than 130°C, more preferably lower than 110°C, for example, higher than 80°C, preferably higher than 90°C.

[0037] As the second dispersion medium, for example, alcohols such as ethanol, isopropanol, butanol, tert-butyl alcohol, isobutyl alcohol, and 2-methoxyethanol (methyl cellosolve) can be cited; esters such as ethyl acetate and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; and aromatic hydrocarbons such as toluene. These second dispersion media can be used alone or in combination. Among these second dispersion media, alcohols can be more preferably cited, and isobutyl alcohol and 2-methoxyethanol can be further preferably cited.

[0038] The content ratio of the second dispersion medium in the dispersion medium is, for example, 0% by mass or more, preferably 5% by mass or more, more preferably 40% by mass or more, for example, 97% by mass or less, preferably 95% by mass or less, more preferably 60% by mass or less. If the content ratio of the second dispersion medium is within the above range, the viscosity of the transparent porous coating can be stably adjusted to a range suitable for spraying.

[0039] D. Method for producing transparent porous coating material

[0040] Next, a method for producing a transparent porous coating material according to an embodiment of the present invention is described. The method for producing a transparent porous coating material includes: a step of pulverizing a pulverized material in a hydrophilic medium to prepare a sol solution in which particles are dispersed in the hydrophilic medium; and a step of replacing the hydrophilic medium contained in the sol solution with the above-mentioned dispersion medium and adjusting the concentration of the particles to the above-mentioned range. If the solvent is replaced after the pulverized material is pulverized in this way, the dispersibility of the particles can be maintained.

[0041] In this method, first, a pulverized material that is a raw material for particles is prepared. As a method for preparing the pulverized material, for example, the method described in Japanese Patent Publication No. 2017-25277 can be cited. The entire description of the publication is cited as a reference in this specification. More specifically, a precursor of the material of the above particles (representatively a silicon compound) is gelled in a hydrophilic medium.

[0042] Examples of the hydrophilic medium include isopropyl alcohol (IPA), ethanol, methanol, butanol, acetone, dimethylformamide (DMF), and dimethyl sulfoxide (DMSO), preferably IPA and DMSO. The hydrophilic medium may be used alone or in combination. In addition, the hydrophilic medium may be mixed with water.

[0043] In this way, a pulverized product (typically a gel-like silicon compound) composed of the material of the above-mentioned particles can be prepared. The pulverized product (typically a gel-like silicon compound) is aged in a hydrophilic medium at, for example, 20° C. to 50° C. for 10 hours or more.

[0044] Next, the pulverized material (representatively a gel-like silicon compound) is pulverized in a hydrophilic medium by any appropriate method. It should be noted that the hydrophilic medium may be a mixed medium mixed with water. The pulverization method is not particularly limited. When the pulverized material is a gel-like silicon compound, high-pressure medium-free pulverization using a homogenizer is preferably used.

[0045] In this way, a sol solution in which the above-mentioned particles are dispersed in a hydrophilic medium can be prepared.

[0046] Next, the hydrophilic medium contained in the sol solution is replaced with the above-mentioned dispersion medium by any appropriate method. The replacement method of the solvent is not particularly limited, and for example, decantation, cross-flow filtration, and dynamic filter can be mentioned. These replacement methods are preferably implemented multiple times. It should be noted that, as required, the concentration of the particles is adjusted to the above-mentioned range using the above-mentioned dispersion medium. In addition, in the case of a mixed medium formed by mixing a hydrophilic medium and water, the hydrophilic medium can be replaced with the above-mentioned dispersion medium after the mixed medium is replaced by a hydrophilic medium (representatively, alcohols with a carbon number of less than 3).

[0047] In this manner, a transparent porous coating material containing the above-mentioned particles and the above-mentioned dispersion medium can be produced.

[0048] E. Spraying

[0049] The transparent porous coating material can be suitably used in spraying. In spraying, the transparent porous coating material is sprayed onto a substrate (typically an optical component such as an optical film) as an object to form a coating film on the substrate. The shape of the substrate is not particularly limited. As the shape observed from the thickness direction of the substrate, for example, there can be mentioned: polygonal shapes such as rectangles; circular shapes; elliptical shapes; irregular shapes with concave and / or convex parts. In addition, the surface shape of the substrate is not particularly limited.

[0050] In one embodiment, the transparent porous forming coating material is spray-coated on the substrate so that the solid content concentration change rate satisfies the following formula (1).

[0051] 1.3≤Solid content concentration change rate≤60···(1)

[0052] (In the formula (1), the solid content concentration change rate represents the solid content concentration in the coating film 10 seconds after spraying, relative to the solid content concentration in the transparent porous forming coating material before spraying).

[0053] When the solid content concentration change rate satisfies the above formula (1), the transparency of the transparent porous film can be further improved, and the thickness unevenness of the transparent porous film can be reduced.

[0054] The solid content concentration of the transparent porous forming coating material before spraying is, for example, 0.1 mass % or more, preferably 1.0 mass % or more, more preferably 2.0 mass % or more, and for example, 6.0 mass % or less, preferably 3.0 mass % or less.

[0055] The solid content concentration in the coating film 10 seconds after spraying is the solid content concentration in the coating film 10 seconds after the spraying of the coating from the spray head stops, for example, 3.7 mass % or more, preferably 4.5 mass %, for example, 6.5 mass % or less.

[0056] In one embodiment, the viscosity [mPa·s] of the coating film 10 seconds after spraying satisfies the following formula (2).

[0057] 0.0549e 1.2x ≤Viscosity of the coating 10 seconds after spraying≤0.0549e 3.3x ···(2)

[0058] (In formula (2), e represents the Napier number; x represents the solid content concentration in the coating film 10 seconds after spraying).

[0059] When the viscosity of the coating film satisfies the above formula (2), both improvement in transparency of the transparent porous film and reduction in thickness unevenness can be sufficiently achieved.

[0060] During spraying, the distance between the nozzle for spraying the transparent porous coating and the substrate (coating distance) can be appropriately adjusted. If the distance between the nozzle and the substrate becomes larger, the above-mentioned solid component concentration change rate becomes larger, and if the distance between the nozzle and the substrate becomes smaller, the above-mentioned solid component concentration change rate will become smaller. The distance between the nozzle and the substrate (coating distance) is, for example, more than 50 mm, preferably more than 100 mm, for example, less than 500 mm, preferably less than 300 mm.

[0061] In one embodiment, during spraying, the transparent porous forming coating is sprayed while the nozzle is moved along the surface direction of the substrate. The atomization pressure of the spraying is, for example, 100 kPa to 1000 kPa, the coating amount of the spraying is, for example, 0.1 mL / min to 20 mL / min, and the moving speed of the nozzle during spraying is, for example, 1 mm / sec to 1000 mm / sec.

[0062] Thus, a coating film forming a void structure as a precursor of a porous layer (void layer) is formed on a substrate. It should be noted that, below, the description is mainly for the case where the particles are pulverized products of gel-like compounds. However, in the case where the particles are other than pulverized products of gel-like compounds, a coating film can also be formed in the same manner. The reason why a suitable void structure can be formed in the coating film when the particles are pulverized products of gel-like compounds can be inferred as follows, for example. However, this inference does not limit the formation method of the transparent porous film.

[0063] The above-mentioned particles (porous particles) are obtained by crushing a gel-like silicon compound, and therefore, the three-dimensional structure of the gel-like silicon compound before crushing is formed in a state of being dispersed into a three-dimensional basic structure. Furthermore, in the above-mentioned method, a precursor of a porous structure based on a three-dimensional basic structure is formed by spraying the crushed material of the gel-like silicon compound on a substrate. That is, according to the above-mentioned method, a new porous structure (three-dimensional basic structure) based on the spraying of the crushed material, which is different from the three-dimensional structure of the gel-like silicon compound, can be formed. Therefore, in the finally obtained transparent porous film, a low refractive index that functions to the same extent as an air layer can be achieved.

[0064] Next, the coating film on the substrate is heated and dried to form a transparent porous film on the substrate. The heating temperature is, for example, 60° C. or higher, preferably 70° C. or higher, more preferably 80° C. or higher, and for example, 200° C. or lower, preferably 120° C. or lower, more preferably 100° C. or lower. The heating time is not particularly limited as long as the coating film can be sufficiently dried.

[0065] In one embodiment, in this process, a cross-linking reaction occurs between the plurality of particles contained in the coating film, thereby fixing the three-dimensional basic structure. Thus, the transparent porous film finally obtained can maintain sufficient strength and flexibility despite having a void structure.

[0066] Thus, a transparent porous film is formed on the substrate.

[0067] F. Transparent porous membrane

[0068] The transparent porous film can be, for example, a connected cell structure formed by a continuous pore structure. A connected cell structure refers to a state in which the pore structure is connected in three dimensions, and can also be considered to be a state in which the internal voids of the pore structure are continuous. By making the transparent porous film have a connected cell structure, the porosity can be increased. The transparent porous film more preferably has a monolithic structure in which the connected cell structure includes a plurality of pores distributed. The monolithic structure refers to a hierarchical structure, which includes, for example, a structure in which nano-sized microvoids exist, and a connected cell structure formed by aggregation of the nanovoids. In the case of forming a monolithic structure, for example, fine voids can be used to impart membrane strength, and coarse connected cell voids can be used to impart high porosity, thereby taking into account both membrane strength and high porosity.

[0069] The transparent porous membrane may be preferably a nanoporous membrane (specifically, a membrane in which 90% or more of the micropores have a diameter of 10 -1 nm~10 3 nm range of transparent porous film).

[0070] The porosity of the transparent porous film is, for example, more than 10% by volume, preferably more than 20% by volume, more preferably more than 30% by volume, more preferably more than 35% by volume, for example, less than 60% by volume, preferably less than 55% by volume, more preferably less than 50% by volume, and more preferably less than 45% by volume. If the porosity is in such a range, the refractive index of the transparent porous film can be brought into an appropriate range, and a given mechanical strength can be ensured. The porosity is a value obtained by calculating the porosity using the value of the refractive index measured by an ellipsometer according to the Lorentz-Lorenz's formula (Lorentz-Lorenz equation).

[0071] The size of the void (hole) in the transparent porous film refers to the diameter of the major axis of the void (hole) and the diameter of the minor axis. The size of the void (hole) is, for example, 2nm~500nm. The size of the void (hole) is, for example, more than 2nm, preferably more than 5nm, more preferably more than 10nm, and more preferably more than 20nm. On the other hand, the size of the void (hole) is, for example, less than 500nm, preferably less than 200nm, and more preferably less than 100nm. The range of the size of the void (hole) is, for example, 2nm~500nm, preferably 5nm~500nm, more preferably 10nm~200nm, and more preferably 20nm~100nm. The size of the void (hole) can be adjusted to the desired size according to the purpose and use. The size of the void (hole) can be quantified by the BET test method.

[0072] The size of the voids (pores) can be quantified by the BET test method. Specifically, after 0.1 g of the sample (the void layer formed) is put into the capillary of the specific surface area measuring device (made by MacMeretic: ASAP2020), the gas in the void structure is degassed by drying under reduced pressure at room temperature for 24 hours. Then, the adsorption isotherm is drawn by adsorbing nitrogen on the above sample to obtain the pore distribution. In this way, the void size can be evaluated.

[0073] The refractive index of the transparent porous film is, for example, 1.25 or less, preferably less than 1.20, more preferably 1.19 or less, further preferably 1.18 or less, and typically 1.10 or more. Unless otherwise specified, the refractive index refers to the refractive index measured at a wavelength of 550 nm.

[0074] The total light transmittance of the transparent porous film is, for example, 85% to 99%, preferably 87% to 98%, and more preferably 89% to 97%. The haze of the transparent porous film is, for example, less than 5%, preferably less than 3%, and more preferably less than 1%. On the other hand, the haze is, for example, more than 0.1%. The haze can be measured, for example, by the method described below.

[0075] The transparent porous film was cut into a size of 50 mm×50 mm, and the haze was measured by using a haze meter (HM-150 manufactured by Murakami Color Research Laboratory Co., Ltd.). The haze value was calculated by the following formula.

[0076] Haze (%) = [Diffused light transmittance (%) / Total light transmittance (%)] × 100 (%)

[0077] The thickness of the transparent porous film is, for example, 30 nm to 5 μm, preferably 200 nm to 4 μm, more preferably 400 nm to 3 μm, and further preferably 600 nm to 2 μm. If the thickness of the transparent porous film is within this range, the transparent porous film can effectively reflect light in the visible to infrared region.

[0078] Hereinafter, an example of a specific structure of a transparent porous film will be described. The transparent porous film of the present embodiment comprises one or more structural units forming a fine void structure, and the structural units are chemically bonded together by the action of a catalyst. As the shape of the structural unit, for example, there can be cited: particle-shaped, fibrous, rod-shaped, and flat-plate-shaped. The structural unit may have only one shape, or may have a combination of two or more shapes. Hereinafter, the case where the transparent porous film is a void layer of a porous body in which the above-mentioned particles are chemically bonded together will be mainly described.

[0079] Such a transparent porous film can be formed by, for example, chemically bonding the particles to each other in the above-mentioned drying process. In one embodiment, the transparent porous film comprises a pulverized product of a gel-like compound, and the pulverized products are chemically bonded to each other. The form of the chemical bonding (chemical bond) between the pulverized products in the transparent porous film is not particularly limited, and examples thereof include cross-linking bonds, covalent bonds, and hydrogen bonds. In the case of using a pulverized product of a gel-like silicon compound, since the particles have a three-dimensional tree-like structure, the tree-like particles will settle and deposit in the coating (a coating of a sol containing the pulverized product of the gel-like silicon compound), thereby being able to easily form a connected bubble structure. In addition, in such a transparent porous film, by, for example, controlling the particle size distribution of the pulverized particles to a desired size when the gel-like silicon compound is pulverized, an integral structure can be formed.

[0080] In addition, in the transparent porous film (void layer), for example, the silicon atoms contained preferably form siloxane bonds. As a specific example, the proportion of unbonded silicon atoms (i.e., residual silanol) in all silicon atoms contained in the void layer is, for example, less than 50%, preferably less than 30%, and more preferably less than 15%.

[0081] Example

[0082] Hereinafter, the present invention will be specifically described in conjunction with the embodiments, but the present invention is not limited to these embodiments. It should be noted that the measuring method of each characteristic is as follows. In addition, as long as there is no special clear record, the "%" and "part" in the embodiments are mass references.

[0083] (1) Whether it can be ejected

[0084] The transparent porous forming coating obtained in each example and each comparative example and the alkali-free glass as a substrate were placed in a spray coater (manufactured by APEIROS CO., LTD., product name API-240). The distance between the spray head (nozzle) and the alkali-free glass was 100 mm.

[0085] Next, the transparent porous forming coating material was sprayed onto the alkali-free glass under the coating conditions of an atomization pressure of 100 kPa and a coating amount of 7 mL / min. The spraying performance was evaluated according to the following criteria. The results are shown in Table 1.

[0086] ○: Fogging of the transparent porous forming coating material was confirmed by visual observation.

[0087] ×: The clouding of the transparent porous forming coating material cannot be confirmed by visual observation.

[0088] Table 1 shows the haze of the obtained transparent porous film.

[0089] [Examples 1 to 6 and Comparative Examples 1, 2]

[0090] (1) Gelation of silicon compounds

[0091] 0.95 g of methyltrimethoxysilane (MTMS), a precursor of a silicon compound, was dissolved in 2.2 g of dimethyl sulfoxide (DMSO) to prepare a mixed solution A. 0.5 g of a 0.01 mol / L aqueous oxalic acid solution was added to the mixed solution A, and the mixture was stirred at room temperature (23° C.) for 30 minutes to hydrolyze MTMS, thereby generating a mixed solution B containing tri(hydroxy)methylsilane.

[0092] To 5.5 g of DMSO were added 0.38 g of 28 mass % ammonia water and 0.2 g of pure water, the mixed solution B was further added, and the mixture was stirred at room temperature (23° C.) for 15 minutes to gel tri(hydroxy)methylsilane, thereby obtaining a mixed solution C containing a gel-like silicon compound.

[0093] (2) Aging treatment

[0094] The mixed solution C containing the gel-like silicon compound prepared as described above was incubated at 40° C. for 20 hours to perform an aging treatment.

[0095] (3) Crushing

[0096] Next, the gel-like silicon compound (the pulverized material) that has been aged as described above is subjected to a pulverization treatment (high-pressure medium-free pulverization). The pulverization treatment (high-pressure medium-free pulverization) is performed using a homogenizer (manufactured by SMT Co., Ltd., trade name "UH-50"), and 1.85 g of the gel-like compound and 1.15 g of IPA in the mixed solution D are weighed in a 5 cc screw bottle, and then pulverized for 2 minutes under the conditions of 50 W and 20 kHz.

[0097] The gel-like silicon compound in the mixed solution C is pulverized by the pulverization treatment, whereby the mixed solution C becomes a sol solution D of the pulverized product (porous particles of the silicon compound).

[0098] Next, the dispersion medium shown in Table 1 was added to the sol solution D of the pulverized product, and after gentle stirring, the solution was left to stand at room temperature for 6 hours to decant the dispersion medium and catalyst in the gel. The same decantation treatment was repeated three times to perform solvent replacement.

[0099] Through the above operation, a transparent porous coating was obtained. The concentration of the pulverized material in the coating (particle concentration) is shown in Table 1. The volume average particle size, which characterizes the particle size deviation of the pulverized material contained in the coating, was confirmed by a dynamic light scattering nano-tracking particle size analyzer (manufactured by Nikkiso Co., Ltd., UPA-EX150 model), and the result was 0.50~0.70.

[0100]

[0101] It should be noted that the details of the abbreviations in the table are as follows.

[0102] IBA: Isobutyl alcohol, manufactured by Tokyo Chemical Industry Co., Ltd.

[0103] EDM: Diethylene glycol ethyl methyl ether, manufactured by Toho Chemical Industry Co., Ltd.

[0104] EMEA: Ethylene glycol monoethyl ether acetate, manufactured by Tokyo Chemical Industry Co., Ltd.

[0105] As is clear from Table 1, according to the embodiments of the present invention, by making the dispersion medium contain a first dispersion medium having a boiling point of 150° C. or higher and adjusting the particle concentration in the coating to 6% by mass or less, spray coating can be performed and a transparent porous film with low haze and excellent appearance can be achieved.

[0106] Industrial Applicability

[0107] The transparent porous-forming coating material according to the embodiment of the present invention can be suitably used for producing a transparent porous film used in various optical products.

Claims

1. A transparent porous coating material, comprising: Particles, and a dispersion medium in which the particles are dispersed, The concentration of the particles in the transparent porous forming coating is 0.1 mass % to 6.0 mass %, The dispersion medium includes a first dispersion medium having a boiling point of 150° C. or higher.

2. The transparent porous forming coating material according to claim 1, wherein The content ratio of the first dispersion medium in the dispersion medium is 3 mass % to 100 mass %.

3. The transparent porous forming coating material according to claim 1 or 2, wherein: The particles are porous particles of silicon compound.

4. A method for producing a transparent porous coating, the method comprising: A step of pulverizing a pulverized material in a hydrophilic medium to prepare a sol solution in which particles are dispersed; and A step of replacing the hydrophilic medium contained in the sol liquid with a dispersion medium including a first dispersion medium having a boiling point of 150° C. or higher, and adjusting the concentration of the particles to 0.1% by mass to 6.0% by mass.

Citation Information

Patent Citations

  • Antireflection film, polarizer and display device

    JP2012189802A

  • Antireflection film, manufacturing method thereof, polarizer, and image display device

    JP2013254183A

  • Coating material and method for producing the same

    JP2017025277A

  • Antireflective film

    WO2004113966A1

  • Low refractive index composition

    CN101501130A