Process for converting lignocellulosic material to organic liquefaction products

By using amorphous unsupported nickel sulfide-molybdenum catalyst to treat lignocellulose at low temperature, the problems of high oxygen content and spontaneous reaction in thermochemical methods are solved, and low oxygen content and stable organic liquefied products are generated, which is suitable for co-processing of refineries in oil refineries. , reducing energy consumption and corrosion risks.

CN118891344AInactive Publication Date: 2024-11-01RISE RES INST OF SWEDEN AB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028421.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-17
Filing Date
2023-03-17
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the existing thermochemical methods convert solid lignocellulose into liquefied products, there are problems such as high oxygen content, spontaneous reactivity, carbon formation and high volatile organic components loss, resulting in low carbon yield of hydrocarbon fuel components. Moreover, bio-oil is corrosive and unstable to refinery equipment and is difficult to process in standard refineries.

Method used

Amorphous unsupported nickel sulfide-molybdenum catalyst is used to mix with lignocellulose starting material, and subject to hydrogen, elevated pressure and temperatures from 270°C to 350°C to generate organic liquefied products, avoiding high energy consumption and high energy consumption of high temperature hydrocracking and High oxygen content.

Benefits of technology

Generate organic liquefied products at low temperatures, reducing solid residues and energy consumption, improving the thermal stability and storage safety of the products, reducing oxygen content and acidity, reducing corrosion risks, and improving the formation of hydrocarbon terminal products efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891344A_ABST
    Figure CN118891344A_ABST
Patent Text Reader

Abstract

In a hydroliquefaction process by subjecting a mixture of a lignocellulosic starting material, an amorphous non-supported nickel sulfide-molybdenum catalyst and a co-feed to not less than stoichiometric amount of hydrogen, elevated pressure, and a temperature in the range of 270 DEG C to up to but not including 350 DEG C, the lignocellulosic starting material may be converted to an organic liquefaction product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to novel methods for converting solid lignocellulosic raw materials into organic liquefied products. Background Art

[0002] It is well known that thermochemical processes, such as pyrolysis and hydrothermal liquefaction (HTL), can depolymerize whole lignocellulosic biomass as well as lignocellulosic biomass fractions, such as kraft lignin and other renewable side streams, from agriculture, forestry and the paper and pulp industry, typically producing liquefied products collectively referred to as “bio-oil” or “bio-crude.” These liquefied products can then be further upgraded using hydrotreating and hydrocracking technologies, which are more or less similar to those used in refineries to upgrade fossil crude oils and their distillates to obtain hydrocarbon mixtures that can be used, for example, as components of transportation fuels.

[0003] Problems frequently encountered in the thermochemical liquefaction (pyrolysis or HTL) of biomass include, for example, relatively high oxygen contents and the spontaneously reactive nature of the resulting depolymerization product mixtures, which contain, inter alia, molecules of different structural classes, such as reactive phenol derivatives in combination with aldehydes and ketones, which together lead to more or less severe repolymerization during storage and / or heating. Other problems are, for example, char formation and losses of highly volatile organic components, which ultimately lead to lower than desired carbon yields of hydrocarbon fuel components after upgrading.

[0004] The high water content combined with the acidic nature of thermochemical bio-oils creates a situation where these bio-oils are highly corrosive to standard construction materials used in refinery upgrading equipment. Using data as an example, pyrolytic conversion of lignocellulosic materials results in oxygen contents in the condensable fraction in the range of 20%->40%. Due to the high content of carboxylic acids and water, the pH of the aforementioned condensable fraction is generally about 2-3. Overall, this means that the total oxygen content and water content are not significantly lower than the more stable non-depolymerized, dried but not otherwise treated, and significantly less acidic lignocellulosic biomass.

[0005] In summary, although the goal of obtaining pumpable liquid bio-oil is generally achieved, the bio-oil or bio-crude products produced by pyrolysis or HTL are corrosive and unstable to storage and heating due to problems with spontaneous repolymerization. In addition, these products show poor miscibility or immiscibility with fossil feedstocks or other renewable feedstocks of interest for easy and flexible co-processing in current standard refinery infrastructure. These properties are obviously problematic when developing practical and robust full-scale processes for directly converting pyrolysis and / or HTL bio-oils into hydrocarbon transportation fuels and chemicals, either alone or by co-processing.

[0006] Typical conditions used in hydroprocessing are above 400°C and pressures of about 180 bar [Reference: Refiningprocesses handbook, Surinder Parkash, 2003 Gulf Professional Publishing, Elsevier]. In addition, prior art using NiMo catalysts to liquefy biomass (Reference: Burton et al 1986, "Catalytic Hydroliquefaction of Lignocellulosic Biomass", International Journal of Solar Energy) has used a temperature of 400°C and tetralin as a co-feed, which is an efficient hydrogen donor solvent, to promote the liquefaction of biomass.

[0007] In short, a simple and robust process of improvement is needed, which can be applied to commercially relevant selections of lignocellulosic raw materials and is suitable for upgrading. From the following description of the summary of the invention and the specific embodiments, these and other purposes will be more easily understood. It will be appreciated by those skilled in the art that one or more aspects can satisfy some purposes, while one or more other aspects can satisfy other purposes. Summary of the invention

[0008] The present disclosure provides a novel hydroliquefaction process that can be performed at unexpectedly low temperatures. According to the present disclosure, a method for converting a lignocellulosic starting material into an organic liquefied product is characterized in that a lignocellulosic starting material, an amorphous non-supported nickel-molybdenum sulfide catalyst, and a co-feed are mixed to obtain a mixture, and the mixture is subjected to a stoichiometric amount of hydrogen, an elevated pressure, and a temperature in the range of 270°C to up to but not including 350°C to produce an organic liquefied product.

[0009] The method according to the present disclosure is a hydroliquefaction method, which converts lignocellulosic biomass into an organic liquefied product, which can, for example, be subsequently converted into fuel or used in the production of chemicals. The advantage of the method according to the present disclosure is that it can be carried out at surprisingly low temperatures and the solid residue is surprisingly low, thus having advantages in reducing energy consumption, thereby giving rise to potential cost benefits. In the hydroliquefaction method of the present invention, the ash-free solid residue from the lignocellulosic starting material is less than 15% by weight, preferably less than 10% by weight, and most preferably less than 5% by weight.

[0010] Another advantage is that the organic liquefied product, which can be an intermediate product intended to be further converted into one or more final products, has a low oxygen content, which makes the organic liquefied product a more thermally stable intermediate product and stable for storage. In addition, based on the 31P-NMR product, the product has a low acidity and contains <0.5mmol / g or preferably <0.4mmol / g of carboxylic acid groups, thus resulting in less corrosion risk.

[0011] The organic liquefied product additionally exhibits improved physical properties, providing process benefits in subsequent process steps, such as during pumping at ambient or elevated temperatures. In addition, due to its low oxygen content, the intermediate organic liquefied product obtained can also be more easily integrated as a feedstock into conventional refineries.

[0012] Another advantage is that the low oxygen content in the organic liquefied product obtained by the process according to the present disclosure enables a reduced exotherm during complete hydrodeoxygenation to form hydrocarbon end products.

[0013] An important advantage of the catalyst being an unsupported catalyst without a carrier is that it can be added at different stages of the process, for example after the starting materials have been ground and thereby intimately mixed with the starting materials.

[0014] The temperature may be in the range of 270° C. to 349° C. The temperature may be in the range of 300° C. to up to but not including 350° C., preferably the temperature may be in the range of 310° C. to up to but not including 350° C., more preferably the temperature may be in the range of 320° C. to up to but not including 350° C.

[0015] The term "elevated pressure" refers to pressures above atmospheric pressure.

[0016] The operating pressure may be in the range of 50 bar to 300 bar. This may improve and accelerate the liquefaction process carried out within the temperature range of the method. Preferably, the pressure may be in the range of 70 bar to 170 bar, more preferably 80 bar to 150 bar.

[0017] The mole fraction of sulfur (S) relative to the mole fraction of molybdenum (Mo) in the amorphous non-supported sulfided nickel-molybdenum catalyst can be 0.1 to 2.3. The inventors have surprisingly found that the amorphous non-supported catalyst disclosed herein is capable of liquefying lignocellulosic starting materials at temperatures significantly lower than conventional hydrocracking processes. Typical hydrocracking temperatures for fossil feedstocks are about 413°C to 440°C and pressures of about 180 bar [Reference: Refining processes handbook, Surinder Parkash, 2003 Gulf Professional Publishing, Elsevier].

[0018] In an embodiment, the mole fraction of sulfur (S) is 0.3 to 2.29. The mole fraction of sulfur may also be 0.1 to 1.0, alternatively 0.3 to 0.99, such as 0.5 to 0.95.

[0019] The molar fraction of nickel (Ni) in the amorphous non-supported sulfided nickel-molybdenum catalyst relative to the molar fraction of molybdenum (Mo) may be 0.1 to 0.3. The molar fraction of nickel (Ni) in the amorphous non-supported sulfided nickel-molybdenum catalyst relative to the molar fraction of molybdenum (Mo) may be 0.1 to 0.2.

[0020] Preferably, the catalyst is introduced into the mixture of lignocellulosic starting materials in the form of a slurry of catalyst particles in a liquid co-feed, optionally the liquid co-feed is a pure liquid or a mixture of different liquid components.The liquid co-feed may be a hydrocarbon co-feed.

[0021] The catalyst may be substantially amorphous as determined by X-ray powder diffraction analysis and optical microscopy using polarized light. Alternatively, the catalyst is amorphous as determined by X-ray powder diffraction analysis.

[0022] The difference between amorphous and crystalline materials, as determined by X-ray powder diffraction analysis, is that crystalline materials produce sharp peaks in the XRD pattern, while amorphous materials do not produce any sharp peaks in the XRD pattern. Therefore, an amorphous catalyst will not produce any sharp peaks in the XRD pattern, as determined by X-ray powder diffraction analysis.

[0023] The catalyst may have a particle size distribution with a median value in the range of 1 μm to 200 μm as determined by laser diffraction.

[0024] The mixture may be subjected to the range of elevated pressure and temperature in accordance with the present disclosure for a period of at least 30 minutes, optionally within a range of 30 minutes to 360 minutes.

[0025] The co-feed is a liquid co-feed and may be selected from vegetable oils and fats, such as tall oil and tall oil pitch, pyrolysis oils, HTL oils, animal fats, fatty acids, fossil or renewable liquid hydrocarbons, and / or recycled or recovered products or product fractions obtained in the process.

[0026] The co-feed may be, but is not limited to, a mixture of vegetable oils, and / or animal fats, and / or pure or mixed fossil or renewable hydrocarbons. The co-feed may be, for example, a paraffin co-feed.

[0027] An advantage of the process according to the present disclosure is that various co-feeds can be used and the process does not require the use of a hydrogen donor solvent having an aromatic and / or cyclic structure as a co-feed. The co-feed may be, for example, a paraffin co-feed.

[0028] Thus, the co-feed may include a solvent other than the hydrogen donor solvent having an aromatic and / or cyclic structure.

[0029] The co-feed may alternatively and further may be substantially free of tetralin, i.e., such that at least 99% of the co-feed is free of tetralin or at least 99.5% of the co-feed is free of tetralin. When the co-feed is substantially free of tetralin, this means that tetralin is not added as a co-feed during the method, but a small amount of tetralin residue may be formed during the method. Alternatively, the co-feed is free of tetralin. The fact that the method can be carried out with a co-feed substantially free of or free of tetralin enables the use of cheaper, conventional and easily available refinery feedstocks or the use of recycled products or fractions of products, thus providing flexibility for the selection of the co-feed, because the co-feed does not need to have a strong hydrogen supply capacity to obtain a high conversion of the solid lignocellulose starting material.

[0030] The lignocellulosic starting material may have a dry content of greater than 50 wt%, preferably in the range of 70-95 wt%, most preferably in the range of 80-92 wt%.

[0031] The lignocellulosic starting material can be selected from wood chips and / or sawdust; forestry residues selected from bark and / or roots; wood that has undergone a drying or torrefaction process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn stover, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight of lignocellulosic material; and mixtures thereof.

[0032] The lignocellulosic starting material may not be subjected to thermochemical treatment, such as pyrolysis or hydrothermal liquefaction, prior to being subjected to the process. Thus, a more simplified process may be achieved.

[0033] The organic liquefaction product may have an oxygen content lower than the feed (including co-feed), optionally, the organic liquefaction product may have an oxygen content at least 5 wt% lower than the feed (including co-feed), for example at least 10 wt% lower than the feed, i.e., the lignocellulosic starting material and the co-feed.

[0034] The total feed may consist of 5 to 90 wt % solid biomass, preferably 10 to 80 wt % solid biomass. The total feed may consist of 60 to 80 wt % solid biomass, or alternatively 10 to 35 wt % solid biomass. This means that the liquid content is 10 wt %, preferably up to 65 wt %, which may provide process advantages, such as a pumpable slurry.

[0035] The process may or may not be divided into two or more hydrotreatment reactors with a flat or increasing temperature profile.Thus, the process may comprise at least a second conversion step after the first hydrotreatment step.

[0036] In the second hydroprocessing reactor, the operating temperature may be in the range of 270° C. to 450° C. Alternatively, in the second hydroprocessing reactor, the operating temperature may be 350° C. or higher, such as in the range of 350° C. to 450° C.

[0037] Alternatively, in the second hydroprocessing reactor, the operating temperature may be in the range of 270°C up to but not including 350°C.

[0038] In a preferred embodiment, the hydroprocessing is carried out in two or more reactors in series, wherein each subsequent reactor is operated at a higher temperature than the first reactor. Preferably, the method is carried out using two reactors in series, and the temperature of the first reactor is selected from the range of 270°C to up to but not including 350°C, and the temperature of the second reactor is selected from the range of 340°C to 400°C. Alternatively, the method is carried out using three reactors in series, and the temperature of the first reactor is selected from the range of 270°C to up to but not including 350°C, the temperature of the second reactor is selected from the range of 340°C to 400°C, and the temperature of the third reactor is selected from the range of 380°C to 400°C.

[0039] According to another aspect, the present disclosure relates to an organic liquefaction product derived from lignocellulosic biomass and obtained from a process as disclosed herein, the organic liquefaction product having an oxygen content in the range of 0.5 wt. % to 35 wt. %, as determined by elemental analysis.

[0040] The inventors have found that, based on dry content, the oxygen content of the lignocellulosic biomass is reduced by at least 40%, preferably at least 50% or most preferably at least 60% when liquefied into an organic liquefied product (here including dodecane and THF soluble parts). This can be seen in the examples, where the oxygen reduction of the organic liquefied product is between 66% and 90% compared to dry lignocellulosic biomass.

[0041] In one embodiment, the organic liquefied product can form two phases: a dodecane soluble phase and a THF soluble phase. The THF soluble phase can account for 1%-80% of the liquefied biomass, preferably 5%-70%. The THF soluble phase is characterized by having 2mol%-50mol% of aromatic substances characterized by 1H-NMR. The THF soluble phase can also be characterized by phenolic OH content, and the phenolic OH content measured by 31P-NMR is 0.01mmol / g-20mmol / g, or preferably 0.1mmol / g-10mmol / g. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Various aspects and embodiments will now be described by way of example with reference to the accompanying drawings, in which:

[0043] Figure 1 shows the XRPD diffraction pattern of the catalyst prepared according to Example 1;

[0044] Figure 2 shows a graph representing the particle size distribution of the catalyst obtained in Example 1;

[0045] Figure 3 shows the TGA data of the organic liquid product phase of Example 2;

[0046] Figure 4 shows the TGA data of the THF-soluble liquefied phase of Example 2;

[0047] Figure 5 shows the TGA data of the THF-soluble liquefied phase of Example 3;

[0048] Figure 6 shows the TGA data of the THF-soluble liquefied phase of Example 3;

[0049] Figure 7 shows the particle size distribution of the catalyst according to Example 4;

[0050] Figure 8 shows the TGA data of the organic liquid product phase of Example 5;

[0051] Fig. 9 TGA data for the THF-soluble liquefied phase of Example 5 is shown. DETAILED DESCRIPTION

[0052] When studying the specific embodiments, it should be understood that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting, since the scope of the aspects and embodiments of the present application will be limited only by the appended claims and their equivalents.

[0053] It must be noted that, as used in this specification and the appended claims, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.

[0054] The terms "lignocellulosic material", "lignocellulosic starting material" and "lignocellulosic feedstock" are used herein to cover all integral non-fractionated lignocellulosic materials consisting essentially of cellulose, hemicellulose and lignin. Depending on the geographical location, different materials are available, such as agricultural residues (e.g. corn stover, crop straw and bagasse), herbaceous crops (e.g. alfalfa, switchgrass), softwood and hardwood, short rotation woody plants, preheated and / or toasted wood, forestry residues (bark as well as branches, roots and tops) and other waste materials (e.g. urban and industrial waste containing whole lignocellulosic biomass, such as waste wood for the construction industry and / or cargo packaging). The inventors have tested pine sawdust with various dry matter contents, ground spruce roots and branches, fresh spruce needles, fresh pine bark and ground urban waste containing wood, plastics, sand, metals and paint residues.

[0055] The terms "unsupported" and "carrier-free" are used to define catalyst materials, such as sulfided NiMo catalysts, that are not deposited on any solid support or carrier material.

[0056] The fact that the catalyst is "amorphous" means that the catalyst is amorphous over its entire surface or at least over a major part of the catalyst surface.

[0057] The obtained organic liquefied product may be liquid at room temperature to at most 500° C. The organic liquefied product may include one or more organic liquid phases.

[0058] The term "solid residue" herein refers to the remaining solids separated from the organic liquefaction product after hydroliquefaction of lignocellulose, as exemplified in the experimental examples hereinafter.

[0059] According to the present disclosure, a process for converting a lignocellulosic starting material into an organic liquefied product is characterized in that a lignocellulosic starting material from a single source or from a mixture associated with the starting material, an amorphous non-supported nickel-molybdenum sulfide catalyst, and a co-feed are mixed and subjected to not less than a stoichiometric amount of hydrogen, elevated pressure, and a temperature in the range of 270° C. to up to but not including 350° C., thereby producing an organic liquefied product. The temperature may be in the range of 270° C. to 349° C.

[0060] Preferably, the catalyst is introduced into the mixture of lignocellulosic starting material in the form of a slurry of catalyst particles in a co-feed.

[0061] In the process there is a co-feed which may be selected from vegetable oils and fats, such as tall oil and tall oil pitch, pyrolysis oil, HTL oil, animal fats, fatty acids, fossil or renewable liquid hydrocarbons, and / or recycled or recovered products or product fractions obtained in the process.

[0062] The lignocellulosic starting material may have a dry content of greater than 50 wt%, preferably in the range of 70-95 wt%, most preferably in the range of 80-92 wt%.

[0063] The lignocellulosic starting material can be selected from wood chips and / or sawdust; forestry residues selected from tree bark and / or tree roots; wood that has undergone a drying or torrefaction process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn stover, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight of lignocellulosic material; and mixtures thereof.

[0064] With regard to materials that have been subjected to a drying or baking process, it is emphasized that baking is considered herein only as a drying step, ie the removal of moisture, and not as a proper thermochemical process.

[0065] According to another embodiment, which may also be freely combined with the above-mentioned aspects and embodiments, the lignocellulosic starting material has not been subjected to a thermochemical treatment, such as pyrolysis or hydrothermal liquefaction, before being subjected to the method.

[0066] According to another embodiment, which can also be freely combined with the above aspects and embodiments, the operating pressure can be in the range of 50 bar-300 bar. When the method is operated in batch mode, the initial pressure is set according to the available head space volume and in a manner to ensure a stoichiometric excess of hydrogen, for example, the initial pressure at ambient temperature is set to 120 bar and allowed to increase and stabilized at 150-300 bar, preferably 250 bar. When the method is operated in a continuous mode, the pressure is preferably set at 70 bar-170 bar, most preferably 80 bar-150 bar.

[0067] The process according to the present disclosure may be carried out in batch, semi-batch or continuous operation mode.

[0068] The lignocellulosic starting material may be subjected to mechanical pretreatment to simplify material handling and increase the area to volume ratio. Suitable pretreatment operations include milling, chipping and grinding. Starting materials of various particle sizes are suitable, for example a particle size of <25 mm, preferably <5 mm.

[0069] A mixture of lignocellulosic starting material, catalyst and liquid co-feed is fed into a reaction zone and subjected to elevated temperature and pressure, for example a temperature in the range of 270° C. up to but not including 350° C. and a pressure in the interval of 50 bar to 300 bar, preferably about 140 bar. The rate at which the material is conveyed through the reactor as well as the temperature and pressure can be adjusted depending on the properties of the starting material and the desired product.

[0070] Where the mixture is subjected to a temperature in the range of 270°C up to but not including 350°C and a pressure in the interval 50-300 bar, the reaction time may be 30 min or more, optionally in the range of 30 to 360 min.

[0071] Pressures in the range of 50-200 bar (5-20 MPa) and temperatures in the range of 270°C up to but not including 350°C are presently considered most suitable for hydroliquefaction and partial hydrodeoxygenation of lignocellulosic raw materials using the present or similar unsupported catalysts.

[0072] Unit operations such as mixing, conveying, gas-liquid, liquid-liquid and liquid-solid separations and equipment used to perform these unit operations, as well as the terminology used to describe and quantify the properties used in conjunction with these unit operations (e.g., heat transfer) are familiar to those skilled in the art, see, for example, textbooks such as Unit Operations of Chemical Engineering, Warren L. McCabe et al., 7th Ed., McGraw-Hill Professional, 2004.

[0073] The disclosure provides a kind of lignocellulosic biomass conversion organic liquefaction product, as the method for intermediate bio-oil or bio-crude oil, it can be used as transportation fuel, as gasoline, jet (jet), diesel or marine fuel after mixing or subsequent processing.Alternatively, the organic liquefaction product obtained can be used for petrochemical industry, for example as steam cracker raw material or as solvent.Under certain conditions, phenolic substances (phenol, cresol etc.) can be reclaimed from the organic liquefaction product and be used as the raw material of chemical and polymer industry.

[0074] Example

[0075] Analytical methods

[0076] The hydroxyl number for analyzing the amount of hydroxyl groups belonging to fatty alcohols (aliphatic OH), phenols (aromatic OH) and OH-groups of carboxylic acids is determined by the method described, for example, in L. Akim et al. Holzforschung 2001, 55, 386-390 using a Bruker Avance 500 UltraShield NMR spectrometer. 31 P-NMR was used. 1 H-NMR is used to characterize the relative amounts of protons that are part of the aromatic, aliphatic, ether / alcohol, aldehyde, ketone, carboxylic acid, and olefin functional groups of the resulting product mixture.

[0077] The boiling point range was determined using thermogravimetric analysis on a Mettler-Toledo TGA / SDTA851e instrument.

[0078] Use Malvern Mastersizer 2000 laser diffractometer to measure particle size distribution.Before measuring, the sample to be analyzed is dispersed in dodecane, and is measured as follows: fill the instrument slurry tank and measuring cell with 160mL dodecane, and exhaust air by stopping / starting stirring.Before sample extraction, the sample vial is vortexed for 1 minute.20-50 μL sample is taken out and transferred to the measuring cell with several smaller portions (5-10 μL) by pipette.After 1 minute of circulation, measurement is started.After the first measurement, the particle slurry is subjected to ultrasonic treatment for up to 4 minutes in the Malvern instrument.After ultrasonic treatment and exhausting air, the second measurement is carried out.

[0079] X-ray powder diffraction analysis (XRPD) was performed on a PANalytical X'Pert PRO spectrometer.

[0080] Example 1: Preparation of nickel-molybdenum slurry catalyst

[0081] 40g molybdenum trioxide, 59.7g 20% ​​(w / w) ammonium sulfide aqueous solution and 122g ultrapure water were added to a 1.8L pressure-resistant stainless steel container. After flushing with nitrogen, the reactor was pressurized to 26 bar with hydrogen. The reactor has been equipped with a blade impeller, which is set to a tip speed of 4-5m / s, and the reactor temperature is adjusted to 64°C-68°C and soaked at this temperature for 4 hours. After cooling to 40°C and decompressing the head space to atmospheric pressure, 301g dodecane is added, followed by 34.1g 36.2% (w / w) nickel sulfate (II) hexahydrate / heptahydrate solution. Nickel sulfate (II) hexahydrate / heptahydrate solution is added in 30min by a syringe pump at a maintained agitator speed. Reactor is pressurized to 18 bar using hydrogen, and heated to 210°C for 6 hours, then soaked at this temperature for another 1 hour. The reactor was cooled to 40°C within 2 hours, after which the pressure was released and the reactor was equipped with a water-cooled distillation head. A nitrogen ballast flow was added to the reactor at approximately 2 L / min, and the reactor temperature was increased at a rate of approximately 2 K / min. The process was continued until the water fraction was distilled, and then approximately 50% of dodecane was distilled. After cooling to room temperature, the reactor contents consisting of an activated nickel-molybdenum slurry catalyst in dodecane were poured into a glass beaker. The solid content of the slurry was found to be 23.4% (w / w). By correcting for the content and purity / content of each reagent, the empirical formula according to the above steps is MoNi 0.163 S 0.722 Elemental analysis shows that MoNi 0.171 S 0.860 .

[0082] Attached Figure 1 The XRPD diffractogram shown for the catalyst prepared according to Example 1 shows no XRPD peaks indicative of any crystallinity, leading to the conclusion that the catalyst according to Example 1 is amorphous.

[0083] Figure 1 The XRPD diffraction pattern of the catalyst prepared according to Example 1 is shown.

[0084] The particle size distribution data measured as described above are as follows Figure 2 The results show that the median particle size is 2 μm.

[0085] Figure 2 The particle size distribution of Example 1 is shown. d(0.1): 1 μm, d(0.5): 2 μm, d(0.9): 9 μm (ultrasonication for 4 minutes).

[0086] Example 2

[0087] Sawdust (10.01 g, dry matter content 91.5% w / w) <0.28 mm and catalyst slurry (3.21 g, content 23.4% w / w in dodecane) prepared according to Example 1 were mixed at room temperature in a high pressure reactor. Before the reactor was pressurized (119 bar) with hydrogen, an inert nitrogen atmosphere was established using a vacuum-nitrogen cycle. The reaction mixture was heated to 320° C. and maintained at this temperature for 120 minutes. The maximum operating pressure during the reaction was 239 bar. After cooling, decompression and establishing an inert atmosphere by vacuum-nitrogen circulation, the reactor contents were poured into a centrifuge vial and centrifuged at a rate of 2.9×10-3G for 20 minutes. The organic liquid phase, aqueous phase and solid residue phase were separated. Two portions of n-pentane (2×30 mL) and three portions of 30 mL of tetrahydrofuran (THF) were used to continuously wash the solid residue, reactor, lid and agitator. After each washing, the mixture was centrifuged and separated. The n-pentane wash phases were combined in a separate container and the THF wash phases were combined in another separate container before evaporation of the solvents (n-pentane and THF). After complete work-up of the pentane and THF phases, including drying, the following products were isolated: an organic liquid phase, which was combined with the contents of the n-pentane wash phase (1.77 g in total, 15% w / w based on the overall feed including dodecane), 2.6 g of an aqueous phase, 4.53 g of a THF-soluble liquefied phase and 0.901 g of a solid residue. 1 H-NMR and 31 P-NMR data are shown in Tables 1 and 2 below, and TGA data are shown in Figure 3 . THF-soluble liquefied phase 1 H-NMR and 31 P-NMR data are shown in Tables 3 and 4 below, and TGA data are shown in Figure 4 The NMR results indicate that the THF-soluble liquefied phase has a high oxygen content, which is confirmed by the elemental analysis data below. Despite the reaction temperature being lower than that typically used in hydroprocessing, the amount of unconverted solid material calculated on dry biomass was only 1.6% w / w. Considering the sawdust ash content of 0.6%, the amount of solid product is very low.

[0088] The TGA data of the THF-soluble liquefied phase show that 65%w / w of the THF-soluble liquefied phase is volatile below 500°C. Therefore, the total organic product yield based on dry biomass is 25%w / w. The yield calculation based on dry biomass does not include dodecane (2.46g) added to the reactor together with the catalyst. It is believed that dodecane is not converted in the method, so it can be subtracted from the organic product amount. The boiling point distribution of the entire organic product is shown in the following table 5.

[0089] Elemental analysis data of the organic liquid phase: C 82.3%, H 13.5%, N 0.2%, S 0.0%, O 2.8%, others 1.1%.

[0090] Elemental analysis data of the THF-soluble liquefied phase: C 77.8%, H 8.1%, N 0.62%, S 0.0%, O 12.8%, others 0.0%.

[0091] Table 1 below shows the organic liquid phase of Example 2. 1 H-NMR (CDCl3) results (normalized integration).

[0092]

[0093] Table 2 below shows the 31 The number of hydroxyl groups in the organic liquefied phase of Example 2 measured by P-NMR.

[0094]

[0095]

[0096] Figure 3 Shown are TGA data for the organic liquid product phase of Example 2. The dashed line represents the boiling point range of diesel.

[0097] Table 3 below shows the THF-soluble liquefied phase of Example 2. 1 H-NMR (DMSO-d6) results (normalized integration).

[0098]

[0099] Table 4 below shows the 31 The number of hydroxyl groups of the THF-soluble liquefied phase of Example 2 measured by P-NMR.

[0100]

[0101] Figure 4 TGA data for the THF-soluble liquefied phase of Example 2 is shown, with the dashed line indicating the boiling point range of diesel.

[0102] Table 5 below shows the boiling point distribution of the total organic products.

[0103]

[0104] Example 3

[0105] Sawdust <0.28 mm (10.17 g, dry matter content 91.5% w / w) and the catalyst slurry prepared according to Example 1 (3.56 g, content 23.4% w / w in dodecane) were mixed in a high-pressure reactor at room temperature. An inert nitrogen atmosphere was established using a vacuum-nitrogen cycle before the reactor was pressurized with hydrogen (118 bar). The reaction mixture was heated to 270°C and maintained at this temperature for 120 minutes. The maximum operating pressure during the reaction was 235 bar. After the work-up steps described in Example 2, 1.67 g of a dark amber organic liquid phase (yield 14% w / w calculated based on the overall feed including dodecane), 1.14 g of an aqueous phase, 6.02 g of a THF-soluble liquefied phase (yield 50%) and 1.14 g of a solid residue were separated. 1 H-NMR and 31 The P-NMR data are shown in Tables 6 and 7 below, and the TGA data are shown in Figure 5 . THF-soluble liquefied phase 1 H-NMR and 31 P-NMR data are shown in Tables 8 and 9 below, and TGA data are shown in Figure 6 The NMR results indicate that the THF-soluble liquefied phase has a high oxygen content, which is confirmed by the elemental analysis data below. Although the reaction temperature is significantly lower than that normally used in hydroprocessing, the amount of unconverted solid material calculated on dry biomass is only 3.4% w / w. Considering the sawdust ash content of 0.6%, the amount of solid product is low.

[0106] The TGA data of the THF-soluble liquefied phase show that 61%w / w of the THF-soluble liquefied phase is volatile below 500°C. Therefore, the total organic product yield based on dry biomass is 28%w / w. The yield calculation based on dry biomass does not include dodecane (2.46g) added to the reactor together with the catalyst. It is believed that dodecane is not converted in the method, so it can be subtracted from the organic product amount. The boiling point distribution of the entire organic product is shown in the following table 10.

[0107] Elemental analysis data of the organic liquid phase: C 81.9%, H 14.4%, N 0.0%, S 0.0%, O 1.9%, others 1.7%.

[0108] Elemental analysis data of the THF-soluble liquefied phase: C 69.9%, H 7.7%, N 0.54%, S 0.04%, O 20.6%, others 1.23%.

[0109] Table 6 below shows the organic liquid phase of Example 3. 1 H-NMR (CDCl3) results (normalized integration).

[0110]

[0111]

[0112] Table 7 below shows the 31 The number of hydroxyl groups in the organic liquefied phase of Example 3 measured by P-NMR.

[0113]

[0114] Figure 5 Shown are TGA data for the organic liquid product phase of Example 3. The dashed line represents the boiling point range of diesel.

[0115] Table 8 below shows the THF-soluble liquefied phase of Example 3. 1 H-NMR (DMSO-d6) results (normalized integration).

[0116]

[0117] Table 9 below shows the 31 The number of hydroxyl groups in the THF-soluble liquefied phase of Example 3 measured by P-NMR.

[0118]

[0119] Figure 6 Shown are TGA data for the THF-soluble liquefied phase of Example 3. The dashed line represents the boiling point range of diesel.

[0120] Table 10 below shows the boiling point distribution of the total organic products.

[0121]

[0122] Example 4: Preparation of Nickel-Molybdenum Slurry Catalyst - Second Example

[0123] Molybdenum (VI) oxide (250 g, 1.74 mol), deionized water (760 mL) and ammonium sulfide (20% w / w aqueous solution, 400 mL, 1.26 mol) were added to a two-gallon Parr high-pressure reactor equipped with a pitch blade mechanical stirrer. The reactor was closed and the reactor vessel was pressurized with nitrogen for leak testing. Formier gas (5% w / w hydrogen in nitrogen) was added continuously in a controlled manner using a capillary outlet to set the system pressure to 50 bar system pressure. The gas coming out of the reactor was bubbled through a hydrogen peroxide scrubber to capture and oxidize sulfur-containing waste gases. The reaction mixture was heated at 68 ° C for 4 h, then cooled to 38 ° C over 1 h, and the mixture was kept at 38 ° C for 2 h. Mixed nickel sulfate (II) hexahydrate and heptahydrate (86.9 g, 0.284 mol) dissolved in water (0.24 L) was added to the reactor, followed by dodecane (2.5 L).

[0124] The reaction mixture was then heated to 210°C over 6 hours, then maintained at this temperature for 1 hour and then cooled to room temperature over 3.5 hours. During the entire heating and cooling period, the Fourmier gas flow and pressure were maintained at 50 bar, which was bubbled through a hydrogen peroxide scrubber solution. The Fourmier gas flow was turned off and water was distilled from the reactor together with part of the dodecane at a jacket temperature of 190°C. The distillation continued for about 1.5 hours and the reactor was then allowed to cool overnight.

[0125] The reactor was opened and the catalyst particles located on the wall of the reactor vessel were scraped into the liquid slurry phase. Dimethyl disulfide (DMDS, 168 mL, 1.88 mol) was added, the reactor was closed and a leak test was performed. The reaction mixture was heated to 320°C over 1.5 hours and then maintained at this temperature for 4 hours before being cooled to room temperature overnight. The reactor was then flushed with nitrogen and the exhaust gas was allowed to enter the hydrogen peroxide scrubber. The obtained black slurry was transferred to a container and homogenized using a mechanical pitch paddle stirrer, and then four samples were collected to determine the slurry content. The average content of the four samples was 18.25% w / w NiMoS-catalyst in dodecane, and the total weight of the resulting slurry was 1.558 kg.

[0126] The particle size distribution of the catalyst batch was analyzed using a Malvern laser diffractometer as described above for the catalyst in Example 1. Figure 7 The data shown in show that the median particle size of the catalyst prepared according to Example 4 is 4 μm.

[0127] Figure 7 The particle size distribution of the NiMoS catalyst according to Example 4 is shown.

[0128] Example 5

[0129] Sawdust with a particle size distribution of <0.28 mm (20.0 g, dry matter content 91.5% w / w), the catalyst slurry prepared according to Example 4 (4.00 g, concentration in dodecane 18.25% w / w) and dodecane (35.3 mL) were mixed in a high-pressure reactor at room temperature. An inert nitrogen atmosphere was established using a vacuum-nitrogen cycle before the reactor was pressurized with hydrogen (140 bar). The reaction mixture was heated to 340° C. and maintained at this temperature for 120 minutes. The maximum operating pressure during the reaction was 270 bar. After the work-up steps described in Example 2, 33.8 g of a dark amber organic liquid phase (yield calculated based on the entire feed including dodecane was 67% w / w), 7.06 g of an aqueous phase, 3.62 g of a THF-soluble liquefied phase (yield 7.2%) and 1.02 g of a solid residue were separated. 1 H-NMR and 31 The P-NMR data are shown in Tables 11 and 12 below, and the TGA data are shown in Figure 8 . THF-soluble liquefied phase 1 H-NMR and 31 The P-NMR data are shown in Tables 13 and 14 below, and the TGA data are shown in Fig. 9 The NMR results indicated that the THF-soluble liquefied phase had a high oxygen content, which was confirmed by the elemental analysis data below. The amount of unconverted solid material calculated on dry biomass was 1.6% w / w.

[0130] The TGA data of the THF-soluble liquefied phase showed that 78% w / w of the THF-soluble liquefied phase was volatile below 500°C. Therefore, the total organic product yield based on dry biomass was 37% w / w. The yield calculation based on dry biomass does not include dodecane added to the reactor. It is believed that dodecane is not converted in the process and can therefore be subtracted from the amount of organic product. The boiling point distribution of the entire organic product is shown in Table 15 below.

[0131] Elemental analysis data of the organic liquid phase: C 84.3%, H 15.0%, N 0.0%, S 0.0%, O 1.08%, others 0.32%.

[0132] Elemental analysis data of the THF-soluble liquefied phase: C 79.5%, H 8.8%, N 0.39%, S 0.04%, O 9.4%, others 1.9%.

[0133] Table 11 below shows the organic liquid phase of Example 5. 1 H-NMR (CDCl3) results (normalized integration).

[0134]

[0135] Table 12 below shows the 31 The number of hydroxyl groups in the organic liquefied phase of Example 5 measured by P-NMR.

[0136]

[0137] Figure 8 Shown are TGA data for the organic liquid product phase of Example 5. The dashed line represents the boiling point range of diesel.

[0138] Table 13 below shows the THF-soluble liquefied phase of Example 5. 1 H-NMR (DMSO-d6) results (normalized integration).

[0139]

[0140] Table 14 below shows the 31 The number of hydroxyl groups of the THF-soluble liquefied phase of Example 5 measured by P-NMR.

[0141]

[0142]

[0143] Fig. 9 Shown are TGA data for the THF-soluble liquefied phase of Example 5. The dashed line represents the boiling point range of diesel.

[0144] Table 15 below shows the boiling point distribution of the total organic product of Example 5.

[0145]

Claims

1. A method for converting a lignocellulosic starting material into an organic liquefied product, characterized in that In a first hydroprocessing step, a lignocellulosic starting material, an amorphous non-supported nickel-molybdenum sulfide catalyst, and a co-feed are mixed to obtain a mixture, and the mixture is subjected to not less than a stoichiometric amount of hydrogen, an elevated pressure, and a temperature in the range of 270° C. to but not including 350° C. to produce an organic liquefied product.

2. The method according to claim 1, wherein: The mole fraction of sulfur (S) in the amorphous non-supported sulfided nickel-molybdenum catalyst relative to the mole fraction of molybdenum (Mo) is 0.1 to 2.

3.

3. The method according to claim 1 or 2, wherein: The mole fraction of nickel (Ni) in the amorphous non-supported sulfided nickel-molybdenum catalyst relative to the mole fraction of molybdenum (Mo) is 0.1 to 0.

3.

4. A method according to any one of the preceding claims, wherein: The catalyst is introduced into the mixture of lignocellulosic starting materials in the form of a slurry of catalyst particles in a liquid co-feed.

5. The method according to claim 4, wherein: The liquid co-feed is selected from vegetable oils and fats, tall oil, tall oil pitch, animal fats, fatty acids, pyrolysis oils, HTL oils, fossil or renewable liquid hydrocarbons, and / or recycled products or product fractions obtained in the process, and any mixtures thereof.

6. The method according to claim 5, wherein: The co-feed is a mixture of vegetable oils, and / or animal fats, and / or fossil or renewable hydrocarbons, such as diesel.

7. The method according to any one of claims 1 to 3, wherein: The total feed consists of 5 to 90 wt% solid biomass, preferably 10 to 80 wt% solid biomass.

8. The method according to claim 7, wherein: The total feed consists of 60 to 80 wt% solid biomass.

9. The method according to claim 7, wherein: The total feed consists of 10 to 35 wt% solid biomass.

10. A method according to any one of the preceding claims, wherein: The mixture is subjected to a pressure in the range of 50 to 300 bar.

11. A method according to any one of the preceding claims, wherein: The organic liquefaction product has a lower oxygen content than the feed including the co-feed, optionally, the organic liquefaction product has an oxygen content at least 5 wt% lower than the feed including the co-feed, for example at least 10 wt% lower than the feed.

12. A method according to any one of the preceding claims, wherein: The lignocellulosic starting material has a dry content of greater than 50 wt%, preferably in the range of 70 to 95 wt%, most preferably in the range of 80-92 wt%.

13. A method according to any one of the preceding claims, wherein: The lignocellulosic starting material is selected from wood chips and / or sawdust; forestry residues selected from bark, and / or roots, and / or branches; wood that has undergone a drying or roasting process; lignocellulose from agriculture, for example straw from crops such as oats, wheat, barley and rye, corn straw, grasses and herbs, fodder crops, oat husks, rice husks, construction waste containing at least 50% by weight of lignocellulosic substances; and mixtures thereof.

14. A method according to any one of the preceding claims, wherein: The lignocellulosic starting material has not been subjected to thermochemical treatment, such as pyrolysis or hydrothermal liquefaction, prior to being subjected to the process.

15. A method according to any one of the preceding claims, wherein: The process may or may not be divided into two or more hydroprocessing reactors with a flat or elevated temperature profile.

16. A method according to any one of the preceding claims, wherein: The catalyst was substantially amorphous as determined by X-ray powder diffraction analysis and optical microscopy using polarized light.

17. A method according to any one of the preceding claims, wherein: The catalyst has a particle size distribution with a median value in the range of 1-200 μm as determined by laser diffraction.

18. The organic liquefied product obtained according to any one of claims 1 to 17, the organic liquefied product having an oxygen content in the range of 0.5 wt% to 35 wt% as measured by elemental analysis.