Process for reducing hydrotreating catalyst deactivation
By adjusting the weight ratio of metal to phosphorus in renewable feedstock and treating it at high temperature, the problem of catalyst deactivation caused by low-quality feedstock was solved, the catalyst life was extended, and the frequency of production interruptions and economic costs were reduced.
Patent Information
- Application Number
- CN202380023548.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2023-04-05
- Publication Date
- 2024-11-01
AI Technical Summary
Existing technologies are insufficient to effectively reduce the impurity content in low-quality renewable feedstocks, leading to catalyst deactivation during hydrotreating, shortening catalyst life, increasing the frequency of production interruptions, and raising economic costs.
By adjusting the weight ratio of metal to phosphorus (M:P) in the renewable feedstock to the range of 0.70 to 1.26 and treating it at a temperature of 190°C to 400°C, a precipitate of metal and phosphorus compounds is formed, thereby reducing catalyst deactivation.
It extends the lifespan of the hydrotreating catalyst, reduces the frequency of production interruptions, lowers economic costs, and improves production efficiency.
Smart Images

Figure CN118891346A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing renewable hydrocarbons from renewable feedstocks. In particular, the method relates to reducing the deactivation of catalysts used in processing renewable hydrocarbons by hydroprocessing. Background Art
[0002] Currently, renewable hydrocarbons suitable for use as fuels, such as diesel fuel, aviation fuel and / or gasoline, are produced from renewable raw materials by hydroprocessing. The sources of renewable raw materials include, for example, oils or fats of plants, animals or fish, and nowadays even more and more waste and residues, such as waste oils or fats and side streams and waste from different process facilities. Depending on the feedstock, various reactions take place during hydroprocessing. Hydroprocessing reactions can include at least double bond hydrogenation, hydrodeoxygenation (HDO), hydrodesulfurization (HDS), denitrogenation (HDN), hydrodearomatization (HDA), hydrocracking (HC) and hydroisomerization.
[0003] Hydroprocessing reactions typically involve the use of hydroprocessing catalysts. Hydrodeoxygenation (i.e., oxygen removal) can be carried out in the presence of sulfided NiMo, CoMo, or CoNiMo catalysts on an alumina support, while hydroisomerization (i.e., branching of hydrocarbons) is typically carried out over bifunctional catalysts that have both a metal dehydrogenation function and an acidic function (e.g., a Pt or Pd catalyst in conjunction with a molecular sieve such as SAPO-11). These catalysts are often sensitive to impurities and tend to deactivate over time, as evidenced by a drop in hydroprocessing rates or eventual complete failure.
[0004] In the quest to improve feedstock sustainability and expand feedstock supply, lower quality feedstocks are used, such as waste and residual materials that contain several different types of contaminants or impurities.
[0005] It is well known that contaminants in renewable feedstocks, such as phosphorus and metals, can cause operational problems, especially in hydroprocessing. Some low-quality feedstocks, including biogenic lipids in particular, contain large amounts of impurities, such as metals (such as Fe, Ca, Na, and Mg), and phosphorus-containing compounds in various chemical forms. Typically, such feedstocks contain different types of impurities than feedstocks of fossil origin.
[0006] Although the amount of these impurities can usually be reduced by pretreatment techniques, it has so far been impossible to completely avoid fouling of hydroprocessing catalysts due to the inability to completely remove the impurities in industrial-scale operations. Catalyst fouling leads to increased deactivation rates and shortens the catalyst life and life cycle, which in turn has important economic consequences, as production eventually needs to be interrupted regularly in order to supply the process with catalyst material with sufficient activity.
[0007] For example, the accumulation of “phosphate glass” (i.e., recalcitrant phosphorus compounds) has been reported to cause pressure drop and accelerate catalyst deactivation. In addition, phosphorus is considered most likely to coat the outer surface of the catalyst and clog the pores. As catalyst particles begin to adhere to each other, the voids slowly fill up and the potential for pressure drop buildup increases. This is why it is important to specify a threshold value for the concentration of each contaminant allowed in the feedstock.
[0008] Therefore, there is a need to extend the life cycle of hydroprocessing catalysts by reducing deactivation when using low-quality renewable feedstocks. It is therefore an object of the present invention to provide a method for reducing the amount of harmful impurities in feedstocks involved in catalytic processes, these impurities in particular causing deactivation of hydroprocessing catalysts. Summary of the invention
[0009] It is an object of the present invention to provide a process which facilitates the use of low-quality renewable feedstocks in the production of hydrocarbons by hydroprocessing.
[0010] Another object of the present invention is to reduce the deactivation of the primary active hydroprocessing catalyst when using low quality renewable feedstocks in the production of hydrocarbons by hydroprocessing.
[0011] The invention is defined by the characterizing features of the independent claim. Some specific embodiments are defined in the dependent claims.
[0012] According to one aspect, there is provided a method for reducing deactivation of a hydroprocessing catalyst used as a primary active catalyst for producing renewable hydrocarbons from a renewable feedstock by hydroprocessing, the renewable feedstock comprising as impurities at least one oxygen-containing compound, at least one metal-containing compound and at least one phosphorus-containing compound, the method comprising the steps of:
[0013] i. adjusting the metal to phosphorus (M:P) weight ratio, measured as elemental metal and elemental phosphorus, of the renewable feedstock to a value in the range of 0.70 to 1.26 to obtain an impurity adjusted renewable feedstock, and
[0014] ii. subjecting the impurity-adjusted renewable feedstock to a temperature of 190°C to 400°C under reducing conditions, thereby forming a solid precipitate comprising at least one metal- and phosphorus-containing compound, and a purified liquid renewable feedstock, and
[0015] iii. contacting the purified liquid renewable feedstock with a primary active catalyst in the presence of hydrogen.
[0016] A typical solution proposed in the prior art is to enhance the purification of renewable raw materials to remove as many impurities as possible and to achieve the lowest possible impurity content. However, it is costly to fully purify the raw materials before they enter the catalytic process, which usually requires specific pretreatment methods and equipment. The purification problem becomes more obvious, difficult and costly when using waste and residual materials that contain large amounts of various impurities, especially so-called difficult-to-remove impurities. The term difficult-to-remove impurities refers to impurities that cannot be removed by the commonly applied pretreatment processes, usually impurities containing complex compounds with undesirable properties (such as solubility). Therefore, the higher the required purity level, the higher the cost rises.
[0017] In contrast, the present disclosure does not propose a solution based on minimizing the level of impurities in the feed. Instead, the present invention proposes adjusting the weight ratio of metal (M) and phosphorus (P) in the feed so that the impurities may be precipitated into a less harmful form (such as the main active catalyst) before reaching the critical part of the processing. Although the present disclosure does not claim to replace the known pretreatment purification technologies, it still provides a possibility to refine renewable raw materials with high impurity content without requiring a large investment in the development of known pretreatment technologies or equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The formation and identification of metal phosphate phases from an impurity-based dust sample from a batch of spent catalysts using X-ray diffraction (XRD) analysis are shown, where a) calcium iron phosphate and b) sodium iron phosphate are depicted.
[0019] Figure 2 The correlation of the impurity dust per unit weight ratio of primary active HDO catalyst to the weight ratio of metal (M) to phosphorus (P) in the feed is shown.
[0020] Figure 3 The correlation of the amount of phosphorus (P) present in the spent primary active catalyst (in weight-%) to the ratio of metal to phosphorus (M:P, on a weight basis) in the feed is shown. DETAILED DESCRIPTION
[0021] When describing the embodiments of the present disclosure, specific terms will be used for the sake of clarity. However, the present disclosure is not intended to be limited to the specific terms so selected, and it should be understood that each specific term includes all technical equivalents that operate in a similar manner to achieve similar purposes.
[0022] In this specification, weight percentages (wt-%) are calculated based on the total weight of the materials in question (usually a blend or mixture). Any amount defined as ppm (parts per million) is based on weight.
[0023] The term "renewable" in the context of renewable feedstock, renewable raw material or renewable fuel or fuel component refers to one or more organic compounds derived from any renewable source (as opposed to fossil origin). Thus, a renewable fuel component is based on renewable sources and therefore does not originate or derive from any fossil-based material. The term fuel is to be understood as both a fuel that can be used directly and a fuel component that meets the requirements of the corresponding usage standards. For example, within the EU, the standard for gasoline is EN 228 (2017), the standard for paraffin diesel is EN 15940 (2019) and the standard for aviation turbine fuel containing synthetic hydrocarbons is D7566 (2020).
[0024] 14 The C isotope content can be used as evidence of the renewable or biological origin of a raw material or product. Carbon atoms from renewable materials contain a greater amount of unstable radiocarbon ( 14 C) atoms. Therefore, by analyzing 12 C and 14 The ratio of C isotopes can distinguish carbon compounds derived from biological sources from carbon compounds derived from fossil sources. Therefore, the specific ratio of this isotope can be used to identify and quantify renewable carbon compounds and distinguish them from non-renewable energy (i.e., fossil carbon compounds). The isotope ratio does not change during chemical reactions. ASTM D6866 (2020) is an example of a suitable method for analyzing the carbon content of biological sources. The article by Dijs et al., Radiocarbon, 48(3), 2006, pp. 315-323 provides an example of how to apply ASTM D6866 to determine the renewable energy content in fuels. For the purposes of the present invention, if a carbonaceous material such as a feedstock or product contains 90% or more modern carbon (pMC) as measured using ASTM D6866, such as about 100% modern carbon, it is considered to be of renewable origin.
[0025] In the present disclosure, when discussing raw materials, unless otherwise specified, it refers to both the first raw material and the additional second raw material. In addition, in the present disclosure, "at least one" means that there are one or more of the mentioned items.
[0026] "Weight ratio" means the ratio of species a to species b, wherein the amounts of species a and species b are determined by weight (e.g., ppm (mg / kg)) in the raw materials using an appropriate method, such as inductively coupled plasma (ICP) or ICP coupled to atomic emission spectroscopy (ICP-AES) or tandem inductively coupled plasma mass spectrometry (ICP-MS / MS). The weight is calculated as the amount of the species in question in elemental form.
[0027] The renewable feedstock can be any type of animal, plant or fish material containing oxygen. The oxygen in the feedstock can be derived from, for example, triglycerides and / or free fatty acids in the feedstock material.
[0028] In one embodiment, the renewable feedstock of the present disclosure contains triglycerides, free fatty acids, or both.
[0029] More specifically, in one embodiment, the raw material is selected from:
[0030] - Vegetable fats, vegetable oils and vegetable waxes; animal fats, animal oils and animal waxes; fish fats, fish oils and fish waxes;
[0031] - fatty acids, bound or free, obtained from vegetable fats, vegetable oils, vegetable waxes; animal fats, animal oils, animal waxes; fish fats, fish oils, fish waxes obtained, for example, by hydrolysis, transesterification or pyrolysis, and mixtures thereof;
[0032] - esters obtained from vegetable fats, vegetable oils, vegetable waxes; animal fats, animal oils, animal waxes; fish fats, fish oils, fish waxes; and mixtures thereof obtained, for example, by transesterification;
[0033] - metal salts of fatty acids obtained from vegetable fats, vegetable oils, vegetable waxes; animal fats, animal oils, animal waxes; fish fats, fish oils, fish waxes obtained, for example, by saponification, and mixtures thereof;
[0034] - esters obtained by esterification of free fatty acids of plant, animal and fish origin with, for example, alcohols;
[0035] - fatty alcohols or aldehydes obtained as reduction products of fatty acids from vegetable fats, vegetable oils, vegetable waxes; animal fats, animal oils, animal waxes; fish fats, fish oils, fish waxes and mixtures thereof;
[0036] - Waste and residues, such as recycled food-grade fats and oils;
[0037] - Fats, oils and waxes obtained through genetic engineering;
[0038] - dicarboxylic acids or polyols, including diols, hydroxyketones, hydroxyaldehydes, hydroxycarboxylic acids and corresponding difunctional or polyfunctional sulfur compounds, corresponding difunctional or polyfunctional nitrogen compounds;
[0039] - Bio-based pyrolysis oil;
[0040] - compounds derived from algae or wood, and
[0041] - mixtures of any of the materials listed herein.
[0042] In one embodiment, the feedstock is based on non-edible oils or fats. In another embodiment, the feedstock comprises vegetable oils. In another embodiment, the vegetable oils are obtained as wood-based byproduct materials from forestry. According to a specific embodiment, the feedstock is selected from wastes and residues of animal fats or oils, vegetable fats or oils and fish fats or oils, and mixtures thereof.
[0043] Exemplary feedstocks include at least triglycerides. The most typical exemplary feedstocks are animal fats and palm oil fatty acids, especially those derived from waste and residues.
[0044] Another exemplary feedstock includes at least fatty acids. The most typical feedstocks are various vegetable oils, such as tall oil feedstocks, such as crude tall oil.
[0045] Natural fats and oils or their derivatives may be provided in pure form or may be provided as part of a feedstock containing other components. Preferably, the feedstock contains at least 20 wt-%, more preferably at least 30 wt-%, most preferably at least 40 wt-% pure natural fats or natural oils or their derivatives.
[0046] The raw materials may contain C8-C 24 Fatty acids, derivatives of the fatty acids, such as fatty acid esters and triglycerides of the fatty acids, metal salts of the fatty acids, or combinations thereof. Fatty acids or fatty acid derivatives (such as esters) can be produced by hydrolysis of bio-oil or by fractionation thereof, or by esterification of triglycerides.
[0047] The raw materials may also include derivatives of natural fats, including C 10 -C 28 Monoglycerides or diglycerides of fatty acids, C 10 -C 28 Fatty acids, non-glycerides C 10 -C 28 Fatty acid esters, C 10 -C 28 Fatty alcohol, C 10 -C 28 Fatty aldehydes and C 10 -C 28 Fatty ketones. C10-C28 fatty acids and their mono- and diglycerides are usually prepared by hydrolysis of the corresponding triglycerides. Non-glyceride C10-C28 fatty acid esters are mainly prepared from triglycerides by transesterification. C10-C28 fatty alcohols, aldehydes and ketones are prepared by reduction (usually by hydrogenation) of the corresponding fatty acids. Advantageously, the feed hydrocarbons may have C 10 -C 24 .
[0048] The raw materials may also be selected from the lauric-myristic acid group (C 12-C 14 ), including the palmitic acid group of terrestrial animal fats (C 16 ), including stearic acid groups of terrestrial animal fats (C 18 ), including the linoleic acid group of whale oil and fish oil (unsaturated C 18 ), including the erucic acid groups of whale oil and fish oil (unsaturated C 22 ), including liquid tallow stearic acid groups of whale oil and fish oil (conjugated unsaturated C 18 ), fats with substituted fatty acids (ricinoleic acid, C 18 ) such as castor oil, oils obtained from plants by genetic manipulation, and mixtures of any two or more thereof.
[0049] Derivatives of natural fats also include any of the above-mentioned natural fats and derivatives whose hydrocarbon chains have been modified, for example by substitution, branching or saturation.
[0050] Depending on the level of pretreatment and residual phosphorus and metal content, crude oil can be classified into crude oil, degummed oil, thermally treated oil and RBD (refined oil, bleached oil and deodorized oil) grades. Animal fats and / or oils can include inedible tallow (tallow), edible tallow, industrial tallow, flotation tallow, lard, poultry fat, poultry oil, fish fat, fish oil, and any two or more mixtures thereof. Grease can include yellow grease, brown grease (brown grease), waste vegetable oil, restaurant grease, grease trap grease from municipal facilities (such as water treatment facilities), waste oil from industrial packaged food operations, pyrolysis oil, and any two or more mixtures thereof.
[0051] According to one embodiment, the raw materials used in the present disclosure include at least one of animal fat, animal oil, vegetable fat, vegetable oil, fish fat, fish oil, microbial oil, algae oil, waste fat, waste oil, residual fat, residual oil, and sludge derived from vegetable oil production. If more than one or two or more raw materials are used, the above content may apply to all raw materials.
[0052] Low quality raw material in this context means raw material that is difficult to purify by known pretreatment or purification methods. Typically, it may include specific impurities that are difficult to remove and that are usually derived from waste and residual materials. On the other hand, some materials suitable as raw materials may inherently contain various impurities that are difficult to remove by conventional methods, or may simply be inherently rich in specific impurities.
[0053] In one embodiment, the triglycerides and / or free fatty acids are derived from a feedstock comprising acidulated soapstock, poultry fat, rendered poultry fat, brown grease, waste cooking oil, tall oil, tall oil fractions, crude tall oil, tall oil pitch, palm oil mill wastewater, crude palm oil, palm oil, palm kernel oil, palm fatty acid distillate, babassu oil, carinata oil, oil), coconut butter, musk butter, sesame oil, corn oil, poppy seed oil, cottonseed oil, soybean oil, laurel seed oil, jatropha oil, palm kernel oil, camellia oil, archaea oil, bacterial oil, fungal oil, protozoa oil, algae oil, algae oil, mustard oil, halophile oil, soybean oil, industrial corn oil, rapeseed oil, rapeseed oil, canola oil, sunflower oil, hemp seed oil, olive oil, linseed oil, mustard oil, peanut oil, castor oil, coconut oil, lard, tallow, whale oil, spent bleaching earth oil, lignocellulose-based feed or at least one of a mixture thereof.
[0054] According to another embodiment, the renewable feedstock and additional renewable feedstock(s) of the present disclosure include acidulated soap stock, (ASK), poultry fat, dried poultry fat (AFP), brown grease (BG), waste cooking oil (UCO), tall oil, tall oil fractions, crude tall oil (CTO), tall oil pitch (TOP), palm oil mill effluent (POME), crude palm oil (CPO), palm oil, palm kernel oil, palm fatty acid distillate (PFAD), babassu oil, carinata oil, coconut butter, musk butter, sesame oil, At least one of sesame oil, corn oil, poppy seed oil, cottonseed oil, soybean oil, bay seed oil, jatropha oil, palm kernel oil, camellia oil, archaea oil, bacterial oil, fungal oil, protozoa oil, algae oil, algae oil, mustard oil, halophile oil, soybean oil (SBO), industrial corn oil, rapeseed oil (RSO), rapeseed oil, canola oil, sunflower oil, hemp seed oil, olive oil, linseed oil, mustard oil, peanut oil, castor oil, coconut oil, lard, tallow, whale oil, spent clay oil (SBEO), lignocellulosic based feed or a mixture thereof.
[0055] A large amount of impurities may be present in renewable raw materials, including vegetable oils and animal fats containing biogenic lipids. Various possible renewable raw materials, especially when derived from, for example, waste and residue materials, may include very high amounts of impurities, particularly phosphorus or metals, or both. For example, acidified soapstock and poultry fat may contain 100-400 ppm of phosphorus, while some oils and fats derived from algae may have thousands of ppm of phosphorus. Brown grease generally has a phosphorus content lower than 100 ppm, while metal content may reach hundreds or thousands of ppm. In the method disclosed herein, low-quality raw materials initially having a high content of phosphorus and / or metals are preferably pretreated using conventional pretreatment methods to reduce the initial amount of impurities to a reasonable level. However, generally the level may not be low enough to be able to carry out subsequent hydroprocessing. The disclosure provides a method that can be processed using raw materials still containing excessive phosphorus and / or metals without shortening the life of the hydroprocessing catalyst.
[0056] The renewable feedstock of the present disclosure may initially comprise
[0057] - phosphorus in an amount of at least 50 ppm, or at least 100 ppm, or at least 200 ppm, or at least 300 ppm, or at least 400 ppm, or at least 500 ppm;
[0058] - at least one metal in an amount of at least 200 ppm, or at least 500 ppm, or at least 1000 ppm; or
[0059] - both phosphorus and at least one metal.
[0060] The metal generally comprises an alkali metal or an alkaline earth metal, and some transition metals such as Fe, Co, Ni or Cu. In one embodiment, the metal may be selected from Na, K, Mg, Ca, Fe, Cu, Mn, Zn or any combination thereof.
[0061] During the adjustment process, all metals present in the feedstock are considered together with phosphorus. The feedstock contains one or more different metal-containing compounds, such as 1, 2, 3, 4, 5, 6, 7 or 8 different metal-containing compounds. The feedstock may also contain some metals in very low amounts, which are close to or exceed the detection limit. These are not considered to have a substantial effect on the process. Therefore, metals that are present in large amounts or in amounts above the detection limit are usually considered. The limit may be, for example, 1 ppm by weight. The feedstock may also contain certain metals in amounts that cannot be detected, so these metals and their effects on the weight ratio of metal to phosphorus cannot be considered in the adjustment, although they do participate in the reaction. However, these amounts are too small to substantially affect the results. The limit may be 1 ppm, or 0.5 ppm or 0.1 ppm.
[0062] The amount of phosphorus is measured as weight (ppm) of elemental phosphorus and the amount of metals as total weight (ppm) of elemental metals using, for example, ICP-AES (ASTM D-5185 (2018)).
[0063] The inventors have found diphosphates and polyphosphates in spent catalysts and dust, indicating that the stoichiometry of the reaction is not simple. In addition, the amounts of phosphorus and metals are given in the form of elemental phosphorus and elemental metals because it is difficult to measure these elements in molecular or ionic form at the levels required in the final step when the purified liquid renewable feedstock is contacted with the primary active catalyst in the presence of hydrogen. The ranges given for the weight ratios of metal to phosphorus (M:P) are empirically derived and correspond to the ranges within which precipitation can be obtained.
[0064] Phosphorus impurities can be contained in the raw materials in various chemical forms in the form of different phosphorus-containing compounds, for example in the form of phospholipids, oil or water-soluble or insoluble phosphorus compounds, or in the form of inorganic phosphates, diphosphates and phosphites. Typical phosphorus-containing compounds can also include glycerophospholipids, sphingolipids, phosphatidic acid complexes, phosphatidylethanolamine, nucleoside phosphates, apatite or bone meal (calcium phosphate), etc.
[0065] Metallic impurities may similarly be contained in the feedstock in various forms in the form of different metal-containing compounds, organic or inorganic, water-soluble or oil-soluble or insoluble.
[0066] If not removed during processing, a large number of impurities in renewable feedstocks used to produce renewable hydrocarbons may eventually end up in renewable fuels such as diesel, jet fuel or gasoline. In addition, impurities in hydroprocessing often cause several problems during the process itself. Although some of these impurities can be removed using known pretreatment techniques, it has not been possible to completely avoid fouling of catalysts used in hydroprocessing processes due to the accumulation of impurities into the catalyst over time. Impurities contained in the most difficult feeds or feedstocks have not been successfully and economically reduced or removed to the desired extent using currently available pretreatment methods.
[0067] Fouling of hydroprocessing catalysts generally leads to an increased deactivation rate and a shortened catalyst life. This in turn has important consequences, since the deterioration of the catalyst functionality eventually leads to the need to regenerate the catalyst or, most commonly, to replace the catalyst with a new one. Catalyst replacement on an industrial refinery scale implies the need to interrupt production during the catalyst replacement. Obviously, the need to replace the catalyst regularly depends only on the length of the catalyst life. Therefore, it goes without saying that being able to extend the catalyst life will increase productivity by reducing the frequency of production interruptions and subsequent production losses.
[0068] Catalyst deactivation, the loss of catalytic activity and / or selectivity over time, is a significant and ongoing problem in industrial catalytic processes. The costs to industry from catalyst replacement and process downtime add up to considerable economic losses each year. The timescale for catalyst deactivation can vary significantly depending on the process and type of catalyst used. Some catalysts may last for seconds, while others may last for decades. However, all catalysts will eventually deactivate and this is inevitable. Typically, the loss of activity and / or selectivity occurs slowly in a well-controlled process. However, process anomalies or improper hardware design may lead to unexpected and early failures. While catalyst deactivation is inevitable for most processes, some of its serious consequences can be avoided or at least postponed by adopting new processing methods.
[0069] Catalyst deactivation in this context means the gradual deterioration of the performance of a catalyst, which eventually reaches a level where it is no longer reasonable to continue using the catalyst. Reasonableness in this context is best described by the ability to produce a product that meets predetermined quality and quantity standards. In practice, this means that every catalyst faces a point in time when it has deactivated to the extent that the spent catalyst needs to be replaced with new catalyst. Deactivation can therefore be described as the length of catalyst life per frequency of shutdowns. This ratio provides a measure of the ability to produce the final product, taking into account the shutdown time required to replace the catalyst due to deactivation. In other words, if the number of shutdowns due to catalyst replacement caused by catalyst deactivation decreases, the amount of production lost in a given time frame will also decrease.
[0070] Catalyst deactivation is generally defined as the presence of impurities on the catalyst surface that block the active sites of the catalyst from the feedstock molecules. Catalyst deactivation can be caused by fouling or poisoning of the catalyst. Fouling is generally considered to be related to the deposition of insoluble components present in the feed or formed by degradation of the feed or reaction intermediates, while poisoning is related to the deposition of positively charged contaminants (such as alkali and alkaline earth metals) on acidic sites or negatively charged contaminants on hydrogenation sites.
[0071] Current technology generally focuses on minimizing the impurity content by removing as much impurities from the feedstock as possible, such as by expanding, optimizing or enhancing various purification or separation techniques. The assumption is that minimizing feedstock impurities will minimize catalyst fouling, which in turn will extend catalyst life by slowing the accumulation of impurities. It is estimated that the use of typical renewable feedstocks purified by, for example, degumming and / or bleaching will result in phosphorus levels of about 2 wt-% or more accumulating into the hydroprocessing catalyst during the catalyst life cycle, whereby catalyst replacement is typically required.
[0072] The present disclosure demonstrates that catalyst deactivation can be suppressed without increasing feedstock purification requirements. Instead, the inventors of the present disclosure have discovered that the weight ratio of impurity metals to phosphorus of the feedstock needs to be adjusted.
[0073] In one aspect of the present disclosure, there is provided a method for reducing deactivation of a hydroprocessing catalyst, wherein the hydroprocessing catalyst is used as a primary active catalyst for producing renewable hydrocarbons from a renewable feedstock by hydroprocessing, the renewable feedstock comprising at least one oxygen-containing compound, at least one metal-containing compound and at least one phosphorus-containing compound as impurities, the method comprising the steps of:
[0074] i. adjusting the metal to phosphorus (M:P) weight ratio, measured as elemental metal and elemental phosphorus, of the renewable feedstock to a value in the range of 0.70 to 1.26 to obtain an impurity adjusted renewable feedstock, and
[0075] ii. subjecting the impurity-adjusted renewable feedstock to a temperature of 190°C to 400°C under reducing conditions, thereby forming a solid precipitate comprising at least one metal- and phosphorus-containing compound, and a purified liquid renewable feedstock, and
[0076] iii. contacting the purified liquid renewable feedstock with a primary active catalyst in the presence of hydrogen.
[0077] Impurities in the raw material (whose amount is to be adjusted) include phosphorus and one or more metals, preferably the most abundant and most disturbing metals are selected from Na, K, Ca, Mg and Fe. However, this choice may depend on the source of the raw material. Phosphorus and metal impurities can be present in the raw material in dissolved form. They are usually present in the form of impurity-containing compounds. Phosphorus and one or more metals may also be present in the same impurity compound, but most typically they are present in different impurity compounds in the raw material. In this specification, a purified liquid raw material means a raw material containing less phosphorus and / or metal (multiple) (such as dissolved phosphorus and metal impurities) than the original raw material. "Dissolved impurities" in this text means impurities remaining in the liquid phase after filtering with a 2 μm filter, that is, impurities in solid form removed by such filtration are not considered dissolved impurities in this article.
[0078] The present disclosure enables the use of lower quality feedstocks without increasing the impurity removal load in the feedstock pretreatment processing unit. In addition, the desired metal to phosphorus weight ratio can serve as a guideline for feedstock selection and treatment prior to hydroprocessing.
[0079] While there are many impurities present in renewable feedstocks, such as biogenic lipids, that can contaminate hydroprocessing catalysts, the factor that is generally considered to be most likely to cause deactivation is phosphorus. Without being bound by any theory, it is expected that phosphorus will attach to the catalyst surface and block feedstock access to the active sites of the catalyst material. Alternatively, phosphorus can react with metallic impurities also present in the feedstock during the hydroprocessing process to form metal phosphates. These metal phosphates are likely to precipitate from the feedstock in the form of solid particles before the phosphorus and metallic impurities have a chance to reach and contaminate the catalyst surface. In fact, the inventors have discovered that X-ray diffraction (XRD) analysis of dust samples (i.e., precipitates) from spent catalyst beds in hydroprocessing reactors indicated the presence of metal phosphate precipitates, such as calcium ferric phosphate and sodium ferric phosphate (see Figure 1 a and 1b). It is further believed that during the hydrotreatment process, phosphorus-containing and metallic impurities already present in the feedstock in solid form (i.e., precipitated form) no longer react adversely.
[0080] A key factor has been identified as contributing to the formation of phosphate-rich solid precipitates. The metal to phosphorus (M:P) weight ratio of the feed has been found to be positively correlated with the amount of impurity dust formed during operation of a hydroprocessing reactor using different feeds. Different feedstocks have different M:P ratios. Feeds with an M:P ratio close to 1 were found to form more solid impurity dust than feeds with lower or higher M:P ratios. Furthermore, the amount of phosphorus attached to the catalyst surface after the same operating time was negatively correlated with the feed M:P ratio. The solid impurity dust formed does appear to affect catalyst fouling. Therefore, a suitable M:P ratio (e.g., a ratio close to 1) helps prevent catalyst fouling and deactivation, thereby extending the life of the catalyst.
[0081] The metal to phosphorus (M:P) weight ratio of the renewable feedstock measured as elemental metal and elemental phosphorus can be, for example, 0.70, 0.75 or 0.80 or 0.85 or 0.90 or 0.95 or 1.0 or 1.05 or 1.10 or 1.15 or 1.2 or 1.25, up to 0.75 or 0.80 or 0.85 or 0.90 or 0.95 or 1.0 or 1.05 or 1.10 or 1.15 or 1.2 or 1.25 or 1.26 to obtain an impurity adjusted renewable feedstock. In a preferred embodiment, the metal to phosphorus (M:P) weight ratio of the renewable feedstock is adjusted to a value in the range of 0.73 to 1.23, such as 0.76 to 1.20, measured as elemental metal and elemental phosphorus to obtain an impurity adjusted renewable feedstock. This provides the highest amount of solid precipitation per kilogram of metal and phosphorus in the renewable feedstock, thereby most effectively reducing catalyst deactivation. Thus, precipitation of large amounts of solids will not reduce catalyst deactivation, but the amount of unbalanced feedstock (i.e., feedstock containing, for example, a high excess of phosphorus and low or no metal) of the catalyst will be reduced when a large portion of the phosphorus and metal are precipitated from the feedstock due to the desired weight ratio of metal to phosphorus.
[0082] The low-quality renewable raw materials disclosed herein are usually collected from various sources in a batch delivery mode. In particular, waste and residual raw materials may arrive at the storage tank area by truck transportation or by sea from a providing facility or a distribution station. The raw materials are directed from the storage tank area to the refinery area, where suitable batches that meet the required raw material specification standards are formed for processing. These standards include determining the impurity distribution of each batch of raw materials. The raw materials arriving at the refinery usually have an analysis certificate indicating the content of various components and impurities. Therefore, according to their properties (such as impurity distribution), the feed raw material batches can be blended together to obtain raw materials suitable for selected processing or pretreatment processes. In addition, the pretreated raw materials can be stored in a storage tank before processing, from which the selected feed can be further mixed into the desired blend to form a final composition, and then directed to, for example, a hydroprocessing reactor. Typically, the raw materials are stored at high temperatures, such as more than 50°C, to keep them in a liquid state and avoid separation.
[0083] In one embodiment, the adjustment of step i may be performed by blending into the renewable feedstock at least one additional renewable feedstock comprising a balanced amount of a metal-containing compound or a phosphorus-containing compound to obtain an impurity-adjusted renewable feedstock having a metal to phosphorus weight ratio of 0.70 to 1.26.
[0084] Several candidates can be selected from feedstocks containing different impurity profiles, and blended together to obtain a blend that meets the desired profile. For example, a batch of algae oil feedstock with a phosphorus content of 700 ppm but very low metal content can be blended with another batch of brown grease feedstock with a low phosphorus content but a metal content as high as 700 ppm, thereby obtaining a high total impurity content but a metal to phosphorus weight ratio close to 1.
[0085] In one embodiment, the balance of the metal-containing compound or phosphorus-containing compound is determined by:
[0086] - first, the amount of metal (M1) and phosphorus (P1) in the renewable raw material in weight-%, and
[0087] - secondly, determining the amount in weight-% of metals (M2) and phosphorus (P2) of at least one further renewable raw material, and
[0088] - Third, at least one additional raw material and its amount are selected to meet the requirement of a weight ratio of the total metal (M1+M2) amount to the total phosphorus (P1+P2) amount of 0.70 to 1.26.
[0089] The number of renewable raw material batches blended together is not critical, provided that the final blend obtained meets the required specification, i.e. the metal to phosphorus weight ratio of the blended raw materials is in the range of 0.70 to 1.26, measured as elemental metal and elemental phosphorus. There may be several renewable raw material batches with different distributions of metal impurities M1, M2, M3, etc. and phosphorus impurities P1, P2, P3, etc. After analysis and classification, the raw material batches can be blended together in appropriate and optimized proportions according to their calculated phosphorus and metal impurity concentrations.
[0090] Blending together renewable raw materials with suitable impurity profiles is not the only way to achieve the desired metal to phosphorus ratio. The desired amounts of phosphorus and metal can be added directly to the renewable raw materials in question in the form of ionic compounds. This applies to both the addition of metal-containing compounds and the addition of phosphorus-containing compounds. However, adding metal-containing compounds to balance the amount of excess phosphorus is considered to be a preferred option compared to the opposite situation.
[0091] The adjustment in step i can be carried out by adding a metal-containing compound (such as an ion-containing metal compound, such as a hydroxide or a fatty acid salt) or a phosphorus-containing compound (such as phosphoric acid or a phospholipid) to the renewable raw material, so as to obtain a metal-to-phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable raw material. In a preferred embodiment, the adjustment in step i is carried out by adding at least one metal-containing compound to the renewable raw material, so as to obtain a metal-to-phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable raw material. Typically, the problematic impurities are phosphorus-containing compounds in the raw material, rather than metal-containing compounds. There are some effective methods, such as pretreatment methods, that can be used to remove excess metals from the raw material, which can be conveniently used. The removal of phosphorus is considered to be more problematic. However, if necessary, the excess metal can also be balanced by adding phosphorus-containing compounds. Therefore, in one embodiment, the adjustment in step i is carried out by adding at least one phosphorus-containing compound to the renewable raw material, so as to obtain a metal-to-phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable raw material.
[0092] Examples of metal-containing compounds that can be added to renewable raw materials are compounds that can provide metal cations, including metal hydroxides, such as sodium hydroxide, potassium hydroxide, calcium hydroxide, magnesium hydroxide, iron hydroxide, etc.; metal salts of fatty acids, such as sodium soaps, potassium soaps, calcium soaps, magnesium soaps, iron soaps, etc.; or mixtures thereof. In this context, the fatty acid can be, for example, stearic acid forming a sodium salt, such as sodium stearate, or any other suitable fatty acid. The metal can include alkali metals, such as Li, Na, K; alkaline earth metals, such as Mg or Ca; and transition metals, such as Fe, Co, Mn; or even Al. It is preferred to use metal-containing compounds that do not provide other substances to the raw material that interfere with subsequent processing.
[0093] In one embodiment, the at least one metal-containing compound is an ion-containing metal compound, preferably a hydroxide or a fatty acid salt.
[0094] Examples of possible phosphorus-containing compounds are phosphoric acid, phospholipids and the like.
[0095] The required amount of one or more chemical balance compounds to be added can be calculated based on the amount of metal or phosphorus in the raw materials used, and the total metal to phosphorus ratio meets the specified range of 0.70 to 1.26.
[0096] In one embodiment, the desired amount of metal-containing compound to be added is determined by:
[0097] - first, the amount of metal (M1) and phosphorus (P1) in the renewable raw material in weight-%, and
[0098] - Secondly, the required amount of metal-containing compound (M2') to be added is calculated as elemental metal to achieve a total metal (M1+M2') to phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable feedstock.
[0099] Some feedstocks can be purified by known pretreatment methods, before or after balancing their weight ratios of metals and phosphorus. The amount of impurities successfully reduced by the selected pretreatment method depends on the type of feedstock. For example, feedstocks such as acidulated soapstock (ASK), dried poultry fat (AFP) and brown grease (BG) cannot be purified alone, but can only be bleached to the extent that they are then suitable for catalytic hydrotreatment. Typically, in acidulated soapstock or poultry fat based feedstocks, the amount of residual phosphorus is high after conventional purification methods. For brown grease, the main problem is the high metal content. The metal content can be so high that very high filtration resistance, or even clogging, can be observed when bleaching brown grease. These types of feedstocks clearly benefit from the adjustment of phosphorus by metals.
[0100] In another embodiment, the renewable raw material is pretreated before or after the conditioning of step i. Preferably, the amount of metal-containing compounds and phosphorus-containing compounds in the renewable raw material is reduced to a value of less than 20 ppm, preferably less than 10 ppm of metal (calculated as elemental metal) and less than 20 ppm, preferably less than 10 ppm of phosphorus (calculated as elemental phosphorus) measured by ICP-AES.
[0101] Adjustment of metals and phosphorus can be combined with pretreatment methods, which can include, for example, filtration, sedimentation, centrifugation, washing, degumming or bleaching, depending on the residual impurities present in the feedstock. In one embodiment, pretreatment includes filtration, sedimentation, centrifugation, washing, degumming or bleaching or any combination thereof.
[0102] The adjustment according to step i of the present disclosure may also be carried out, depending on the level of impurities, by selectively reducing the amount of phosphorus-containing impurities, or possibly alternatively reducing the amount of metal-containing impurities, by a selected pretreatment method or combination thereof (if applicable). In one embodiment, the adjustment in step i is carried out by pretreating the renewable raw material (such as bleaching or degumming or both) to reduce the amount of phosphorus-containing compounds or metal-containing compounds to obtain a level in which the weight ratio of metal to phosphorus of the impurity-adjusted renewable raw material is 0.70 to 1.26.
[0103] The above methods for adjusting the amount of metal and phosphorus impurities can also be combined. Therefore, in another embodiment of the present disclosure, the adjustment in step i is performed by any combination of the following methods:
[0104] - blending at least one additional renewable raw material into the renewable raw material, the additional renewable raw material comprising a compensating amount of a metal-containing compound or a phosphorus-containing compound,
[0105] - adding metal-containing compounds to renewable raw materials,
[0106] - reducing the amount of phosphorus-containing compounds or metal-containing compounds by pretreatment,
[0107] The impurity-adjusted renewable raw material thus obtained has a metal to phosphorus weight ratio of 0.70 to 1.26.
[0108] Once the feedstock reaches a balance of the appropriate metal to phosphorus ratio, it is subjected to high temperature treatment. The pressure and environmental conditions at high temperature can vary, and preferably, the feedstock is subjected to high temperature under reducing conditions including the presence of hydrogen or water (such as water vapor or steam). Studies have found that simply briefly placing the balanced feedstock at a temperature of 190-400°C is sufficient to cause solid precipitation in the form of dust. The exposure time may be only a few minutes to a few hours, depending on the severity of the temperature. Therefore, the resulting feed stream contains fine-grained solid dust precipitation and purified liquid renewable raw materials for catalytic hydroprocessing. In one embodiment, the high temperature in step ii is 240°C to 380°C, such as 250°C to 370°C, or even 260°C to 360°C. Especially temperatures within the processing temperature range, such as hydroprocessing or hydrodeoxygenation temperatures in related reactors are advantageous because a separate thermal treatment unit is not required. According to one embodiment, the treatment at high temperature can be, for example, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 405°C, 410°C, 425°C, 430°C, 440°C, 455°C, 460°C, 470°C, 480°C, 490°C, 505°C, 510°C, 520°C, 530°C, 540°C 90 or 395°C up to 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, 265°C, 270°C, 280°C, 285°C, 290°C, 295°C, 300 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C, 375°C, 380°C, 385°C, 390°C, 395°C, 400°C. High temperatures are selected so as to obtain the best results for removing impurities. The temperature may depend to a certain extent on the reaction time. The temperature may also be selected based on other steps of the process. The temperature may also depend on the impurities to be removed and their reaction with the metal phosphate. In addition, the size of the reactor section used for the heat treatment in step ii may play a role in selecting the optimal temperature as well as side reactions, because some feedstocks may contain components that begin to oligomerize or crack at certain temperatures.
[0109] Lecithin generally begins to decompose at temperatures of about 180°C, however, longer retention times may be required for complete decomposition and it is often more practical to use higher processing temperatures.
[0110] Raw materials are placed in a time period of 0.5 minute to 2 hours at high temperature. The time required usually depends on temperature, and the higher the temperature, the shorter the required processing time. Some raw materials may also be more sensitive to heating than other raw materials. Therefore, the duration of heat treatment can be, for example, from 0.5 minute, 1 minute, 5 minutes, 10 minutes, 15 minutes, 30 minutes, 45 minutes, 1 hour, 1 hour 15 minutes or 1 hour 30 minutes to up to 30 minutes, 45 minutes, 1 hour, 1 hour 15 minutes, 1 hour 30 minutes, 1 hour 45 minutes or 2 hours. Under favorable conditions, it is found that the precipitation after treatment at high temperature is instantaneous, so very short exposure time may be enough. Preferably, heat treatment at high temperature is 0.5 minute to 1 hour 30 minutes, such as 1 minute to 1 hour, or even 2 minutes to 50 minutes. Processing at high temperature means effective time in this article, and those skilled in the art can easily calculate the effective time according to reactor type and residence time therein, whether the process is continuous process or intermittent process and according to required heating and cooling time.
[0111] Typically, the feedstock is subjected to high temperatures in a pressure reactor and the pressure may be 2-20 MPa. The treatment may be carried out under elevated hydrogen pressure or under pressure below the equilibrium pressure.
[0112] After the feedstock is subjected to adjustment of the ratio of beneficial metals to phosphorus and subsequent exposure to high temperatures to precipitate phosphorus- and metal-containing compounds from the feedstock, a purified liquid renewable feedstock is obtained. This purified liquid feedstock can now be directed to a hydrotreating catalyst together with hydrogen for at least catalytic reduction or removal of oxygen and branching of the formed hydrocarbon chains by isomerization to obtain a branched hydrocarbon blend suitable for purposes such as renewable fuels or renewable chemicals. Hydrotreating can be achieved by combined hydrodeoxygenation and isomerization or by continuous hydrodeoxygenation and isomerization. Thus, in one embodiment, hydrotreating comprises hydrodeoxygenation; combined hydrodeoxygenation and isomerization; or continuous hydrodeoxygenation and isomerization.
[0113] The term "hydrotreating" or "hydrotreatment" refers herein to a chemical unit operation in which the reaction of hydrogen is used to remove impurities, such as oxygen, sulfur, nitrogen, phosphorus, silicon and metals, especially as part of a petroleum refining process. Hydrotreating also includes hydroisomerization. Hydrotreating can be carried out in one or more reactor units or in one or more catalyst beds in one or more steps. Preferably, hydrotreating is carried out in two steps. For example, hydrotreating in one step may consist of hydrodeoxygenation combined with hydroisomerization, and hydrotreating in two steps may consist of a first hydrodeoxygenation step followed by a hydroisomerization step. Preferably, hydrotreating comprises a first hydrodeoxygenation step followed by an isomerization step.
[0114] The term hydrotreatment as used herein refers essentially to hydrodeoxygenation (HDO), i.e. the removal of oxygen in the form of water in the presence of molecular hydrogen under the influence of a (HDO) catalyst; hydroisomerization, i.e. the branching of normal paraffins to form isoparaffins in the presence of molecular hydrogen under the influence of a hydroisomerization catalyst; hydrodesulfurization (HDS), i.e. the removal of sulfur as hydrogen sulfide by molecular hydrogen under the influence of a (HDS) catalyst; hydrodemetallization (HDM), i.e. the removal of metals by trapping them with a (HDM) catalyst; hydrodenitrogenation (HDN), i.e. the removal of nitrogen by molecular hydrogen under the influence of a (HDN) catalyst; hydrodearomatization (HDA), i.e. the saturation or ring opening of aromatics by molecular hydrogen under the influence of a (HDA) catalyst. In general, hydrotreatment means deoxygenation by hydrogenation, i.e. hydrodeoxygenation (HDO) and hydrogenation of double bonds that may be present. The effluent of hydrotreatment is essentially paraffinic hydrocarbons, containing less than 1 wt-% of oxygen and only trace amounts of possible impurities.
[0115] Hydroprocessing may include hydrodeoxygenation and isomerization, using a temperature in the range of 200°C to 400°C, a pressure in the range of 1 MPa to 20 MPa, such as 2 to 15 MPa, or even 3 to 10 MPa, and a hydrogen flow rate in the range of 100 Nl H2 / l to 1500 Nl H2 / l feed. The expression Nl H2 / l means the normal number of liters of hydrogen per liter of feed entering the HDO reactor. According to a specific embodiment, the hydrodeoxygenation reaction conditions include a temperature in the range of 250°C to 400°C, a pressure in the range of 2 MPa to 12 MPa, a flow rate of 0.5-3 h -1 The invention relates to a hydrodeoxygenation catalyst having a WHSV (weight hourly space velocity) in the range and a hydrogen flow rate of 350-900 Nl H2 / l feed.
[0116] The hydrotreatment can be carried out at a temperature of 270°C to 380°C, such as 275°C to 370°C, or 285°C to 360°C. The temperature can be, for example, from 270°C, 275°C, 280°C, 285°C, 290°C, 295°C, 300°C, 305°C, 310°C, 315°C, 320°C, 325°C, 330°C, 335°C, 340°C, 345°C, 350°C, 355°C, 360°C, 365°C, 370°C or 375°C. , 370°C, 375°C, and 380°C. The pressure during hydrotreating may be from 2 MPa to 12 MPa. The pressure can be, for example, from 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, or 12 MPa to as high as 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 11 MPa, or 12 MPa.
[0117] In particular, in the case of HDO, the weight hourly space velocity (WHSV) can be between 0.25 h -1 Up to 3.0 h -1 In the range of 0.7 h -1 Up to 3.0 h -1 , depending on the hydrogen consumption. The hydrogen flow rate, especially for HDO, can be in the range of 100 Nl H2 / l to 1500 Nl H2 / l feed, more preferably 250 Nl H2 / l to 900 Nl H2 / l feed. In one embodiment, the primary active catalyst comprises a catalyst suitable for hydrodeoxygenation or combined hydrodeoxygenation and isomerization.
[0118] In one embodiment, in the presence of at least a main active catalyst, hydrodeoxygenation is carried out in a hydrodeoxygenation reactor or zone, and the main active catalyst comprises a metal on a carrier. The main active hydroprocessing catalyst generally comprises at least one component selected from the 6th, 8th or 10th group of the periodic table IUPAC. Specifically, the main active hydroprocessing catalyst includes at least one of nickel, molybdenum, cobalt, tungsten and a combination thereof. The main active catalyst may, for example, include NiMo, CoMo, NiW or CoNiMo. The main active hydroprocessing catalyst generally has a carrier comprising at least one of alumina, silica, zeolite and a combination thereof. In particular, the main active hydroprocessing catalyst may be a sulfided NiMo or CoMo catalyst. If the feed still contains sulfur even after purification, the catalyst does not necessarily need to be sulfided. In one embodiment, in the presence of at least one main active catalyst, hydrodeoxygenation is carried out in a hydrodeoxygenation reactor or zone, and the main active catalyst comprises a metal on a carrier. In another embodiment, the metal includes Ni, Mo, Co, W or any combination thereof, and the carrier includes alumina, silica, zirconium oxide, zeolite or a mixture thereof.
[0119] According to one embodiment, the hydroprocessing conditions are adjusted to best serve the stream in question. In practice, this may mean that the reaction conditions and the catalyst used may vary slightly depending on the desired end product.
[0120] The hydroprocessing step may also include mixing the feedstock purified by the present method with another renewable feedstock or several different renewable feedstocks to co-hydroprocess them.
[0121] The hydrodeoxygenation can be carried out as described, for example, in FI 100248, EP 1741768, WO 2007 / 068795, WO 2016 / 062868 or EP 2155838 and using a conventional hydrotreating catalyst as the main active catalyst in the presence of hydrogen.
[0122] Advantageously, the HDO is carried out to obtain a hydrodeoxygenated material comprising less than 1 wt-% oxygen.
[0123] The partially deoxygenated material may be recycled to the hydrodeoxygenation process.Preferably, the ratio of purified liquid renewable feedstock obtained by the process of the present disclosure to recycled hydrodeoxygenated material is from 1 :1 to 1 :20.
[0124] Hydrodeoxygenation and hydroisomerization can be carried out in parallel or sequentially in one or more reactors. The reactor may also contain one or more catalyst beds, with the same or different amounts of catalyst. Fresh feed may be directed to any or all catalyst beds in the reactor arrangement used, and the feed flow rate into the catalyst bed may vary between individual beds.
[0125] Both the hydrodeoxygenation step and the hydroisomerization step can be carried out in the same reactor, and even in the same reactor bed. The hydroisomerization catalyst can be a noble metal bifunctional catalyst, such as a commercial catalyst containing Pt, for example Pt-SAPO or Pt-ZSM, or for example a non-noble metal catalyst, such as NiW. The hydrodeoxygenation and hydroisomerization steps can be carried out in the same catalyst bed, using for example a NiW catalyst in both the hydrodeoxygenation and the isomerization.
[0126] According to one embodiment, the hydroisomerization catalyst comprises at least one of platinum, palladium, nickel and combinations thereof, and a zeolite selected from ZSM-12, ZSM-23, SAPO-11, SAPO-41 and fernerite on an alumina and / or silica support.
[0127] The isomerization step may be carried out at a temperature of 200° C. to 400° C., such as 280° C. to 370° C., or 300° C. to 350° C. The pressure may be 1 MPa to 6 MPa, or 2 MPa to 5 MPa, or 2.5 MPa to 4.5 MPa. The WHSV may be 0.5 l / h to 3 l / h, such as 0.5 l / h to 2 l / h, or 0.5 l / h to 1 l / h, and the H2 flow rate may be 100 to 800 Nl H2 / l feed, or 200 to 650, or even 350 to 500 Nl H2 / l feed.
[0128] During the isomerization process, normal paraffins are branched to form isoparaffins. Preferably, the conditions are selected so that the branches are located at or near the ends of the molecules, thereby improving the cold flow properties of the renewable fuel.
[0129] The isomerization treatment is a step that is primarily used to isomerize the hydrodeoxygenated feedstock. That is, while most thermal or catalytic conversions (such as HDO) result in a slight degree of isomerization (usually less than 5 wt-%), the isomerization step that may be employed in the present process is one that results in a significant increase in the isoparaffin content.
[0130] Isomerization, such as hydroisomerization, may be carried out in a conventional hydroisomerization unit, such as those described in FI 100248, EP 1741768, WO 2007 / 068795, WO 2016 / 062868 or EP 2155838. Hydroisomerization involves the addition of hydrogen to the reaction.
[0131] Most typically, the renewable hydrocarbons produced by the present processes and methods are used in renewable fuels, such as gasoline, diesel or aviation chemical fuels or chemicals. The renewable hydrocarbons can be used directly as fuels, or they can also be used as components of fuels.
[0132] The feedstock, which has been balanced in terms of adjusting the amount of metal and phosphorus impurities, is subjected to high temperatures before contacting the main active catalyst of the hydroprocessing. It is possible that at least one pretreatment zone is heated to a temperature close to the hydroprocessing temperature, for example, a temperature between 190-400°C. In oil refining, there are various traditional and commercially available solutions for different pretreatment zones, in different or the same reactors, such as separate guard reactors, including guard beds or graded layers in separate reactors, or in the same reactor when hydroprocessing occurs. Guard beds and grading are well-known concepts, for example, see US5879642. In addition, the hydroprocessing reactor containing a fixed main active catalyst bed of discrete solid materials can include carriers or retaining materials at its inlet and / or outlet and / or between the material beds, which are substantially inert to the hydroprocessing reaction. These inert materials can capture dust particles, i.e., impurity dust, such as phosphorus-containing compounds, metal-containing compounds, coke particles, catalyst fines, sediments, or other entrained foreign particulate materials from the reactor inlet feed stream at least partially in the form of solid impurities. The capture of impurities will prevent undesirable materials from clogging the main active catalyst bed, preventing the main active catalyst bed from being poisoned or deactivated. These inert materials can include ceramic materials in the form of pellets or spheres, which are resistant to crushing, high temperature and high pressure, such as glass balls, silicon dioxide and aluminum oxide, or any mixture thereof. Typically, pretreatment zones do not actively carry out, for example, hydroprocessing, because they do not include the same main active hydroprocessing catalyst, but if necessary, they can include various similar materials that can at least partially hydroprocess the raw material. Alternatively, they may only be mechanical filtration zones for insoluble solid impurities of dust-type raw materials, without any catalytically active materials inside. These guard beds or graded material layers are well known in oil refining (see Riazi, MR et al., (editor), Petroleum Refining and Natural GasProcessing, 2013, ISBN 978-0-8031-7022-3 Pages 230-231). In recent years, various effective methods and complex configurations have been developed to remove particles, such as those described in WO 2004 / 094039 A1. In the present disclosure, one or more pretreatment zones or layers, such as guard beds or graded layers, may be used, which contain various materials, such as inert materials with respect to hydroprocessing or materials that are less active than the primary active catalyst of the hydroprocessing. In an embodiment, the hydroprocessing further comprises directing the impurity-adjusted renewable feedstock through a heated pretreatment zone, preferably upstream of the primary active catalyst.
[0133] The guard bed and the graded layer can be appropriately arranged in various configurations upstream of the hydroprocessing reactor or inside the hydroprocessing reactor, preferably upstream of the main active hydroprocessing catalyst bed. The purpose of using the pretreatment zone is to promote and enhance the generation of dust, for example, by the catalytic hydrogenation reaction of phosphorus and metal compounds, and to filter out the dust precipitation formed from the raw material before the raw material enters one or more main active hydroprocessing catalyst beds. Therefore, the pretreatment zone preferably contains the same or similar catalyst material as described in the hydroprocessing. However, the catalytic activity of the pretreatment zone catalyst is lower than the activity of the main active hydroprocessing catalyst. Several alternatives to different grades and guard bed materials with different capture capabilities for multiple metals are commercially available. Those skilled in the art can customize the activity of the pretreatment zone catalyst according to their needs. The catalyst used in the pretreatment zone can also be diluted with an appropriate inert medium. In addition, the dilution of the catalyst helps to balance the exothermic reaction and promote temperature control in the hydroprocessing reactor.
[0134] In another embodiment, the heated pretreatment zone includes a compound that is less active for hydrodeoxygenation than the primary active catalyst, such as a compound that is inactive for hydrodeoxygenation. The graded bed or guard bed may contain the same catalyst material used in the HDO catalyst bed, such as NiMo, but the graded bed or guard bed catalyst is less active. Catalyst activity can be reduced by, for example, diluting the active material with an inert material, changing the catalyst material composition, or having only a small amount of active material in the layer (such as less active material than in the primary active catalyst layer used for HDO).
[0135] Without being bound by any theory, it is believed that during the thermal treatment of the metal and phosphorus adjusted feedstock at high temperatures, phosphorus-containing compounds and metal-containing compounds present in the feedstock form metal phosphates as found in the spent catalyst bed analysis (see Figure 1 ). In addition to reducing conditions (such as the presence of hydrogen or water), some phosphorus-containing compounds (such as certain phospholipids) may require the presence of a catalyst material that is less active for hydrodeoxygenation than the primary active catalyst in order to react and form a convenient solid precipitate. If water is used, it is typically used in an amount of about 1 wt-% or more, such as 3 wt-% or less. The solid dust-like precipitate can be effectively removed from the feedstock by simple separation methods (such as filtration). Therefore, the metal and phosphorus compounds that react to form the solid precipitate will no longer be present in the subsequent hydroprocessing process. In addition, in the hydroprocessing of purified liquid feedstocks, catalyst deactivation can be reduced and the life cycle of the catalyst bed can be extended.
[0136] The objective is to balance the metal and phosphorus content of the feedstock to a sufficient degree so that metal phosphates can be formed at a suitably high temperature by optimal thermal treatment, i.e. to ensure favorable reaction conditions for metal phosphate formation and subsequent removal of the solid dust containing the metal phosphates formed. The impurity dust (i.e. the solid precipitate formed) can be collected during the hydroprocessing process, wherein the dust is mainly retained in the hydroprocessing catalyst, but it is preferably removed from the feedstock before the dust enters the main active hydroprocessing catalyst (e.g., the hydrodeoxygenation catalyst). However, it is foreseeable that dust particles that remain in or bypass the hydroprocessing catalyst bed prior to treatment according to the present disclosure are less harmful than phosphorus- or metal-containing compounds in the feedstock.
[0137] Preferably, the feedstock contacted with the hydrodeoxygenation catalyst should not contain more than 10 ppm, preferably not more than 5 ppm, more preferably not more than 1 ppm of alkali and alkaline earth metal impurities calculated as elemental alkali and rare earth metals; not more than 10 ppm, preferably not more than 5 ppm, more preferably not more than 1 ppm of other metals calculated as elemental metals; and not more than 30 ppm, preferably not more than 15 ppm, more preferably not more than 5 ppm of phosphorus-containing impurities calculated as elemental phosphorus. For any impurities other than phosphorus, sodium, potassium, magnesium, calcium and iron, any excess amounts may be removed by other methods known per se. The less pure the feedstock is when it arrives at the refinery, the more methods are needed to purify it to meet the catalyst requirements and to ensure that the catalyst life or life cycle remains reasonable for industrial production purposes.
[0138] The precipitate containing solid impurities formed in the present disclosure may include, for example, iron phosphate, sodium phosphate, potassium phosphate, magnesium phosphate, calcium phosphate or mixed phosphates thereof, such as sodium iron phosphate, or mixtures of these different types of phosphates. After exposure to high temperatures, in addition to solid precipitation, most metals and phosphorus will no longer be present in a harmful form in subsequent processing, thereby reducing the tendency and rate of catalyst deactivation. Therefore, compared with the original raw material, the purified liquid renewable raw material of the present disclosure contains less phosphorus and / or metals. Using pretreatment to remove solid precipitation can reduce at least 85 wt-% of solid precipitation, such as at least 90 wt-% or even 95 wt-%. When another method for removing precipitation from a heat-treated raw material (such as step ii of the method) is used, the removal efficiency is preferably within the same range as filtering by pretreatment.
[0139] In one embodiment, the solid precipitate formed in step ii. is retained in a heated pre-treatment zone.
[0140] The renewable raw material adjusted for appropriate impurities in step i may be further heated before entering a subsequent pretreatment zone or reactor (i.e., a pretreated precipitation retention layer or a main active catalyst bed for hydroprocessing). The temperature of the raw material may be increased using a heat exchanger upstream of the pretreatment zone. The heated raw material is then directed to the pretreatment zone where precipitation occurs, and the precipitation is retained in the layer therein so that the purified liquid renewable raw material enters the hydroprocessing zone or reactor. Therefore, in one embodiment, the renewable raw material adjusted for impurities is subjected to a temperature of 190°C to 400°C by directing it through a heat exchanger.
[0141] It has been further found that the presence of hydrogen facilitates precipitation. In one embodiment, the impurity-adjusted renewable feedstock enters pretreatment or hydroprocessing in the presence of hydrogen. Hydrogen can be directed to the pretreatment zone / reactor or hydroprocessing zone / reactor together with the feedstock or separately. The hydrogen pressure can be 1 MPa to 12 MPa, and the hydrogen flow rate is in the range of 100 to 1500 Nl H2 / l feed.
[0142] In a hydrotreating process unit, such as a hydrodeoxygenation reactor, a catalyst is used to remove oxygen from the feedstock, resulting in an effluent leaving the reactor. The conversion performance of the catalyst is a function of time. Eventually, the performance of the catalyst will deteriorate to a level that requires catalyst replacement, an expensive and complex maintenance task, where the shorter the time taken to replace the catalyst, the smaller the production loss. The time the catalyst is in use is represented by the catalyst cycle length, which is the length of the catalyst life cycle of the process unit. In a hydrodeoxygenation unit, the cycle length is defined by estimating the time that the unit can be operated at full capacity without the hydrodeoxygenation conversion falling below a critical level, based on a predefined standard set for the hydrodeoxygenation conversion, without reducing the unit load.
[0143] The ability to use low-quality feedstocks, such as waste and residue feedstocks rich in impurities, in the production of renewable fuels opens the possibility of sourcing a wider range of raw materials. Problematic impurity elements in waste and residue feedstocks are particularly phosphorus and metals, as well as impurities such as chlorides and nitrogen. Phosphorus and metals in particular tend to accumulate on catalysts and deactivate them, resulting in a shortened catalyst life cycle.
[0144] When describing embodiments of the invention, all possible combinations and permutations of embodiments have not been explicitly described. However, the mere fact that certain measures are stated in mutually different dependent claims or described in different embodiments does not indicate that a combination of these measures cannot be used to advantage. The invention contemplates all possible combinations and permutations of the described embodiments.
[0145] It should be understood that the embodiments of the present invention disclosed are not limited to the specific structures, process steps or materials disclosed herein, but are extended to equivalents that will be recognized by those of ordinary skill in the relevant art. It should also be understood that the terms used herein are only used for the purpose of describing specific embodiments and are not intended to be limiting.
[0146] Furthermore, the described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.In the description, numerous specific details are provided to provide a thorough understanding of the embodiments of the invention.
[0147] In this document, the verbs "to comprise" and "to include" are used as open limitations that neither exclude nor require the presence of unrecited features. Unless expressly stated otherwise, the features recited in the dependent claims are mutually freely combinable. Furthermore, it should be understood that the use of "a" or "an" throughout this document, i.e. the singular, does not exclude a plural.
[0148] The inventors herein intend that the terms "comprising," "including," and "containing" be optionally replaced in each instance with the terms "consisting of," "composed of," and "composed of," respectively.
[0149] Example
[0150] Example 1
[0151] A crude feedstock containing waste cooking oil (UCO) and animal fat (AF) was used for hydrodeoxygenation (HDO) experiments. The crude feedstock was purified by pretreatment using bleaching, which resulted in a pretreated feedstock having phosphorus in an amount ranging from 0.1-7.0 ppm measured as elemental phosphorus and 0.1-0.5 ppm of each metal measured as elemental metals, with the most abundant metals used herein, namely, Fe, K, Ca, Na, and Mg. The pretreated feedstock was analyzed for phosphorus and metal amounts by first digesting the feedstock sample with acid in a microwave oven to obtain a visually clear water / acid matrix, then diluting it to a known amount and analyzing it using ICP-MS / MS (tandem inductively coupled plasma mass spectrometry) according to an acid-based calibration.
[0152] The pretreated feedstock is introduced into the HDO reactor. The HDO reactor is contained in a graded layer upstream of the HDO zone and the main active catalyst bed therein. The graded layer mainly contains alumina and a small amount of low-activity NiMo catalyst. The thickness of the graded layer is one-fourth the thickness of the HDO catalyst layer. The reactor temperature at the inlet of the graded layer is about 270°C, the pressure is 5 MPa, and the WHSV is 0.75 h -1 The pretreated feedstock was introduced into the graded layer together with hydrogen (900 Nl H2 / l feed).
[0153] According to the classification, the feedstock is directed to the hydrodeoxygenation zone containing the main active HDO catalyst bed. The HDO catalyst material in this bed is sulfided NiMo on an alumina support. The HDO zone inlet temperature is 320°C and the pressure is 5 MPa with a WHSV of 3 h -1 , the feedstock was introduced into the catalyst together with hydrogen, wherein the ratio of hydrogen to feedstock was 900 Nl H2 / l feedstock.
[0154] The reactor is operated to a predetermined point (meeting the criteria for the end of the HDO catalyst life cycle), where the catalyst needs to be replaced due to the deactivation of the HDO catalyst, thereby replacing the catalyst material with fresh catalyst material. Most of the loose dust formed at the entrance of the classification layer is retained in the classification layer, about 80-90%, and the rest of the dust is carried onto the HDO catalyst. Figure 1 As shown, the formed dust was collected and analyzed by X-ray diffraction (XRD), and the total amount of accumulated phosphorus was quantitatively determined using ICP-MS / MS.
[0155] Figure 1 The dust in the reactor is shown to contain calcium iron phosphate (a) and sodium iron phosphate (b).
[0156] As described above, six HDO catalyst life cycle experiments were conducted to determine the phosphorus and metal content (and M:P ratio) in the pretreated feedstock directed to the HDO process, as well as the amount of dust generated. Table 1 shows the metal to phosphorus ratio (kg of metal calculated as elemental metal / kg of phosphorus calculated as elemental phosphorus) of the feed M:P for the six catalyst life cycle experiments.
[0157]
[0158] Table 1
[0159] Figure 2 The amount of metal phosphate dust ("trash dust") in kg filtered into fractions and main active HDO catalyst as a function of the ratio of metal to phosphorus (kg total metal / kg elemental phosphorus) is described. The amount of "trash dust" is normalized to the amount of main active HDO catalyst (kg). Figure 2 The dust in the layer refers to the precipitated impurities, mainly metal phosphates, entrained into the layer after operating the hydroprocessing reactor with different renewable feeds. The weight of the main active HDO catalyst is the weight initially loaded in the reactor. The M:P ratio is calculated based on the total amount of impurities fed to the reactor during operation.
[0160] Experiments in hydrodeoxygenation reactors have shown that the weight ratio of metal to phosphorus in the feedstock needs to be in the range of about 0.70-1.26 (see Figure 3), so that after a production cycle, only low levels of phosphorus of about 2.0 wt-% or less remain in the catalyst bed. Lower amounts of metal cause phosphorus to accumulate in the spent HDO catalyst material, while higher amounts also begin to increase the amount of phosphorus in the spent HDO catalyst. Figure 3 and Table 2 show the increase in the accumulation behavior (in wt-%) of phosphorus in the HDO catalyst bed as the metal to phosphorus weight ratio of the feedstock deviates from a minimum value of about 1.
[0161]
[0162] Table 2
[0163] The key factor identified as contributing to the formation of phosphate-rich impurity precipitates is the metal to phosphorus (M:P) weight ratio in the feed, which is positively correlated with the amount of impurity dust formed during the operation of the hydrodeoxygenation reactor, where different feedstocks have different M:P ratios. It was found that feeds with an M:P ratio of about 1 formed more impurity dust than feeds with lower or higher M:P ratios. In addition, the amount of phosphorus attached to the catalyst after the same operation was negatively correlated with the feed M:P ratio. The results obtained indicate that selecting the right M:P weight ratio can help prevent catalyst contamination with phosphorus, thereby extending the life of the catalyst.
[0164] The advantage of adjusting the M:P weight ratio and thereby minimizing the amount of P in the primary active HDO catalyst is that the activity of the catalyst can be maintained for a longer period of time, thereby achieving a higher overall throughput during the production cycle. For example, it was observed that in a production cycle with a feed M:P weight ratio of 0.63, 9436 kg of cumulative feedstock could be processed per kg of active HDO catalyst. In another production cycle, at a feed M:P weight ratio of 0.81, the cumulative feedstock processed increased by 60% to 15223 kg per kg of active HDO catalyst compared to the above cycle. Therefore, the higher throughput obtained when the feed M:P weight ratio is within the favorable range indicates that the catalyst is less deactivated, allowing operation at higher feed rates for longer periods of time.
[0165] Example 2
[0166] Brown grease-based raw material (1) and rendered poultry fat-based raw material (2) were pre-treated by degumming and bleaching. Brown grease-based raw material with a phosphorus content of 0.3 ppm and a metal (total of Na, Mg, K, Ca and Fe) content of 1.3 ppm was mixed with a rendered poultry fat-based raw material with a higher phosphorus content of 13.5 ppm and a metal (total of Na, Mg, K, Ca and Fe) content of 1.3 ppm. The weight-based mixing ratio of raw material (1) to raw material (2) was 2:1. The mixed raw materials obtained an M:P ratio of about 0.96.
[0167] The mixed feedstock was introduced into a fixed bed HDO reactor, which internally contained a graded layer upstream of the main catalyst bed according to Example 1, containing mainly alumina and a small amount of low activity NiMo catalyst.
[0168] The reactor was operated according to predetermined criteria for catalyst replacement. For experiments with M:P ratios in the range of 0.76 to 1.20, catalyst replacement was required due to deactivation after a slightly longer period of time than in Example 1 (approximately 5%).
[0169] It was not possible to operate the reactor correctly using feedstocks (1) and (2), respectively, due to the rapid degradation of the catalyst performance, which was attributed to the excessively high amount of metal or phosphorus depending on the feedstock.
[0170] It was concluded that even with unsuitable feeds it is possible to achieve good results provided they are adjusted to a metal to phosphorus ratio close to 1, for example by mixing the feeds appropriately together and heat treating them in the presence of hydrogen and a material capable of at least partial hydrotreating to enable the formation of a precipitate.
Claims
1. A method for reducing deactivation of a hydroprocessing catalyst, wherein the hydroprocessing catalyst is used as a primary active catalyst for producing renewable hydrocarbons from a renewable feedstock by hydroprocessing, the renewable feedstock containing as impurities at least one oxygen-containing compound, at least one metal-containing compound and at least one phosphorus-containing compound, the method comprising the steps of: i. adjusting the metal to phosphorus (M:P) weight ratio, measured as elemental metal and elemental phosphorus, of said renewable feedstock to a value in the range of 0.70 to 1.26 to obtain an impurity adjusted renewable feedstock, and ii. subjecting the impurity-adjusted renewable feedstock to a temperature of 190°C to 400°C under reducing conditions, thereby forming a solid precipitate comprising at least one metal- and phosphorus-containing compound, and a purified liquid renewable feedstock, and iii. contacting the purified liquid renewable feedstock with the primary active catalyst in the presence of hydrogen.
2. The process according to claim 1, wherein the adjustment in step i. is performed by blending into the renewable feedstock at least one additional renewable feedstock comprising a balanced amount of metal-containing compounds or phosphorus-containing compounds to obtain a metal to phosphorus weight ratio of 0.70 to 1.26 for the renewable feedstock for the impurity adjustment.
3. The method according to claim 2, wherein the balance of the metal-containing compound or phosphorus-containing compound is determined by: Firstly, the amount of metal (M1) and phosphorus (P1) in said renewable raw material in weight-% is determined, and Secondly, determining the amount of metal (M2) and phosphorus (P2) in weight-% of the at least one further renewable raw material, and Third, at least one additional raw material and its amount are selected to meet the requirement of a weight ratio of the total metal (M1+M2) amount to the total phosphorus (P1+P2) amount of 0.70 to 1.
26.
4. The process according to any one of claims 1 to 3, wherein the adjustment in step i. is carried out by adding at least one metal-containing compound to the renewable raw material, thereby obtaining a metal to phosphorus weight ratio of 0.70 to 1.26 for the impurity adjusted renewable raw material.
5. The method according to claim 4, wherein the at least one metal-containing compound is an ion-containing metal compound, preferably a hydroxide or a fatty acid salt.
6. The method according to claim 4 or 5, wherein the desired amount of the metal-containing compound to be added is determined by: - firstly, determining the amount of metal (M1) and the amount of phosphorus (P1) in said renewable raw material in weight-%, and - Secondly, the required amount of metal-containing compound (M2') to be added is calculated as elemental metal to achieve a total metal (M1+M2') to phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable feedstock.
7. The method according to any one of claims 1 to 3, wherein the adjustment in step i is performed by pre-treating the renewable raw material such as bleaching or degumming or both to reduce the amount of the phosphorus-containing compounds or metal-containing compounds, thereby obtaining a level of metal to phosphorus weight ratio of 0.70 to 1.26 for the renewable raw material wherein the impurities are adjusted.
8. The method according to claim 1, wherein the adjustment in step i is performed by any combination of the following methods: - blending at least one additional renewable raw material into the renewable raw material, the at least one additional renewable raw material comprising a compensating amount of a metal-containing compound or a phosphorus-containing compound, - adding a metal-containing compound to said renewable raw material, - Reduction of the amount of phosphorus-containing compounds or metal-containing compounds by pretreatment, A metal to phosphorus weight ratio of 0.70 to 1.26 for the impurity-adjusted renewable raw material is thereby obtained.
9. The method according to any one of claims 1 to 8, wherein the renewable raw material is pretreated before or after the conditioning of step i.
10. The process according to any one of claims 1 to 9, wherein the amount of metal-containing compounds and phosphorus-containing compounds in the purified liquid renewable feedstock is reduced to a value of less than 20 ppm of metals calculated as elemental metals and less than 20 ppm of phosphorus calculated as elemental phosphorus as measured by ICP-AES.
11. The method according to any one of claims 8 to 10, wherein the pretreatment comprises filtering, settling, centrifuging, washing, degumming or bleaching or any combination thereof.
12. The method according to any one of claims 1 to 11, wherein the renewable feedstock contains triglycerides and / or free fatty acids.
13. The method of claim 12, wherein the triglycerides and / or free fatty acids are derived from a feedstock comprising at least one of acidulated soapstock, poultry fat, rendered poultry fat, brown grease, waste cooking oil, tall oil, tall oil fractions, crude tall oil, tall oil pitch, palm oil mill effluent, crude palm oil, palm oil, palm kernel oil, palm fatty acid distillate, babassu oil, carinata oil, coconut butter, musk butter, sesame oil, corn oil, Oil, poppy seed oil, cotton seed oil, soybean oil, bay seed oil, jatropha oil, palm kernel oil, camellia oil, archaea oil, bacterial oil, fungal oil, protozoa oil, algae oil, algae oil, mustard oil, halophile oil, soybean oil, industrial corn oil, rapeseed oil, rapeseed oil, canola oil, sunflower oil, hemp seed oil, olive oil, linseed oil, mustard oil, peanut oil, castor oil, coconut oil, lard, tallow, whale oil, spent clay oil, lignocellulose based feed or mixtures thereof.
14. The method of any one of claims 1-13, wherein the hydrotreating comprises hydrodeoxygenation; combined hydrodeoxygenation and isomerization; or continuous hydrodeoxygenation and isomerization.
15. The process according to any one of claims 1 to 14, wherein the main active catalyst comprises a catalyst suitable for hydrodeoxygenation or combined hydrodeoxygenation and isomerization.
16. The process according to claim 14 or 15, wherein the hydrodeoxygenation is carried out in a hydrodeoxygenation reactor or zone in the presence of at least the pro-active catalyst, the pro-active catalyst comprising a metal on a support.
17. The method of claim 16, wherein the metal comprises Pd, Pt, Ni, Co, Mo, Ru, Rh, W or any combination thereof, and the support comprises alumina, silica, zirconia, zeolite or a mixture thereof.
18. The method of any one of claims 13-17, wherein the hydroprocessing further comprises directing the impurity-adjusted renewable feedstock through a heated pretreatment zone, the heated pretreatment zone preferably being located upstream of the primary active catalyst.
19. The method of claim 18, wherein the heated pretreatment zone comprises a compound that is less active for hydrodeoxygenation than the primary active catalyst, such as a compound that is inactive for hydrodeoxygenation.
20. A process according to claim 18 or 19, wherein the solid precipitate formed in step ii. is retained in the heated pre-treatment zone.
21. The method according to any one of claims 1-20, wherein the elevated temperature in step ii. is from 240°C to 380°C, such as from 250°C to 370°C, or even from 260°C to 360°C.
22. The method according to any one of claims 1 to 21, wherein the metal to phosphorus (M:P) weight ratio measured as elemental metal and elemental phosphorus of the renewable feedstock is adjusted to a value in the range of 0.73 to 1.25 to obtain an impurity adjusted renewable feedstock.
23. The method of any one of claims 1-22, wherein the reducing conditions comprise the presence of hydrogen or water.
Citation Information
Patent Citations
Production of diesel fuel from renewable feedstocks containing phosphorus
US20090321311A1
Purification of feedstock by heat treatment
US20190203154A1
Purification of recycled and renewable organic material
US20210292657A1
A method for treating lipid materials
US20220073840A1