Water electrolysis catalyst comprising iridium oxide powder, electrode film for water electrolysis, and film with catalyst layer
By using amorphous iridium oxide powder as the water electrolytic catalyst and appropriately mixing it with ionomers, the problem of insufficient activity and durability of the anode electrode film in the prior art is solved, and the effect of efficient hydrogen generation and low oxygen overvoltage is achieved. .
Patent Information
- Application Number
- CN202380022333.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-01
AI Technical Summary
The existing water electrolytic catalysts are difficult to meet the requirements of high activity and low oxygen overvoltage in the anode electrode film, and at the same time, the durability is insufficient, which affects the hydrogen generation efficiency.
Using a water electrolytic catalyst composed of amorphous iridium oxide powder, the activity and durability of the catalyst are improved by adjusting the production method and structure, and appropriately mixed with the ionomer to reduce the oxygen overvoltage.
A water electrolytic catalyst with high activity and low oxygen overvoltage is achieved, which improves hydrogen generation efficiency and exhibits excellent proton conductivity and voltage efficiency in solid electrolyte-type water electrolytic device.
Smart Images

Figure CN118891398A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a water electrolysis catalyst for electrolyzing water to generate hydrogen, an electrode membrane for water electrolysis containing the catalyst, and a membrane with a catalyst layer, and particularly to a water electrolysis catalyst composed of iridium oxide powder. Background Art
[0002] In view of the increasingly serious environmental and energy problems in recent years, the utilization of hydrogen as a renewable new energy source is highly anticipated. For example, the development and practical application of hydrogen engines that use hydrogen as a direct fuel and fuel cells that use hydrogen as a fuel to generate electricity are underway.
[0003] In order to effectively use hydrogen as an energy source, it is necessary to stably and safely manufacture and supply it. So far, hydrogen has been manufactured by steam reforming fossil fuels, but from the perspective of environmental issues and fossil fuel depletion, the importance of hydrogen generation processes using water electrolysis has increased. As hydrogen generation processes using water electrolysis, they are roughly divided into three types: alkaline water electrolysis, solid polymer water electrolysis, and water vapor electrolysis. Among these, solid polymer water electrolysis can produce hydrogen more efficiently than alkaline water electrolysis, so future development is expected.
[0004] In solid polymer water electrolysis, an electrolytic cell (single cell) is formed by sandwiching a solid polymer electrolyte membrane (PEM) as an electrolyte between an anode / cathode electrode and a power supply, and a water electrolysis device formed by stacking multiple electrolytic cells is used. Most solid polymer electrolyte membranes use proton-conductive fluororesin-based ion exchange membranes (perfluorocarbon sulfonic acid membranes). In addition, a catalyst layer composed of a water electrolysis catalyst is used as the anode and cathode electrodes. In recent years, a catalyst-coated membrane (CCM) with a catalyst layer formed on an electrolyte membrane as an electrode membrane composed of a mixture of water electrolysis catalyst particles and a solid electrolyte (ionomer) has been used as a main component of a water electrolysis device.
[0005] The present application relates to a catalyst for water electrolysis suitable for an anode electrode membrane in a water electrolysis device. Here, as a catalyst for water electrolysis to date, a noble metal catalyst formed by loading a noble metal on an inorganic oxide is known. For example, a catalyst formed by loading iridium oxide or ruthenium oxide on a tin oxide carrier as an inorganic oxide can be cited.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 5199575
[0009] Patent Document 2: Japanese Patent Application No. 2020-500692 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The efficiency of hydrogen production using a water electrolysis device depends largely on the performance of the electrode membrane. In this regard, the anode electrode membrane is required to have high activity, low oxygen overvoltage, and good voltage effect. In addition, the anode electrode membrane is also required to be durable. This is because the solid polymer electrolyte membrane as an electrolyte is a resin membrane with strong acidity such as sulfonic acid groups, and the anode supplied with water is exposed to a severe corrosive environment.
[0012] In the above-mentioned conventional water electrolysis catalysts, reducing oxygen overvoltage and ensuring corrosion resistance are also considered. However, it is difficult to say that they fully correspond to the above-mentioned required characteristics, and there is room for improvement. In addition, the performance of the electrode membrane should be evaluated in the state of becoming an electrode, rather than based solely on the performance of the catalyst. Highly active catalysts are also difficult to exert their capabilities due to the composition of the electrode membrane. That is, in order to improve the efficiency of hydrogen production using a solid electrolyte water electrolysis device, a comprehensive study should be conducted on both the water electrolysis catalyst and the electrode composition.
[0013] As mentioned above, hydrogen is a highly anticipated energy source as a renewable energy source. In addition to fuel cells, it is also expected to be used in raw material applications such as synthetic natural gas and industrial applications in oil refineries / iron factories. Hydrogen is suitable for storage and transportation, and hydrogen production using water electrolysis can effectively utilize surplus electricity. Therefore, water electrolysis technology has become one of the most powerful technologies for large-scale power storage technology. In order to make this water electrolysis technology practical, comprehensive research is required. The present invention was completed under such a background, and clarified the composition of the water electrolysis catalyst suitable for the anode electrode membrane in the solid electrolyte water electrolysis device and the electrode membrane that enables it to function effectively.
[0014] Means for solving problems
[0015] As can be known from the above-mentioned prior art (patent documentation 1, 2), it is known that iridium oxide has the activity as a water electrolysis catalyst. Iridium oxide is a noble metal oxide of electrical conductivity and has physical / chemical stability, and is therefore useful as an electrode catalyst. Moreover, the above-mentioned water electrolysis catalyst in the past is the form of a loaded catalyst formed by loading noble metals such as iridium oxide on an inorganic oxide carrier.
[0016] Relative to this prior art, the inventors etc. first in order to realize the optimization of the form of water electrolysis catalyst, the powder consisting of iridium oxide is used as water electrolysis catalyst. The present invention is different from these supported catalysts, and only using iridium oxide powder to constitute catalyst is to give high conductivity to water electrolysis catalyst. Because water electrolysis catalyst is the material that constitutes electrode (anode) together with ionomer, therefore originally just require conductivity. As the previous water electrolysis catalyst of supported catalyst, due to the insufficient conductivity of the inorganic oxide as carrier, the conductivity of catalyst itself is reduced. The inventors, in order to maintain conductivity, only use iridium oxide powder to constitute water electrolysis catalyst.
[0017] In addition, the inventor believes that, considering the use environment of water electrolysis catalyst, it is not preferred to mix / dope other metals / noble metals in iridium oxide powder. For example, in the water electrolysis catalyst of above-mentioned patent document 1, although the oxygen overvoltage of ruthenium oxide added to iridium oxide is low, the durability is worse than iridium oxide. And, owing to ionization and separation in electrolysis, the durability of the catalyst as a whole is reduced. Not only ruthenium oxide, but also the addition of metals etc. also has an impact on durability. Therefore, the inventor believes that water electrolysis catalyst should be constituted only by iridium oxide powder without intentionally adding elements.
[0018] Here, about iridium oxide powder, it is known that there is crystalline iridium oxide of rutile structure manufactured by various methods. The preliminary confirmation test of the inventor also confirmed that the catalytic activity for water electrolysis is exerted in the crystalline iridium oxide powder. In addition, the inventor examined that by adjusting the manufacturing method, etc., iridium oxide powder that can exert higher activity can be obtained, and conducted in-depth research. It was found that in the powder composed of amorphous iridium oxide, further catalytic activity was shown, thereby thinking of the present invention.
[0019] That is, the present invention is a water electrolysis catalyst, which is composed of iridium oxide powder, the iridium oxide powder contains amorphous iridium oxide powder, and the average particle size of the iridium oxide powder is 0.01 μm or more and 30 μm or less. The composition and production method of the water electrolysis catalyst according to the present invention and the electrode membrane for water electrolysis preferably using the water electrolysis catalyst are described below.
[0020] (A) Water electrolysis catalyst and method for producing the same according to the present invention
[0021] As described above, the water electrolysis catalyst of the present invention is composed of iridium oxide powder. Moreover, the water electrolysis catalyst at least partially contains powder composed of amorphous iridium oxide. That is, the water electrolysis catalyst of the present invention is composed only of amorphous iridium oxide, or is a mixture of amorphous iridium oxide and crystalline iridium oxide (rutile IrO2).
[0022] According to the research of the present inventors, amorphous iridium oxide has a low oxygen overvoltage relative to crystalline iridium oxide and shows high activity. Although the reason may not be clear, the present inventors have examined that the electron state changes and the activity is improved due to the oxygen defects or deformation of the crystal structure that are believed to be contained in the amorphous iridium oxide powder.
[0023] The water electrolysis catalyst of the present invention can be composed entirely of amorphous iridium oxide powder, or can partially contain crystalline iridium oxide. This is because crystalline iridium oxide powder is also active in water electrolysis reaction. As the ratio of amorphous iridium oxide in the catalyst, based on the mass of the entire catalyst, it is preferably set to more than 15 mass %. This is because, when the ratio of amorphous iridium oxide powder is less than 15 mass % by mass ratio, there is no difference in the activity of the catalyst with only crystalline iridium oxide. The ratio of amorphous iridium oxide powder is more preferably set to 20 mass %, more preferably more than 30 mass % by mass ratio. And, it is particularly preferred to make the entire catalyst amorphous iridium oxide (100 mass %).
[0024] The water electrolysis catalyst composed of iridium oxide powder of the present invention shows specific behavior in thermal analysis method or crystallographic analysis method due to the amorphous iridium oxide that it necessarily contains. As a thermal analysis method, thermogravimetric differential thermal analysis (TG-DTA analysis) can be cited. TG-DTA is an analysis method that measures the mass change of the sample (TG) and the temperature difference (differential thermal) between the sample and the reference substance while heating the sample and the reference substance. When the water electrolysis catalyst according to the present invention is subjected to TG-DTA analysis, it shows an exothermic peak in the region of 300°C to 450°C. This exothermic peak is exhibited because the amorphous iridium oxide is converted into crystalline (rutile) iridium oxide by heating. In the ordinary crystalline iridium oxide powder, such an exothermic peak is not shown, so the exothermic peak of TG-DTA is particularly useful in determining the water electrolysis catalyst according to the present invention.
[0025] In addition, the water electrolysis catalyst of the present invention can also be determined by X-ray diffraction analysis (XRD), which is widely known as a crystallographic analysis method. In the XRD diffraction pattern of the water electrolysis catalyst of the present invention, amorphous iridium oxide shows a wide peak. The diffraction peak position of amorphous iridium oxide is different from that of crystalline iridium oxide, and is observed at at least any one angle of 2θ=22°, 34°, and 58°. However, the water electrolysis catalyst of the present invention sometimes contains crystalline iridium oxide powder, in which case the diffraction pattern of crystalline iridium oxide is also observed. Therefore, the diffraction peak of amorphous iridium oxide is sometimes difficult to distinguish due to the overlap with the diffraction peak of crystalline iridium oxide. In this regard, even if it is a catalyst containing crystalline iridium oxide powder, the exothermic peak in the region of 300°C to 450°C in the above-mentioned TG-DTA can be observed, so it is convenient to determine the water electrolysis catalyst of the present invention.
[0026] The water electrolysis catalyst of the present invention is preferably composed of only amorphous iridium oxide or only amorphous and crystalline iridium oxide, and the iridium oxide is of high purity. It is particularly preferred to reduce the predetermined impurity elements. Here, as impurity elements that should be particularly limited, Na, Cl, and Fe can be listed.
[0027] The Na content of the water electrolysis catalyst of the present invention is preferably less than 100ppm, and the Cl content is preferably less than 100ppm. In the water decomposition reaction that promotes water electrolysis, since the protons generated at the anode are effectively conducted in the electrode membrane, the catalyst constituting the electrode membrane needs proton conductivity. In addition, Na in the iridium oxide powder may become a cause of reduced proton conductivity due to cationization during electrolysis. In addition, since Cl promotes the deterioration of parts and components of device equipment, batteries, etc., it is preferred to limit Cl. Therefore, in the present invention, it is preferred that the contents of Na and Cl in the iridium oxide powder are respectively limited within the above range.
[0028] In addition, Fe is an impurity that tends to accelerate the generation of free radicals in water electrolysis. The generated free radicals attack the sulfonic acid portion of the solid electrolyte membrane, causing an unzipping reaction, which affects the durability of the solid electrolyte membrane. Therefore, in the water electrolysis catalyst of the present invention, the Fe content is preferably set to 100 ppm or less.
[0029] In addition to the above impurities, unavoidable impurity elements include Cu, Al, Mn, Zn, etc. The total content of these impurities is preferably 100 ppm or less.
[0030] It should be noted that, in the water electrolysis catalyst to which the present invention relates, the amorphous iridium oxide powder as its necessary composition can contain water (water of crystallization). The intermolecular bonding of amorphous iridium oxide is loose, and sometimes captures water of crystallization inside. Considering that the treatment object of water electrolysis catalyst is water, such water of crystallization does not become impurities. In addition, the regulation of its content is not particularly necessary. In addition, even amorphous iridium oxide may not always contain water of crystallization.
[0031] In addition, in the case where the water electrolysis catalyst of the present invention contains amorphous iridium oxide, its ratio can be estimated by TG-DTA analysis or Ir concentration analysis using a standard curve method. As described above, when performing TG-DTA analysis, the amorphous iridium oxide that is necessarily contained in the water electrolysis catalyst of the present invention exhibits an exothermic peak in the region of 300°C to 450°C. The peak intensity increases or decreases according to the proportion of amorphous iridium oxide in the water electrolysis catalyst. Therefore, TG-DTA analysis can be performed in advance on both a catalyst consisting only of amorphous iridium oxide and a catalyst not containing amorphous iridium oxide (a catalyst consisting only of crystalline iridium oxide), and the peak intensity of the exothermic peak of the catalyst consisting only of amorphous iridium oxide is measured, thereby preparing a standard curve. In addition, in this case, by preparing a water electrolysis catalyst with a known ratio of more than one amorphous iridium oxide and measuring the intensity of its exothermic peak, the accuracy of the standard curve can be improved. Then, regarding the TG-DTA analysis of the water electrolysis catalyst to be measured, the proportion of amorphous iridium oxide can be estimated based on the presence or absence and intensity of an exothermic peak in the region of 300° C. to 450° C.
[0032] In addition, the ratio of amorphous iridium oxide in the water electrolysis catalyst can also be estimated according to its Ir concentration. As mentioned above, the amorphous iridium oxide powder used in the present invention tends to contain water (crystallization water). Due to the water contained, the water electrolysis catalyst containing amorphous iridium oxide powder tends to slightly reduce the Ir concentration relative to the water electrolysis catalyst consisting of crystalline iridium oxide powder. Therefore, the Ir concentration in the catalyst consisting only of amorphous iridium oxide and the catalyst not containing amorphous iridium oxide can be measured, and a standard curve can be made according to them. In this case, the Ir concentration of the water electrolysis catalyst known by measuring the ratio of amorphous iridium oxide can also be supplemented, thereby improving the accuracy of the standard curve. By the standard curve based on the Ir concentration, the ratio of amorphous iridium oxide in the water electrolysis catalyst as the object of measurement can be estimated. It should be noted that, as mentioned above, when considering the influence of crystal water, the Ir concentration of the water electrolysis catalyst containing amorphous iridium oxide of the present invention is preferably 70 mass % or more and 85 mass % or less. In addition, since the Ir concentration varies depending on the content of amorphous iridium oxide containing crystal water, a more preferred Ir concentration is 82 mass % or less, and a further preferred Ir concentration is 80 mass % or less.
[0033] The average particle size of the iridium oxide powder constituting the water electrolysis catalyst of the present invention is 0.01 μm or more and 30 μm or less. When it is less than 0.01 μm, Ir may be dissolved during use and the catalyst may be degraded. When it exceeds 100 μm, the activity may be reduced with the reduction of the reaction area, affecting the proton conductivity or conduction in the catalyst layer. The average particle size is the average value (volume average particle size (M)) of the particles of the iridium oxide powder constituting the water electrolysis catalyst. V )). Even when amorphous iridium oxide powder and crystalline iridium oxide powder are mixed, the calculation is based on all the iridium oxide powder.
[0034] The average particle size of the iridium oxide powder constituting the water electrolysis catalyst can be determined using various commercially available particle size / particle size distribution measuring devices. For example, in a laser diffraction / scattering particle size distribution measuring device, the particle size of the iridium oxide powder can be determined by dry method. In addition, the particle size of a plurality of iridium oxide powders can also be determined based on the observed image of an electron microscope (SEM, TEM), and its average value can be obtained.
[0035] In addition, the specific surface area of the iridium oxide powder is preferably 5 m 2 / g above 200m 2 The specific surface area of the iridium oxide powder can be measured by a gas adsorption method or the like.
[0036] Next, the method for manufacturing the iridium oxide powder constituting the water electrolysis catalyst of the present invention is described. Since the water electrolysis catalyst of the present invention is composed of amorphous iridium oxide powder as a whole or in part, it is necessary to manufacture amorphous iridium oxide powder. In this regard, several methods are known for manufacturing crystalline rutile iridium oxide powder. As a method for manufacturing crystalline iridium oxide powder, for example, the ADAMS method known since ancient times as a method for manufacturing precious metal oxide particles can be cited. Regarding the method for manufacturing iridium oxide powder using the ADAMS method, a solution obtained by adding nitrate (NaNO3, etc.) to an iridium chloride solution is evaporated and dried to absorb heat, NO2 gas is generated / removed, and further heated at more than 500°C, thereby obtaining iridium oxide. In addition, as a method for manufacturing iridium oxide powder, there is a precipitation method via iridium hydroxide. In the precipitation method, a solution of an iridium compound such as iridium chloride is used as a raw material, and the solution is neutralized with an alkali to precipitate a hydroxide (Ir(OH)4, etc.). Then, the iridium hydroxide is dehydrated and calcined to obtain iridium oxide powder.
[0037] The present inventors have found a method for producing amorphous iridium oxide powder with reference to the method for producing crystalline iridium oxide powder. In this method, iridium hydroxide is generated according to the precipitation method, and amorphous iridium oxide powder is produced by subsequent temperature management. The method for producing amorphous iridium oxide powder is described below.
[0038] As the raw material of iridium compound, iridium chloride (IrCl3), iridium chloride (H2IrCl6), iridium nitrate (Ir(NO3)3), iridium sulfate ((Ir2(SO4)3)) and the like are used. Iridium hydroxide is generated by adding a base to the aqueous solution of these iridium compounds. There is no particular restriction on the base added at this time. The temperature of the reaction system during alkali neutralization is preferably set to above 60°C and below 95°C. When it is below 60°C, the neutralization reaction proceeds slowly, so the nucleation becomes slow and the particles are likely to become coarse. In addition, when it exceeds 95°C, it is difficult to produce stable nucleation due to the boiling of the solution. In addition, due to evaporation, the concentration changes, making it difficult to carry out a stable neutralization reaction.
[0039] By dehydrating and drying the iridium hydroxide generated / precipitated by the neutralization reaction after recovery, iridium oxide powder can be obtained. At this time, in order to obtain amorphous iridium oxide powder, it is preferred to adjust the drying temperature to 40°C or more and 300°C or less. When it is lower than 40°C, the drying time becomes very long. And, when drying at a temperature exceeding 300°C, although only a part, it is possible to produce amorphous iridium oxide crystallization. The more preferred drying temperature is set to 50°C or more and 90°C or less. The drying time is adjusted according to the drying temperature, preferably set to 1 hour or more and 30 hours or less. Amorphous iridium oxide powder can be obtained by this drying treatment, and then no calcination treatment is carried out by heating at a higher temperature. This is because it becomes crystalline by calcination treatment. It should be noted that it is preferred to wash the iridium hydroxide recovered before drying. This is to remove unpreferred impurity elements such as Na and Cl. Cleaning can be carried out by appropriately combining pure water and acid (nitric acid, etc.).
[0040] The amorphous iridium oxide powder obtained by the above-mentioned preparation method can be used as a water electrolysis catalyst. In addition, the amorphous iridium oxide powder thus prepared can be mixed with crystalline iridium oxide powder to be used as a water electrolysis catalyst. As for the crystalline iridium oxide powder at this time, the material obtained by the preparation method such as the above-mentioned ADAMS method can be mixed, or commercially available crystalline iridium oxide powder can be obtained.
[0041] In addition to the above-mentioned mixing method, the water electrolysis catalyst containing crystalline iridium oxide powder can also be manufactured by heat treatment of amorphous iridium oxide powder. As mentioned above, amorphous iridium oxide powder becomes crystalline iridium oxide by heating. Therefore, by sintering the amorphous iridium oxide powder to make it partially crystalline, a mixed iridium oxide powder can be obtained. The sintering is preferably carried out at 300°C or above and 1040°C or below. When it is lower than 300°C, the structural change from amorphous to crystalline does not occur. In addition, when it exceeds 1040°C, the iridium oxide powder is likely to become iridium metal. In the case of obtaining a water electrolysis catalyst composed of amorphous and crystalline iridium oxide powders by sintering such amorphous iridium oxide powder, their mixing ratio can be adjusted by the treatment time. The treatment time depends on the sintering temperature.
[0042] (B) Electrode membrane for water electrolysis and membrane with catalyst layer (CCM) according to the present invention
[0043] Next, the electrode membrane for water electrolysis according to the present invention and a membrane with a catalyst layer (CCM) having the electrode membrane will be described. The electrode membrane for water electrolysis according to the present invention is a mixture of the above-mentioned water electrolysis catalyst and an ionomer.
[0044] In the anode electrode membrane of the water electrolysis device, in order to+ ) is quickly transferred to the polymer electrolyte membrane, which requires proton conductivity. In addition, the electrode membrane originally requires electrical conductivity. The ionomer of the electrode membrane for water electrolysis is a proton conductor, and on the other hand, it is an insulator (resistor). The water electrolysis catalyst composed of the iridium oxide powder of the present invention is a conductor, but has no proton conductivity. Therefore, when the mixing amount of the ionomer increases, the proton conductivity increases, and on the other hand, the electrical conductivity decreases, and the mixing amount of the catalyst has an opposite tendency.
[0045] The inventors of the present invention have found a suitable configuration for an electrode membrane to which the water electrolysis catalyst (iridium oxide powder) according to the present invention is applied, while considering the above-mentioned inverse relationship between the mixing amounts (mixing ratio) of the catalyst and the ionomer. That is, the mass of iridium (mg / cm 2 ) and the mass of the ionomer (mg / cm 2 ), the mixing ratio per unit area of the catalyst for water electrolysis and the ionomer is preferably iridium: ionomer = 2: 1 or more and 5: 1 or less. This mixing ratio can reduce the oxygen overvoltage of the anode electrode membrane, thereby forming an electrode membrane with excellent voltage efficiency.
[0046] The water electrolysis catalyst constituting the water electrolysis electrode membrane of the present invention is as described above. On the other hand, as the ionomer mixed with the catalyst, cation exchange resins of fluorine resins having sulfonic groups, carboxyl groups, and phosphino groups can be cited. They are known by the product name of Nafion (registered trademark), and products of the dispersed solution type can be preferably used. The concentration of the dispersed solution is generally 5% by mass or more and 20% by mass, and can be obtained from the market.
[0047] The thickness of the electrode membrane for water electrolysis of the present invention is preferably 2 μm or more and 10 μm or less. It is difficult to form a thin electrode membrane of less than 2 μm, and even if it can be formed, it lacks durability. On the other hand, when the thickness of the electrode membrane increases, the active points increase due to the increase in the content of the water electrolysis catalyst or the increase in the porosity, while the proton conductivity decreases. Considering the balance between the active points and the proton conductivity, the thickness of the electrode membrane is preferably set to the above range.
[0048] The electrode membrane for water electrolysis according to the present invention is useful as an anode electrode of a CCM in a water electrolysis device. As described later, the electrode membrane is formed by coating a mixed solution containing the above-mentioned water electrolysis catalyst on a polymer electrolyte membrane.
[0049] In the CCM of the water electrolysis device, a cathode electrode membrane is formed together with the above-mentioned anode electrode membrane. The cathode electrode membrane is a mixture of a hydrogen generation catalyst and an ionomer. As a hydrogen generation catalyst, a platinum-loaded carbon catalyst (Pt / C catalyst) or the like is applied. However, in the present invention, there is no particular limitation on the composition and membrane thickness of the cathode electrode membrane.
[0050] In the CCM of the present invention, for the electrode film of the present invention as the anode, it is preferred that the iridium content per unit coating area (Ir 1mg cm -2 ) is 0.50C or more. The increase in capacitance improves the voltage efficiency of water electrolysis using CCM. The water electrolysis catalyst composed of the iridium oxide powder of the present invention has a high specific surface area, suitable electrical conductivity and proton conductivity. By using the water electrolysis catalyst, the capacitance of the electrode membrane can be increased to the above range.
[0051] In addition, for the polymer electrolyte membrane of the CCM involved in the present invention, its material is the same as that of the prior art and is not particularly limited. As the polymer electrolyte membrane, a cation exchange membrane of a fluorine resin system having a sulfonic group, a carboxyl group, and a phosphine group having the same composition as the ionomer of the electrode membrane is known. They are known by the product name of Nafion (registered trademark), and as their models, 112, 115, 117, 450, etc. can be preferably used. From the reason of the overvoltage generated by the resistance of the membrane, the thickness of the polymer electrolyte membrane is preferably thinned. On the other hand, considering the cross leakage, the thickness of the polymer electrolyte membrane is preferably thickened. Taking into account the balance between the two, the thickness of the polymer electrolyte membrane is preferably 10 μm or more and 200 μm or less, more preferably 50 μm or more and 150 μm or less.
[0052] Furthermore, the CCM of the present invention constitutes a unit electrolytic cell together with components such as a power supply. The power supply uses a structure having conductivity and capable of circulating gas and liquid. As examples, a powder sintered body of a metal such as Ti, Ta, stainless steel, expanded metal, metal mesh, porous body (sponge metal), etc. can be used.
[0053] The electrode membrane for water electrolysis of the present invention can be manufactured by using the polymer electrolyte membrane that will become the electrolytic cell as a substrate, and coating a mixed solution (sometimes also referred to as ink, paste, slurry, etc.) of a water electrolysis catalyst and an ionomer thereon. As the dispersion medium of the mixed solution, water, 1-propanol, etc. can be applied. In addition, when using a solution-type Nafion liquid, the dispersion medium directly becomes the dispersion medium of the mixed solution. The ionomer used for the electrode membrane can be obtained in a dispersed solution state, and a mixed solution can be made by adding iridium oxide powder therein. There is no particular restriction on the coating method of the dispersion medium. The substrate can be immersed in the mixed solution, or a drip method, a spray method, etc. can be used.
[0054] After the mixed solution is applied, a heat treatment is performed to form an electrode film. The heating temperature at this time is preferably set to 100°C or more and 130°C or less. In addition, pressure can be applied while heating to form the electrode film and press it onto the substrate. The pressure at this time is preferably set to 100kgf / cm based on the coating area. 2 This is because applying too much pressure will destroy the pores in the electrode membrane and reduce the active points of the catalyst. The pressure is more preferably set to 10 kgf / cm 2 Above 75kgf / cm 2 As such a process of simultaneously applying pressure and heating, hot pressing can be cited.
[0055] It should be noted that the manufacture of the electrode membrane of the present invention can be carried out simultaneously with the cathode electrode membrane in the manufacturing stage of CCM. The cathode electrode membrane is also manufactured by coating and pressing the mixed solution of the hydrogen generation catalyst. The CCM is manufactured by coating the mixed solution as the anode electrode membrane and the cathode electrode membrane on each surface of the polymer electrolyte membrane as the substrate and hot pressing at the same time.
[0056] Effects of the Invention
[0057] As described above, the present invention relates to a water electrolysis catalyst suitable for an anode electrode membrane in a solid electrolyte type water electrolysis device. The iridium oxide powder of the present invention has excellent proton conductivity while maintaining water electrolysis activity. Moreover, in the electrode membrane of the iridium oxide powder, by setting a suitable catalyst mixing ratio, the oxygen overvoltage in water electrolysis is reduced, and the voltage efficiency is excellent. In addition to the hydrogen generation device of the solid electrolyte type water electrolysis, the present invention is also useful in an alkaline ion water purifier and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] [ Figure 1 ] is a diagram showing an XRD diffraction pattern of a water electrolysis catalyst composed of amorphous iridium oxide powder produced in the first embodiment.
[0059] [ Figure 2 ] is a graph showing the TG-DTA curve of the amorphous water electrolysis catalyst (iridium oxide powder) produced in the first embodiment.
[0060] [ Figure 3 ] is a graph showing the IV characteristic curve in water electrolysis of the CCM manufactured in the first embodiment.
[0061] [ Figure 4 ] is a graph showing a CV curve in water electrolysis of the CCM manufactured in the first embodiment.
[0062] [ Figure 5] is a graph showing IV characteristic curves in water electrolysis of CCMs having different catalyst mixing ratios manufactured in the second embodiment.
[0063] [ Figure 6 ] is a diagram showing a DTA curve of a water electrolysis catalyst composed of iridium oxide powder having different contents of amorphous iridium oxide produced in the third embodiment.
[0064] [ Figure 7 ] is a graph showing the relationship between the content of amorphous iridium oxide and DTA at the exothermic peak intensity.
[0065] [ Figure 8 ] is a graph showing the relationship between the content of amorphous iridium oxide and the Ir concentration.
[0066] [ Fig. 9 ] is a graph showing the relationship between the content of amorphous iridium oxide powder of CCM manufactured in the third embodiment and the battery voltage. DETAILED DESCRIPTION
[0067] First Embodiment : The following is an explanation of an embodiment of the present invention. In this embodiment, amorphous iridium oxide powder was produced by precipitation method, and CCM was produced using the powder as a water electrolysis catalyst. Then, the electrolysis characteristics were evaluated.
[0068] [Manufacturing of amorphous iridium oxide powder]
[0069] Iridium chloride as a raw material is made into an aqueous solution (concentration 100 g / L), and the aqueous solution is added to a NaOH solution maintained at 90°C for neutralization. Thus, a precipitate of iridium hydroxide is generated / precipitated. The precipitate is recovered by vacuum filtration and washed with 60°C pure water and nitric acid. Then, the hydroxide is dried at 60°C for 22 hours. Thus, amorphous iridium oxide powder is manufactured.
[0070] The iridium oxide powder produced was analyzed by ICP, and it was confirmed that the contents of Na and Cl were both less than 100 ppm. In addition, it was confirmed that the total content of Fe, Cu, Al, Mg, Cr, and Mn was also less than 100 ppm. In addition, the particle size of the iridium oxide powder was measured using a laser diffraction / scattering particle size distribution measuring device (Horiba, Ltd.: LA950), and the average particle size was 4.2 μm.
[0071] Next, the manufactured amorphous iridium oxide powder was subjected to XRD and TG-DTA. In XRD, an XRD analyzer (Rigaku Corporation: miniFlex) was used to set the X-ray source to Cu kα rays to measure the diffraction pattern. In addition, in TG-DTA, a differential thermal balance analyzer (NETZSCH Japan KK: STA2500 Regulus) was used, and the standard sample was set to α-alumina and the heating rate was set to 5°C / min for analysis. In these analyses, in addition to the amorphous iridium oxide powder manufactured in the present embodiment, a rutile-type crystalline iridium oxide powder was also analyzed for comparison. The rutile-type iridium oxide powder is manufactured by sintering the amorphous iridium oxide involved in the present embodiment manufactured as described above at 600°C.
[0072] Figure 1 The XRD diffraction pattern of the amorphous iridium oxide powder manufactured in the present embodiment is shown. Compared with the diffraction pattern of the crystalline iridium oxide powder, the amorphous iridium oxide powder is observed to have a wide peak. It can be confirmed that the peak positions of these peaks are different from the peak positions of the crystalline iridium oxide powder.
[0073] Figure 2 It is the result of TG-DTA. From the measurement results of the amorphous iridium oxide powder manufactured in the present embodiment, a mass reduction is observed after about 100°C from the beginning of the sample heating. This mass reduction is believed to be caused by the evaporation of the crystal water contained in the amorphous iridium oxide powder. The mass reduction caused by the detachment of the crystal water is not observed in the TG curve of the crystalline iridium oxide powder. In addition, in the DTA curve of the amorphous iridium oxide powder of the present embodiment, a clear exothermic peak is observed at about 350°C. This exothermic peak is believed to be caused by the structural change from amorphous iridium oxide to crystalline iridium oxide. In this way, it is confirmed that the amorphous iridium oxide powder, which is a necessary component of the water electrolysis catalyst of the present invention, shows a behavior that is significantly different from that of the crystalline iridium oxide powder when the TG-DTA analysis is performed.
[0074] [Manufacturing of CCM]
[0075] Next, the amorphous iridium oxide powder was used as a water electrolysis catalyst (anode electrode membrane) to manufacture CCM. 2 g of iridium oxide powder and 10 g of ionomer (Nafion dispersion (DE520) manufactured by Aldrich Chemical Company Inc.) were mixed to manufacture ink. During mixing, the catalyst and ionomer were mixed while being crushed and stirred using a bead mill (crushing medium: 2 mm). The ink was applied on a polymer electrolyte membrane (Nafion115, size: 70 mm×70 mm) with a thickness of 127 μm. The ink was applied using a sprayer, and the Ir coating amount was set to 1 mg / cm 2 The coating area was set to 3.3 cm×3.3 cm. In addition, a commercially available platinum catalyst ink was applied to the other side of the polymer electrolyte membrane by a spray coater to form a cathode electrode membrane.
[0076] After coating the catalyst inks that will become the electrode membranes on both sides of the polymer electrolyte membrane, they were pressed together using a hot press. The pressing conditions at this time were 120°C and 50 kgf / cm 2 The pressure was applied for 30 minutes. Thus, an electrode with a thickness of about 7 μm and an electrolysis area of about 10 cm was produced. 2 In this embodiment, the mixing ratio per unit area of the water electrolysis catalyst and the ionomer in the anode electrode membrane is iridium:ionomer = 3:1. In addition, the mixing ratio per unit area of the hydrogen generation catalyst and the ionomer in the cathode electrode membrane is platinum:ionomer = 1:1.
[0077] [CCM's evaluation]
[0078] Pt-plated Ti fibers were assembled on both sides of the CCM to form an electrolytic cell for evaluation. Water electrolysis was performed using the electrolytic cell. The conditions for water electrolysis were a current density of 0 to 3.5 cm / s. 2 , and the cell voltage was measured at an electrolysis temperature of 50° C. For comparison, a CCM was produced by using the same crystalline iridium oxide powder as described above and the same configuration and process as in the present embodiment, and an electrolysis cell was prepared and the cell voltage was measured.
[0079] Figure 3 The results of the electrolysis test (IV (cell voltage)) are shown. Figure 3 It is found that the oxygen overvoltage of the amorphous iridium oxide powder is lower than that of the crystalline iridium oxide powder.
[0080] In more detail, the catalyst overvoltage of the water electrolysis catalyst (the sum of the oxygen overvoltage and the hydrogen overvoltage) is calculated by subtracting the theoretical electrolysis voltage of the electrolysis cell and the overvoltage of the resistance component from the cell voltage. 2 The calculated value of the catalyst overvoltage at the time of 1.86V was 0.39V for the amorphous iridium oxide powder (battery voltage 1.86V), and 0.45V for the crystalline iridium oxide powder (battery voltage 1.93V). That is, it was confirmed that the voltage of the amorphous iridium oxide powder was reduced by about 13% relative to the crystalline iridium oxide powder. Therefore, the suitable water decomposition characteristics of the amorphous iridium oxide powder were confirmed. At this point, it can be considered that the crystalline iridium oxide powder is also useful as a water electrolysis catalyst, but it can be considered that a more active catalyst can be obtained by applying the amorphous iridium oxide powder. It should be noted that in the calculation of the above-mentioned catalyst overvoltage, the theoretical electrolysis voltage of the electrolysis cell was calculated by calculating the reaction Gibbs energy at the operating temperature (50°C). In addition, with regard to the resistance component, the resistance value was measured in the electrolysis test using a low resistance meter (manufactured by Tsuruga Electric Co., Ltd., MODEL 356E: measurement frequency 10kHz) during electrolysis.
[0081] Next, the CV curves of the two electrolytic cells prepared in this embodiment were measured to evaluate the charge of each anode. The battery voltage range was set to +0.05V to +1.3V, and the CV curves were measured under the conditions of a scan rate of 50mV / sec, a battery temperature of 50°C, and an RHE reference. The results are shown in FIG. Figure 4 As shown. The charge is the area of positive current within the above potential range. As a result, the charge of the electrode generated by the amorphous iridium oxide powder is calculated as per unit coating area of iridium (Ir 1mg cm -2 )6.31C, the charge of the electrode generated by the crystalline iridium oxide powder is calculated as per unit coating area of iridium (Ir 1mg cm -2 )2.5C. The charge of amorphous iridium oxide powder is 2.5 times greater than that of crystalline iridium oxide powder, which can be said to be effective for electrolysis. It should be noted that, as mentioned above, the charge of the electrode generated by the crystalline iridium oxide powder is also 2.5 times greater per unit coating area of iridium (Ir 1mg cm -2 )2.0C or more, so it can be considered that crystalline iridium oxide powder also has adaptability as a water electrolysis catalyst. And, the water electrolysis catalyst containing amorphous iridium oxide of the present invention becomes an excellent catalyst relative to crystalline iridium oxide powder.
[0082] Second EmbodimentIn this embodiment, regarding the composition of the electrode membrane (CCM) of the anode, a plurality of CCMs are manufactured by adjusting the mixing ratio of the water electrolysis catalyst and the ionomer. The water electrolysis catalyst used here is the amorphous iridium oxide powder of the first embodiment. The mixing ratio of the electrode membrane is adjusted by adjusting the mixing ratio of the catalyst and the ionomer in the catalyst ink.
[0083] Here, as the mixing ratio per unit area of the water electrolysis catalyst and the ionomer in the anode electrode membrane, four types of CCMs were manufactured, with iridium:ionomer ratios of 3:2, 2:1, 3:1, and 5:1. It should be noted that in any case, the composition of the cathode electrode membrane is the same as that of the first embodiment (platinum:ionomer = 1:1).
[0084] Then, an electrolytic cell was constructed in the same manner as in the first embodiment and a water electrolysis test was performed. Figure 5 As shown. Figure 5 The comparison current density is 2.0A / cm 2 The voltage value at the time of iridium: ionomer is 2:1, 3:1, and 5:1 electrodes (CCM), the voltage value is roughly the same. On the other hand, it is confirmed that the electrode with iridium: ionomer of 3:2 has a relatively high oxygen overvoltage relative to the above three electrodes, preferably within these ranges. In the actual anode electrode, considering proton conductivity and catalyst cost, it is estimated that iridium: ionomer is more preferably about 2:1 to 3:1.
[0085] Third Embodiment In the present embodiment, a mixture of amorphous iridium oxide powder and crystalline (rutile type) iridium oxide powder is used as a water electrolysis catalyst, and the difference in characteristics depending on the mixing ratio is studied.
[0086] In the present embodiment, the amorphous iridium oxide powder and the crystalline iridium oxide powder identical material that are manufactured in the first embodiment are used, and they are mixed and used as a water electrolysis catalyst. During mixing, a ball mill is processed to fully mix. At this time, the ratio of the amorphous iridium oxide powder is set to 100 mass % (amorphous only), 80 mass %, 60 mass %, 40 mass %, 20 mass %, 0 mass % (crystalline only).
[0087] Then, TG-DTA analysis was performed on each of the produced water-splitting catalysts. Figure 6 The TG-DTA curves at measurement temperatures between 300°C and 500°C are shown.
[0088] from Figure 6It can be confirmed that in the DTA curve of the water electrolysis catalyst containing more than 20% by mass of amorphous iridium oxide powder, an exothermic peak is shown near 389°C. It can also be seen that as the content of amorphous iridium oxide increases, the intensity of these exothermic peaks increases. Here, the DTA value of the DTA curve of the catalyst with an amorphous iridium oxide content of 0% by mass at 389°C is used as the reference point (0μV / mg), and the DTA value of each catalyst at 389°C is measured and plotted. The resulting standard curve ("amorphous %" vs. "DTA") is as follows: Figure 7 As shown. Figure 7 It can be seen that a linear approximation can be applied to the relationship between the ratio of amorphous iridium oxide in the water electrolysis catalyst and DTA.
[0089] In addition, in the present embodiment, the Ir concentration of each water splitting catalyst was analyzed. The Ir concentration was analyzed by an inductively coupled plasma emission spectrometry (ICP) device (SPECTRO Arcos FHS12 manufactured by AMETEK and iCAP 6500 manufactured by Thermo Fisher Scientific). Then, the relationship between the amorphous iridium oxide content and the Ir concentration (mass concentration) in the catalyst was studied ("amorphous %" vs. "Ir concentration"). Figure 8 The results are shown. Compared with the results of TG-DTA analysis ( Figure 7 ) Similarly, it is believed that there is a good correlation between the ratio of amorphous iridium oxide and the Ir concentration. It is believed that by measuring the Ir concentration in the catalyst, a calibration curve of the content of amorphous iridium oxide can also be obtained.
[0090] Then, for each water electrolysis catalyst produced in this embodiment, CCM production and electrolysis cell production were carried out in the same manner as in the first embodiment, and IV characteristics were evaluated. These production conditions and measurement conditions were the same as in the first embodiment. Fig. 9 The results of measuring the cell voltage of the electrolytic cell using each water electrolysis catalyst are shown.
[0091] from Fig. 9 It is known that when the iridium oxide powder contains amorphous iridium oxide, the battery voltage is reduced compared to the crystalline iridium oxide powder alone. From the trend of the battery voltage reduction, if the content of amorphous iridium oxide is about 15% by mass or more in terms of mass ratio, it can be inferred that appropriate water decomposition characteristics are imparted. The catalyst with the lowest battery voltage can be considered to be a catalyst containing only amorphous iridium oxide (100% by mass), but it can be considered that even if the content is not increased to that extent, the improvement of water decomposition characteristics can be seen.
[0092] Industrial Applicability
[0093] The present invention is a water electrolysis catalyst suitable for an anode electrode membrane in a solid electrolyte water electrolysis device. The iridium oxide powder of the present invention has excellent proton conductivity while maintaining the activity of water electrolysis, and by appropriately mixing with an ionomer, the oxygen overvoltage is reduced, thereby becoming an electrode membrane with excellent voltage efficiency. In addition to a hydrogen generation device for solid electrolyte water electrolysis, the present invention is also useful in alkaline ion water purifiers and the like.
Claims
1. A water electrolysis catalyst consisting of iridium oxide powder, The iridium oxide powder contains amorphous iridium oxide powder. The average particle size of the iridium oxide powder is not less than 0.01 μm and not more than 30 μm.
2. The water electrolysis catalyst according to claim 1, wherein The ratio of the amorphous iridium oxide powder to the entire iridium oxide powder is 15 mass % or more in terms of mass ratio.
3. The water electrolysis catalyst according to claim 1 or claim 2, wherein: When thermogravimetric differential thermal analysis (TG-DTA) was performed, an exothermic peak was observed in the region of 300°C to 450°C.
4. The water electrolysis catalyst according to any one of claims 1 to 3, wherein The Na content is 100 ppm or less, and the Cl content is 100 ppm or less. 5 . An electrode membrane for water electrolysis, which is obtained by mixing the catalyst for water electrolysis according to any one of claims 1 to 4 and an ionomer.
6. The electrode membrane for water electrolysis according to claim 5, wherein: The mass of iridium (mg / cm 2 ) and the mass of the ionomer (mg / cm 2 ), the mixing ratio per unit area of the catalyst for water electrolysis and the ionomer is iridium:ionomer = 2:1 or more and 5:1 or less.
7. The electrode membrane for water electrolysis according to claim 5 or claim 6, wherein: The thickness of the water electrolysis electrode membrane is 2 μm or more and 10 μm or less.
8. A membrane with a catalyst layer, comprising the electrode membrane for water electrolysis according to any one of claims 5 to 7 as an anode, and an electrode membrane containing a catalyst for hydrogen generation as a cathode, The unit coating area of the water electrolysis electrode membrane of the anode per iridium (Ir 1mg cm -2 ) has a capacitance of 0.50C or more.