Method for representing semiconductor doping by using light neutralization time constant of corona surface charge

Through the charge light neutralization technology, the doping concentration is determined using the optical neutralization time constant τph, which solves the problem of insufficient measurement speed and flux in the existing CnCV technology, and realizes efficient doping measurement, which is suitable for the multi-bandgap semiconductors of wideband gap Characterization of layer film doping depth distribution.

CN118891532AActive Publication Date: 2024-11-01SEMILAB SDI LLC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202480001587.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-03-08
Publication Date
2024-11-01
Estimated Expiration
2044-03-08

AI Technical Summary

Technical Problem

The existing non-contact capacitance voltage (CnCV) technology has limited measurement speed and flux when measuring wideband gap semiconductor doping concentrations, limiting the production efficiency and quality control of large-scale epitaxial sheets.

Method used

Using charge photoneutralization technology, the corona charge is rapidly neutralized by short wavelength irradiation, and the doping concentration is determined using the light neutralization time constant τph, which improves the measurement speed and flux, and realizes the step of replacing the accumulated charge by a single large corona charging instead of the accumulated charge. , enhances the sensitivity of doping measurement.

Benefits of technology

The speed and flux of doping measurement are improved, the test flux is increased, and the measurement efficiency can be increased by up to ten times based on conventional CnCV technology. It is suitable for the characterization of multilayer film doping depth distribution of wide-bandgap semiconductors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891532A_ABST
    Figure CN118891532A_ABST
Patent Text Reader

Abstract

A method of characterizing semiconductor doping in a wide band gap semiconductor sample comprises: measuring an initial value V0 of a surface voltage at a region of a surface of the semiconductor sample in darkness; charging the region to deep depletion in darkness by depositing a defined corona charge at the region; measuring a surface voltage value at the area in darkness after charging; irradiating the charged region with light of a specific photon flux feff having a photon energy higher than the semiconductor band gap sufficient to generate free minority carriers in the semiconductor sample to cause photoneutralization of corona charges; using a non-contact time-resolved measurement of the surface voltage V (t) to monitor the relationship of light neutralization induced corona charge decay to the illumination time t at the area; analyzing the monitored time-resolved surface voltage decay data V (t) to determine a light neutralization time constant [tau] ph; and using the light neutralization time constant [tau] ph under the specific photon flux feff as a semiconductor doping index, and characterizing the semiconductor doping concentration at the region based on the value of the light neutralization time constant [tau] ph.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates generally to characterization of semiconductor doping in wide bandgap semiconductors, and more particularly to methods for contactless measurement of doping in epitaxial layers and systems for performing such measurements. Background Art

[0002] Doping a semiconductor with donor or acceptor impurities changes the electrical properties of the semiconductor and is a key technological element in the manufacture of semiconductor devices. Doping is usually done by introducing impurity atoms that replace host atoms in the semiconductor crystal lattice. Doping concentration is the concentration of dopant atoms per volume of semiconductor, and its measurement is often used for quality control in the production of semiconductor devices.

[0003] For example, devices based on wide bandgap semiconductors (including SiC, GaN, AlGaN and AlGaN / GaN) are widely used in power electronics and high frequency applications. Such devices typically include doped epitaxial layers, where strict doping control of the epitaxial wafer is necessary. In order to meet the needs of the rapidly developing wide bandgap semiconductor technology and large-scale epitaxial wafer (epi-wafer) manufacturing, corresponding large-scale doping testing is required. For this purpose, non-contact measurement technology may be preferred. Non-contact metrology can eliminate the cost and time involved in manufacturing test devices, and can avoid the post-measurement wafer cleaning required in the case of many conventional doping measurement methods (e.g., Mercury Probe methods).

[0004] An example of a non-preparation non-destructive doping measurement method for wide bandgap semiconductors described in US 10,969,370 B2 can be performed using a commercially available corona non-contact capacitance voltage (CnCV) tool manufactured by Semilab SDI. CnCV uses corona charging to electrically bias the semiconductor surface to deep depletion, similar to the voltage biasing of a metal Schottky barrier, however, this is achieved without metal contacting the semiconductor surface. In the CnCV method, the charge bias dose ΔQ is monitored with a Kelvin probe. C The surface voltage response ΔV. Differential capacitance C = ΔQ in sequential charge measurement C / ΔV gives the non-contact CV characteristics. Doping concentration N D By 1 / C 2 The slope of πvs V is determined, which is a standard procedure in CV methods. For a typical 12-site pattern, the throughput of CnCV measurements using commercially available tools is currently limited to about 5 wafers per hour. Summary of the invention

[0005] Conventional CnCV technology can be modified to employ a new doping-sensitive phenomenon that can be exploited to increase test throughput. Conventional CnCV uses corona charge bias to depletion, which is achieved through multiple incremental corona charge deposition steps. In response to the deposited charge, the surface voltage V changes and is measured with a non-contact vibrating Kelvin probe. Similar to mercury probes and Schottky junction devices, CnCV employs a 1 / C 2 -V characteristics to determine the doping concentration. CnCV is a quasi-static technique with many relatively slow charge bias steps involved in acquiring the CV characteristics. This generally limits the measurement speed and throughput in multiple wafer monitoring, where each wafer typically has 9 or 12 test sites and wafer mapping with 49 sites.

[0006] The deposited corona charge can be rapidly neutralized and removed from the bare surface of a wide bandgap semiconductor by short wavelength illumination. The corresponding time constant of the corona photoneutralization can be very short, enabling rapid sweeping of the depletion barrier. In measurements on epitaxial SiC with different doping, a direct relationship between the corona charge photoneutralization time constant and the doping concentration was determined. This relationship is confirmed for other wide bandgap semiconductors and is valid over a wide range of doping concentrations. The enhanced flux doping measurement method in the present disclosure is based on this newly identified relationship.

[0007] Therefore, in the present invention, a charge biasing method with a novel doping measurement principle is described, which can increase the measurement speed and throughput, for example, by up to ten times compared to the conventional CnCV technique described above.

[0008] The method described here can replace the sequence of accumulating charge steps with a single large corona charging to deep depletion. Afterwards, the deposited charges on the semiconductor surface are photoneutralized using near-UV irradiation that generates excess carriers. The photoneutralization time constant is determined from time-resolved surface voltage measurements and this time constant is a doping measurement parameter.

[0009] During the photoneutralization process, the minority carriers photogenerated within the charge-induced surface depletion layer are mobile. They are guided to the surface by the depletion electric field and captured by the corona ions of opposite polarity, thus neutralizing the corona charge and reducing the depletion width. The technique involves measuring and analyzing the corresponding changes in the surface voltage with respect to the irradiation time.

[0010] In wide bandgap semiconductors, photoneutralization of corona ions is irreversible. The corona charge is not restored after photoneutralization, and the surface voltage changes induced by photoneutralization are not reversed in the dark. This enables the process to be monitored by measuring the surface voltage when irradiating the charged area or after continuous irradiation pulses. The present disclosure covers both measurement configurations. Specifically, the measurement when irradiating the charged area is adopted in a system configuration in which the irradiation is below the surface voltage probe. The measurement after the irradiation pulse is used in a system configuration in which the irradiation is at a position separated from the surface voltage probe.

[0011] This measurement technique exploits the irreversible nature of the surface voltage change induced by illumination to separate charge photoneutralization from other surface photovoltage effects. The corresponding test involves monitoring the surface voltage in the dark after cessation of illumination. For good measurement conditions, dark recovery should be negligible, for example in the range of 0.1%.

[0012] In certain embodiments, the measurement technique uses the depletion layer Schottky barrier electrostatic charge-voltage relationship to extract the charge photoneutralization rate and determines the photoneutralization time constant τ from the logarithmic characteristic of the surface voltage versus the irradiation time. ph Based on the time constant τ ph and τ ph vs N D The calibration correlation is used to determine the doping concentration N D . Time constant vs surface voltage characteristic τ ph -V provides a means for evaluating the doping depth profile. Uniform doping is achieved by constant τ ph In the logarithmic light neutralization and surface voltage characteristics, multilayer films with different doping will show different τ in a certain period of time. ph The corresponding surface voltage reflects the different depths below the surface.

[0013] Typically, a measurement setup consists of three system components with the following capabilities:

[0014] (a)-Corona charging is used to bias the semiconductor surface charge to deep depletion.

[0015] (b)-Non-contact surface voltage measurement.

[0016] (c) - Short wavelength irradiation with photon energy above the semiconductor energy gap.

[0017] The semiconductor sample wafer may be placed on a conductive chuck with rapid movement capability for positioning the test sample area (ie, test sites on the wafer) under system components (a), (b), and (c) according to a measurement cycle.

[0018] A housing for the measurement system may be provided to prevent stray light (eg, short wavelength stray light) from reaching the wafer, which could otherwise cause uncontrolled corona charge neutralization on the wafer surface.

[0019] Time constant τ ph can be used directly as a relative doping concentration index. For accurate quantitative measurement of doping concentration, the method may include a calibration function for the time constant, which is determined by measuring a reference sample wafer with a known doping concentration. Alternatively or additionally, the light neutralization time constant τ may be used. ph Wafer-specific calibration is performed by performing corona CV doping measurements on the same sample area (same wafer site) as the measurements.

[0020] In conventional corona charging methods for semiconductor and dielectric characterization, the response to changes in deposited corona charge density is usually monitored by measuring the corresponding changes in surface voltage. In the present technology, the measurement of surface voltage is also adopted, however, the change in charge density of corona deposition is achieved by photoneutralization of charge rather than by charge deposition. The measurement of charge photoneutralization and surface voltage can be performed simultaneously or sequentially, depending on the configuration of the light source and the surface voltage probe. The illumination under the probe enables measurement during the actual corona photoneutralization. This allows the sample site to be illuminated and measured without transferring the wafer between the irradiation and measurement probes, which can be beneficial to the speed and flux of the measurement. The configuration with a separate light source can promote higher illumination uniformity than the illumination under the surface voltage probe. This can be beneficial to accuracy and tool-to-tool matching.

[0021] The disclosed technology may use multiple light sources with different configurations and wavelengths, which may be selected and optimized based on the requirements of the specific semiconductor wafer fabrication in which the technology is to be used.

[0022] In general, in one aspect, the invention features a method of characterizing semiconductor doping in a wide bandgap semiconductor sample, the method comprising: measuring an initial value V0 of a surface voltage at a region of a surface of the semiconductor sample in darkness; charging the region to deep depletion in darkness by depositing a prescribed corona charge at the region; measuring a value of the surface voltage at the region in darkness after charging; and measuring the surface voltage at the region with a specific photon flux f. eff The light irradiates the charged area, the specific photon flux φ eff having photon energy above the semiconductor bandgap sufficient to generate free minority carriers in the semiconductor sample to cause photoneutralization of the corona charge; monitoring the photoneutralization-induced corona charge decay at an area vs. irradiation time t using non-contact time-resolved measurement of surface voltage V(t); analyzing the monitored time-resolved surface voltage decay data V(t) to determine the photoneutralization time constant τph ; and using a specific photon flux f eff The light neutralization time constant τ ph As the semiconductor doping index, the semiconductor doping concentration at the region is characterized based on its value.

[0023] Implementations of the method may include one or more of the following features.

[0024] The method may include a specific corona charge photoneutralization time constant τ based on the surface voltage ph vs V is used to characterize the doping concentration depth distribution of semiconductor samples.

[0025] The method may include an average τ based on the surface voltage range ph The doping values ​​of individual epitaxial layers are characterized.

[0026] In some examples, τ is determined according to the following equation ph :

[0027]

[0028] Where t is the irradiation time, V const is the surface voltage probe offset. The method may include using a probe having a known doping concentration value N D One or more reference samples of τ ph The calibration function τ is determined by the calibration measurement ph vs ND and the inverse calibration function N D vs τ ph (expressed as f cal ). In some examples, the method includes setting the effective photon flux φ eff The time constant τ measured under ph Normalized to the calibration photon flux φ eff ,as follows: and using the normalized time constant according to the following equation Determine the absolute doping concentration:

[0029] The method may include calibrating τ for the doping concentration ph , where the calibration is specific to the semiconductor wafer sample and is based on τ at multiple sites (e.g., 9 sites, 12 sites, or 49 sites) of the wafer sample. ph During the characterization of the measured wafer sample, the calibration is performed at one site, where all τ ph The measurements are performed under the same illumination conditions. Calibration can include measuring the corona charge photoneutralization time constant τ using the corona non-contact CV (CnCV) method ph and independently measure the doping concentration N D, where the two measurements are performed one after the other at the same wafer site and within a similar corona charge-induced depletion voltage range. The method may comprise using τ ph and N D To determine whether N D =τ ph ·f cal The wafer-specific inverse calibration function value f cal .

[0030] In some examples, the method includes determining τ at each wafer site based on ph and using f determined at a single locus cal The doping concentration at all different wafer sites is determined using the wafer-specific value of .

[0031] The capacitance probe may be a non-contact vibrating Kelvin probe.

[0032] The area may be irradiated while the surface voltage is being monitored, or the area may be irradiated separately from monitoring the surface voltage.

[0033] The semiconductor sample may include a semiconductor selected from the group consisting of SiC, GaN, and AlGaN.

[0034] The method may include based on V measured after corona charging but before irradiation Dark and dark decay rate ΔV Dark / Δt Dark To identify defective areas in semiconductor samples.

[0035] The method may include measuring a dark decay amplitude ΔV based on the dark decay amplitude ΔV measured after illumination. Dark To identify the contribution of surface photovoltaic effects other than corona light neutralization to the monitored surface voltage.

[0036] Other features and advantages will be apparent from the drawings, description, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1A is a schematic diagram of an exemplary system for measuring doping of semiconductor wafers using corona charge deposition followed by irradiation-induced charge photoneutralization and determination of the photoneutralization time constant from non-contact time-resolved surface photovoltage. In this example, the configuration includes an irradiator positioned below the surface voltage probe.

[0038] Figure 1B yes Figure 1A Schematic diagram of an alternative configuration of the example system shown in , where illumination is at a location separate from the surface voltage probe.

[0039] Figure 2is a diagrammatic representation of the steps in an example measurement procedure for determining the photoneutralization time constant from the time-resolved surface voltage decay.

[0040] Figure 3A is a graph showing example results of surface voltage measured during corona charge photoneutralization versus irradiation time.

[0041] Figure 3B is used to determine Figure 3A Graph of an example of the light neutralization time constant corresponding to the transient state in FIG.

[0042] Figure 3C is the surface voltage specific τ ph A graph showing a uniform doping depth profile.

[0043] Figure 4 is a graph showing an example of the corresponding logarithmic surface voltage decay for an n-type SiC epitaxial wafer having 3 layers of different doping.

[0044] Figure 5 is a graph of example doping calibration results showing the photoneutralization time constant τ ph Compared with the doping concentration N measured on n-type 4H-SiC D Using -4E12 q / cm 2 The negative corona charge density was measured using an incident photon flux of 1.2 × 10 13 Photons / cm 2 s irradiated with 325nm wavelength. Doping concentration N D Corresponds to the CV mercury probe results.

[0045] Figure 6 is an energy band diagram showing the photoneutralization of corona charges on an n-type wide bandgap semiconductor. The threshold energy hv is the energy gap E g .

[0046] Figure 7 is a graph showing example results of the dependence of the light neutralization time constant on the incident photon flux. The results are for a doping concentration of N D =6.11e15 cm -3 and N D =1.85E16 cm -3 N-type SiC. D Values ​​are based on CV mercury probe results. DETAILED DESCRIPTION

[0047] refer to Figure 1A, schematically shows an example apparatus 100 for corona charge-voltage photoneutralization characterization of a semiconductor wafer sample 101. The wafer sample comprises a substrate 104 and an epitaxial layer 103 supported by the substrate 104. The apparatus 100 comprises a corona charge source module 120 for precise charge deposition on a test site 126, a surface voltage measurement module 130 for surface voltage measurement, and a light source module 140 for irradiating the wafer surface.

[0048] Wafer 101 is supported by wafer chuck 110, which is positioned on a movable stage 112. Stage 112 can move wafer chuck by translation and rotation. Coulomb counter 114 is connected to wafer chuck 110.

[0049] The corona charge source module includes a corona charge electrode arranged to deposit a corona charge 124 at sites 126 on the surface of the wafer 101. The surface voltage measurement module 130 includes a Kelvin probe having an electrode 132 arranged to vibrate a small distance (e.g., one millimeter or less) above the surface of the wafer 101. Although the examples described herein use a Kelvin probe, other capacitive probes may be used.

[0050] The light source module 140 includes a light source 142 arranged to illuminate the surface of the wafer 101 located directly below the Kelvin probe electrode. During operation, the light source 142 delivers illumination having a wavelength suitable for photo-neutralization of corona charges at the wafer surface below the Kelvin probe electrode 132. The light source 142 may include, for example, a light emitting diode (LED) or a near-UV laser. For an LED, the light beam may be additionally monochromatized by passing through a narrow bandpass filter.

[0051] refer to Figure 1B, an alternative device 100' is shown, in which the light source module 140' includes a light source 144, which is positioned to illuminate a location on the surface of the wafer 101 that is different from the location below the electrode 132. Similar to the light source 142, the light source 144 can include an LED or a laser that can emit light having a wavelength suitable for corona charge photoneutralization. In general, the illumination wavelength provided by the light sources 142 and 144 can be selected according to the wafer being measured. In general, the photon energy should be higher than the semiconductor energy gap. For the measurement of 4H-SiC with an energy gap of 3.26eV, appropriate light wavelengths include =355nm or =325nm corresponding to photon energies hv=3.49eV and hv=3.82eV, respectively. Both photon energies exceed the SiC energy gap, which is required to generate free carriers (electron-holes) involved in the corona charge photoneutralization process. For measurements on other semiconductors, the light wavelength can be selected based on the value of the energy gap and the absorption coefficient. Shorter wavelength = 315 nm illumination may be suitable for measuring doping on GaN and AlGaN materials, which have energy gaps greater than that of SiC. Other wavelengths of light, about 380 nm or less, may be used, depending on the application. Light sources 142 and 144 are arranged to provide uniform illumination within the surface area of ​​the corona charging spot, such as a circular spot of about 10 mm or less in diameter (e.g., about 6 mm in diameter).

[0052] Computer controller 150 is used to control the operation of the apparatus and to perform data analysis to determine information about the doping of sample 101 using the measurement and analysis steps described below.

[0053] Figure 1A and Figure 1B The example devices 100 and 100' shown in Figures 1 and 2 respectively show two illumination configurations: namely, a light source 142 (LED 1) for illumination below the vibrating electrode of the Kelvin probe electrode 132, and a light source 144 (LED 2) for illumination separate from the Kelvin probe 132. Standard high-precision Kelvin probes may use opaque gold electrodes. In the case where the Kelvin probe electrode 132 is opaque, low-angle illumination from the side may be used, such as Figure 1A In some embodiments, a transparent Kelvin probe may be used that is illuminated through an electrode. Generally, high uniformity of illumination may be more easily achieved when illumination is performed using light source 144 alone, such as Figure 1B shown.

[0054] In the Kelvin probe method, a capacitive electrode vibrating a fraction of a millimeter above the measurement surface generates an alternating current that is zeroed by compensating for the DC bias, thereby providing a measurement of the voltage difference between the electrode and the semiconductor. For this application, an accurate and fast-responding Kelvin probe is preferred, such as a probe with a time constant of about 5ms and an accuracy of 0.2mV. For deeply depleted corona charges biased to n-type (negative bias) and p-type (positive bias) semiconductors, the surface voltage measurement range is typically -100V to +100V. An electrode diameter of 1mm or 2mm is suitable for measuring the surface voltage in a uniform central area of ​​the corona charging and irradiation area.

[0055] Corona charging is achieved using corona discharge in the air generated by a high DC voltage applied from the power supply 122 to the discharge electrode 124. Negative polarity discharge in the air generates ions, while positive discharge produces (h2O) n H + ions. The corona discharge electrodes (needles for point charging or wires for whole wafer charging) can be confined in an enclosure, and ion deposition is not field driven; instead, ions diffuse through the aperture openings to the wafer surface. Considering a 10 -5 The very short mean free path of cm, ions lose kinetic energy and become thermalized before reaching the semiconductor surface. Such a configuration enables non-invasive corona charge biasing. Accurate corona charging is usually carried out in a clean room environment with controlled humidity and temperature. The control of the deposited corona charge density is achieved by setting the high voltage, discharge current and deposition time cycle of the corona power supply 122. The deposition time cycle can be about 1 second or shorter. The deposited charge density dose can be monitored in situ with a coulometer 114.

[0056] The corona is charged to a depth of depletion from about 1x10 12 q / cm 2 Extends to about 1x10 13 q / cm 2 , and charging can be achieved in a single charging step. The charge deposited on the surface at the test site 126 is mirrored as an opposite charge in the semiconductor surface space charge region and acts as an electrical bias. The charging dose is much larger than the surface charge initially present, typically about 1x10 11 q / cm 2 Therefore, according to the doping concentration N D , you can choose the charging dose Q C To obtain the desired depletion width W D =-Q C / qN D .

[0057] Wide bandgap semiconductor devices are primarily fabricated on n-type epitaxial layers, and 4H-SiC is a commonly used material. Therefore, exemplary results for methods for n-type 4H-SiC and negative polarity corona charging are presented in the present disclosure. To measure such wafers, the method may also include stabilizing new epitaxial 4H-SiC wafers using a UV pretreatment chamber, which may be part of the apparatus 100. Immediately after the epitaxial growth process, 4H-SiC may exhibit rapid dissipation of deposited corona charge. This is caused by surface diffusion of corona ions. If present, this effect may interfere with the measurement of photo-induced charge photoneutralization. Pretreatment to eliminate surface diffusion effects may be performed simultaneously with doping measurements of multiple sets of wafers. This capability may be added to an automated version of the apparatus 100.

[0058] A stable bare surface of depleted SiC typically exhibits good corona charge stability in the dark. The large energy gap prevents thermal generation of free minority carriers that could neutralize the corona charge. In this method, the charge stability in the dark after charging is verified by a corresponding stability of the surface voltage. For this purpose, the method may include a prescribed period of surface voltage measurement in the dark after charging but before illumination. Such a measurement is an example of a dark decay rate measurement and is based on the dark surface voltage V as a function of time. dark The decay rate is generated by the change of the dark surface voltage decay rate. A large dark surface voltage decay rate and a nominal expected surface voltage amplitude below the deposited charge density can indicate a defect that causes charge dissipation and therefore interferes with the corona charge photoneutralization measurement. In this case, the measurement can be repeated on an adjacent wafer site that is defect-free and has a negligible dark decay rate. In the epitaxial 4H-SiC used as an example in the present disclosure, the interfering defects are device-killing triangular defects, downfall defects, or carrot defects. These defects can have sub-millimeter sizes, and shifting the measurement position by a distance greater than the Kelvin probe diameter (e.g., 3mm to 5mm in the case of a 2mm diameter Kelvin probe) can be sufficient to eliminate the interference.

[0059] In some embodiments, additional verification steps may also be performed. For example, such steps may include measurements of the surface voltage performed in the dark after turning off the photoneutralization of the light-induced charge. This verification relates to the irreversible nature of the photoneutralization and is intended to identify other surface photovoltaic effects that are reversible in the surface depletion layer.

[0060] Typically, measurements are made under conditions where corona charge photoneutralization dominates. This can be tested in measurements of surface voltage recovery in the dark, immediately after irradiation. For optimized measurement conditions, the amplitude of this surface voltage recovery, indicative of other effects, should be, i.e., insignificant compared to the corona charge photoneutralization amplitude, e.g., in the range of about 100 mV or less for corona charge photoneutralization amplitudes of about 20 V or more. In SiC, using a surface voltage recovery at about 10 V or more, the surface voltage recovery should be indicative of other effects, i.e., insignificant compared to the corona charge photoneutralization amplitude, e.g., in the range of about 100 mV or less for corona charge photoneutralization amplitudes of about 20 V or more. 13 to about 10 14 Photons / cm 2 Low effective photon fluxes in the s range enable this insignificant contribution.

[0061] Characterization of semiconductor doping includes determination of the time constant τ for photoneutralization of corona charges under surface depletion conditions ph Once τ is determined ph , which is used as the doping index. τ ph The value is converted into doping concentration N D =τ ph ·f cal , where f cal is the so-called inverse calibration function. The time constant τ is discussed further below. ph and the calibration function f cal of determination.

[0062] Figure 2 The table in shows the steps involved in a measurement procedure that can be used to obtain time-resolved surface voltage data to determine the photoneutralization time constant. Figure 2 The surface voltage measured at each step is shown in the graph included in FIG. 1 . The surface voltage measurement is performed using the apparatus 100 or 100 ′ and Figure 1A The illumination configuration shown measures the properties of a typical n-type epitaxial wafer of 4H-SiC. The wafer is held on a conductive chuck 110 by vacuum suction. The chuck 110 provides a backside electrode that is capacitively coupled to the wafer during corona charging and measurement. The non-contact nature of the method means that there is no physical contact with the front surface of the wafer (in this case, the surface of the epitaxial layer 103). All lights in the system are initially turned off and the wafer is in the dark. The wafer chuck is removable and is used for Figure 2 Step 1 in which the wafer test site is positioned below the Kelvin probe electrode 132 for measuring an initial surface voltage V0 in the dark, for example V0 = 0.8 V. After the initial surface voltage measurement, the test site 126 is transferred to a position below the corona charging source (e.g. Figure 1A and Figure 1B As shown), and in step 2, it will have a prescribed charge density Q C (e.g. -1.5x10 12 q / cm 2) is deposited on the surface of epitaxial layer 103 at test site 126. As a result of the charge deposition, the surface is biased to be deeply depleted. For step 3, the charging site is shifted to a position below Kelvin probe electrode 132. The deeply depleted surface voltage after charging is then measured, giving a post-charge value, such as V D = -59 V. In step 4, the test site is illuminated with short wavelength light having a photon energy higher than the 3.26 eV energy gap of 4H-SiC, suitable for causing photoneutralization of corona charges. For example, irradiation with a 325 nm wavelength (hv = 3.82 eV) of a near-UV LED may be used. Figure 1A In the example shown, illumination of the Kelvin probe below the electrode 132 with a light source 142 can be used so that the depletion layer surface voltage V(t) can be continuously monitored while illuminating the charged region. Figure 1B In the case of the exemplary device 100' shown, the illumination is at a location separate from the surface voltage probe. Therefore, monitoring cannot be performed while the charging area is illuminated. Instead, it is done using a sequence of steps including a short illumination period (typically about 10ms to 20ms duration) and surface voltage measurement. In this sequence, the charging area moves from a location under the surface voltage measurement probe 132 to a location under the illumination source 144, then back to the surface voltage probe... and so on.

[0063] The final step 5 of the measurement cycle consists in recording the surface voltage after the short-wavelength light is turned off. This value is Figure 2 is called dark voltage V after The very small depletion voltage recovery serves to confirm the negligible contribution of the surface photovoltaic effect other than the corona charge photoneutralization.

[0064] An example of measured V(t) is Figure 3A The initial part of the voltage transient in the dark shows no decay before illumination. This dark part is an indication of negligible charge dissipation due to surface diffusion or any defect-related charge neutralization. During illumination, rapid photoneutralization of the corona charge is evident as a corresponding surface voltage decay. This recorded V(t) time dependence can be reliably analyzed using the Schottky barrier voltage-charge equation, providing a method for determining the corona charge photoneutralization time constant τ ph The depletion surface barrier is related to the surface charge density (V D ~Q C 2 ) can be used to derive the surface voltage decay corresponding to the decay of the corona charge. In practice, τ ph It can be determined from the inverse slope of the time decay of the logarithmic surface voltage during photoneutralization as Where V0 is the initial precharge value, including the offset associated with the Kelvin probe calibration. Figure 3A V(t) data in Figure 3B Shown in.

[0065] This fitting procedure gives the average τ over the specified surface voltage range. ph values, in this case in the range of -5V and -59V. Figure 3B The good linear fit in the range indicates a constant τ ph This is consistent with uniform doping vs depth in this epilayer.

[0066] For doping depth profile, a voltage-specific time constant corresponding to a given depletion surface voltage V can be used based on the photoneutralization V vs irradiation time characteristic V(t). It is calculated from the relative surface voltage decay rate as Figure 3C Shown for Figure 3A The voltage-specific τ as a function of the depletion surface voltage is shown in the data ph , which indicates a constant τ within this voltage range consistent with a uniform doping depth profile in the epilayer ph value.

[0067] Figure 4 The example in shows the logarithmic surface voltage time decay of an epitaxial wafer with 3 layers of different doping. Each layer is characterized by a corresponding τ proportional to the doping value ph1 , τ ph2 and τ ph3 Layers 1, 2 and 3 are counted from the top of the epitaxial layer structure.

[0068] Figure 5 For n-type 4H-SiC and with wavelength λ = 325 nm and effective incident photon flux φ eff =1.2x10 13 Photons / cm 2 s of light exposure, light neutralization time constant τ ph With doping concentration N D This correlation can be used to determine the calibration function N D vs τ ph , which corresponds to a specific doping range N D and irradiation conditions λ and

[0069] Light neutralization time constant τ ph As the dopant concentration N D The increase in the corona charge Q is usually C The smaller surface depletion width W D =Q C / q N D This results in a smaller photogeneration of the depleted internal holes. Figure 6 As shown, the free holes h generated in the depletion + are active in photoneutralization, and they are guided to the surface by the depletion electric field. At the surface, the negative corona ions capture holes, Q - +h + →Q↑ and the neutralized corona species detach from the surface.

[0070] Under increased doping, the smaller hole generation caused by the reduced depletion width can be reduced by increasing the incident photon flux Q eff To overcome. Figure 7 As shown, τ ph is inversely proportional to the incident photon flux. Therefore, by increasing the incident photon flux, D In this method, the measurement speed is the main advantage. In this regard, the time constant τ ph and the incident photon flux ( ph ~1 / φ eff ) can be used to optimize the measurement. For example, for 10 16 cm -3 N in the range D , by increasing the photon flux to 10 14 Photons / cm 2 s range, a time constant τ of about 0.1s can be achieved ph Combining increased photon flux with shorter wavelength light, such as λ = 315 nm or λ = 300 nm, allows fast measurements of highly doped samples, such as 10 18 cm -3 .

[0071] As mentioned before, calibration can be used to convert the measured time constant into doping concentration. For this purpose, the time constant can be calculated for a specific doping range and (λ,φ eff ) values ​​determine a family of specific calibration functions. For accurate measurement, the individual specific calibration functions can be limited to N D and A subset of the entire range of values ​​of , for example, a precise calibration function can cover N D and φ eff The calibration function can be determined using a precise setting of the measurement and illumination conditions of a reference wafer with a known doping concentration. For example, a calibration function can be determined using a N pre-measured using a mercury probe CV method. D The exact same irradiation conditions can then be used when measuring the doping in the fabricated epilayers in a production environment.

[0072] From the calibration τ ph vs N D The data quantitatively determine the doping concentration using the expression f cal The inverse function N D vs τ ph Perform the measurement at the same wavelength as that used for calibration, e.g. Figure 5 and Figure 7 The photon flux used during the measurement is φ eff Usually different from the photon flux φ used for calibration cal , because it is adjusted considering the measurement speed requirement. ph The dependence of the incident photon flux on the measured τ ph Normalize. Then use the normalized value For N D vs τ ph The inverse function f cal In order to calculate the doping concentration as exist Figure 5 In the example of cal =12e13 photons / cm 2 s under φ cal However, applications such as Figure 7 This calibration gives the correct N for different photon fluxes shown. D Value, within 0.5%.

[0073] An alternative approach uses a wafer-specific calibration performed during actual measurement of a given wafer. Figure 1A and Figure 1B The devices 100 and 100' shown in FIG. 1 are suitable for this purpose. Wafer-specific calibration involves: (1) the corona charge photoneutralization time constant τ ph The two independent measurements are performed one after the other on the same wafer site. The results are used to determine the inverse calibration function f cal , satisfying N D =τ ph .f cal At all other test locations on the wafer, only τ phk (k is the position number). Using the measured τ phk and the wafer-specific function f cal The same value of determines the doping N at different k positions on the wafer Dk =τ phk .f cal .

[0074] In general, measurements with wafer-specific calibration are done with identical illumination conditions for all measured sites. The conditions can be optimized for different doping ranges. However, no precise knowledge of the incident photon flux is required, since the method uses the measured τ ph Instead of normalizing the photon flux The measurements described above can be performed at any number of sites on the wafer. Typical production line testing involves 12 wafer site measurements or 49 site wafer mapping. Wafer-specific calibration adds typically 40 seconds to the unit site CnCV doping measurement time. τ at a single site ph The measurement time is short, for example about 4 seconds. For a 12-site test with wafer-specific calibration, the measurement time per wafer can be about 90 seconds. This measurement speed can give a throughput of about 30 wafers / hour, including wafer handling overhead time. For a 49-site wafer mapping with an additional calibration time of 40 seconds, this results in a total measurement time of about 240 seconds and a throughput of about 13 wafers / hour with wafer handling overhead.

[0075] Measurements using wafer-specific calibration can reduce uncertainties by reproducing the illumination conditions and still provide very fast, high-throughput epitaxial SiC doping monitoring.

[0076] The above-described photoneutralization method uses a specific photoneutralization time constant definition based on a logarithmic analysis of charge decay. However, it should be noted that, in general, the photoneutralization kinetic sensitivity to dopants determined in the present invention can be defined using a different time constant for doping measurements, such as the half-life of charge decay, a stretched or compressed exponential time constant of charge decay, etc.

[0077] Although a single application of the photoneutralization method is described above, the technique and benefits are not limited to bare SiC doping monitoring. More generally, the corona photoneutralization technique can be applied to characterize other wide bandgap materials and structures, such as GaN and HEMTs. For example, the technique can be applied to determine HEMT characteristics such as pinch-off voltage (V p ) and 2DEG sheet charge.

[0078] Accordingly, other embodiments are within the following claims.

Claims

1. A method for characterizing semiconductor doping in a wide bandgap semiconductor sample, the method comprising: measuring an initial value V0 of a surface voltage at a region of the surface of the semiconductor sample in darkness; charging the area to deep depletion in darkness by depositing a prescribed corona charge at the area; measuring a surface voltage value at the area in darkness after charging; With a specific photon flux φ eff The light irradiates the charged area, the specific photon flux φ eff having a photon energy above the semiconductor bandgap sufficient to generate free minority carriers in the semiconductor sample, thereby causing photoneutralization of the corona charge; monitoring the photoneutralization-induced corona charge decay at the region as a function of the irradiation time t using non-contact time-resolved measurement of the surface voltage V(t); Analyze the monitored time-resolved surface voltage decay data V(t) to determine the photoneutralization time constant τ ph ; as well as Using a specific photon flux φ eff The light neutralization time constant τ ph As the semiconductor doping index, the semiconductor doping concentration at the region is characterized based on its value.

2. The method according to claim 1 further comprises a surface voltage-specific corona charge photoneutralization time constant τ ph The relationship between V and the doping concentration depth distribution of the semiconductor sample is characterized.

3. The method according to claim 1 further comprises: ph The doping values ​​of individual epitaxial layers are characterized.

4. The method according to claim 1, wherein: τ ph Determined according to the following equation: Where t is the irradiation time, V const is the surface voltage probe offset.

5. The method according to claim 4 further comprises using a method having a known doping concentration value N D One or more reference samples of τ ph The calibration function τ is determined by the calibration measurement ph With N D The relationship and f cal The inverse calibration function N D With τ ph relationship.

6. The method according to claim 5, further comprising: The effective photon flux φ eff The time constant τ measured under ph Normalized to the calibration photon flux φ cal ,as follows as well as Use the normalized time constant according to the following equation Determine the absolute doping concentration:

7. The method according to claim 4 further comprises calibrating τ for doping concentration ph ,in, The calibration is specific to the semiconductor wafer sample and is based on τ at multiple locations on the wafer sample. ph The characterization period is performed on one site of the measured wafer sample, where all τ ph The measurements were performed under the same illumination conditions.

8. The method according to claim 7, wherein: The calibration includes measuring the corona charge photoneutralization time constant τ using the corona non-contact CV (CnCV) method ph and independently measure the doping concentration N D , where both measurements are performed sequentially one after the other at the same wafer site and within a similar corona charge-induced depletion voltage range.

9. The method according to claim 8, further comprising using τ ph and N D To determine whether N D =τ ph .f cal The wafer-specific inverse calibration function value f cal .

10. The method of claim 7 further comprising determining τ at each wafer site based on ph and using the wafer-specific f determined at a single site cal values ​​to determine the doping concentration at all different wafer sites.

11. The method according to claim 1, wherein: The capacitive probe is a non-contact vibrating Kelvin probe.

12. The method according to claim 1, wherein: The area is illuminated while monitoring the surface voltage.

13. The method according to claim 1, wherein: The region is irradiated separately from monitoring the surface voltage.

14. The method according to claim 1, wherein: The semiconductor sample includes a semiconductor selected from the group consisting of SiC, GaN, and AlGaN.

15. The method of claim 1 further comprising: Dark and dark decay rate ΔV Dark / Δt Dark To identify defective areas of the semiconductor sample.

16. The method of claim 1, further comprising: Dark To identify the contribution of surface photovoltaic effects other than the corona light neutralization to the monitored surface voltage.

17. A system for characterizing semiconductor doping in a wide bandgap semiconductor sample, the system comprising: Surface voltage measurement probe; Corona charge source; light source; a movable wafer chuck configured to support the semiconductor sample relative to the surface voltage measurement probe, the corona charge source, and the light source; as well as a computer controller in communication with the surface voltage measurement probe, the corona charge source, the light source, and the movable wafer chuck, the computer controller being programmed to cause the system to: (i) measuring an initial value V0 of a surface voltage at a region of the surface of the semiconductor sample in darkness; (ii) charging the area to deep depletion in darkness by depositing a defined corona charge at the area; (iii) measuring a surface voltage value at the region in the dark after charging using a surface voltage measurement probe; (iv) using a specific photon flux φ from the light source eff The light irradiates the charged area, the specific photon flux φ eff having a photon energy above the semiconductor bandgap sufficient to generate free minority carriers in the semiconductor sample, thereby causing photoneutralization of the corona charge; (v) monitoring the photoneutralization-induced corona charge decay at the region as a function of the irradiation time t using a contactless time-resolved measurement of the surface voltage V(t) using a surface voltage measurement probe; (vi) Analysis of the monitored time-resolved surface voltage decay data V(t) to determine the photoneutralization time constant τ ph ;as well as (vii) Based on the specific photon flux φ eff The light neutralization time constant τ ph To characterize the semiconductor doping concentration in the region.

18. The system of claim 17, wherein: The light source is arranged to illuminate an area at a position different from a position below the surface voltage measurement probe.

19. The system of claim 18, wherein: The computer controller is programmed to cause the system to illuminate the area prior to measuring the surface voltage at the area to monitor photoneutralization-induced corona charge decay at the area.

20. The system of claim 18, further comprising a moving stage supporting the wafer chuck, and the computer controller is programmed to move the stage to the area between the surface voltage measurement probe and the light source.

21. The system of claim 17, wherein: The light source is arranged to illuminate the area when the area is located below the surface voltage measurement probe.

22. The system of claim 21, wherein: The computer controller is programmed to cause the system to illuminate the area while monitoring photoneutralization-induced corona charge decay at the area.

23. The system of claim 21, wherein: The surface voltage measurement probe includes a transparent electrode, and the light source is arranged to direct light to the area through the transparent electrode.

24. The system of claim 17, wherein: The surface voltage measurement probe is a non-contact vibrating Kelvin probe.

25. The system of claim 17, wherein: The light source includes a light emitting diode or a near UV laser.

26. The system of claim 17, wherein: Based on τ of one or more reference semiconductor samples with known doping concentrations ph The calibration measurements are used to calibrate the system.

Citation Information

Patent Citations

  • Separation Of Doping Density And Minority Carrier Lifetime In Photoluminescence Measurements On Semiconductor Materials

    CN102483378A

  • Semiconductor detection device and detection method thereof

    CN111430258A

  • Field-biased nonlinear optical metrology using corona discharge source

    CN112352150A

  • Method for nondestructively measuring doped concentration and distribution of drift zone of semiconductor device

    CN1243948A

  • Method for measuring doping content of semiconductor based on free carrier absorption technique

    CN1971868A