Method for manufacturing pellicle frame with adhesive layer, pellicle frame with pellicle, pellicle frame with adhesive layer, pellicle, and photomask with pellicle

By placing a protective film with a high glass transition temperature on the surface of the adhesive layer and performing heat treatment, the problem of retaining bubbles and gas paths during photomask adhesion is solved, and the stability of the adhesive surface and protective film assembly is achieved. .

CN118891583APending Publication Date: 2024-11-01MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027893.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

During the photolithography process, the protective film assembly is prone to form retention bubbles when attached to the photomask, resulting in the generation of gas paths. Especially under EUV exposure conditions, the gas paths may expand and cause foreign matters to invade, affecting the performance of the photomask.

Method used

By placing a protective film on the surface of the adhesive layer, and the glass transition temperature of the protective film is higher than the heating temperature during the heating treatment, the strain of the protective film is suppressed, thereby flattening the surface of the adhesive layer and reducing the number of retained bubbles.

Benefits of technology

Effectively suppresses the number of retained bubbles when the protective film assembly is attached to the photomask, reduces the generation of gas paths, ensures the uniformity of the bonding surface of the photomask and the stability of the protective film assembly, and avoids peeling during exposure. question.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891583A_ABST
    Figure CN118891583A_ABST
Patent Text Reader

Abstract

Provided is a method for manufacturing a pellicle frame with an adhesive layer, the method being capable of suppressing the number of bubbles remaining when a pellicle is attached to a photomask. This method for manufacturing a pellicle frame with an adhesive layer is provided with: a step for preparing a frame precursor provided with a pellicle frame (11) and a precursor layer that is formed on the pellicle frame (11) and is a precursor for an adhesive layer (12); forming a frame precursor with a protective film by disposing a protective film (21) having a glass transition temperature higher than the heating temperature of the following engineering on the surface of the precursor layer; and heating the frame precursor with the protective film to form the adhesive layer (12), the surface of which is planarized, from the precursor layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a pellicle assembly frame with an adhesive layer, a pellicle assembly frame with a protective film, a pellicle assembly frame with an adhesive layer, a pellicle assembly, and a method for manufacturing a photomask with a pellicle assembly. Background Art

[0002] The miniaturization of semiconductor integrated circuits has been promoted by photolithography. In photolithography, a photomask with a pattern formed on one side is used. For the photomask, a pellicle assembly is used to prevent foreign matter such as dust from adhering to the surface of the photomask. In many cases, the pellicle assembly has an adhesive layer and is attached to the photomask. Hereinafter, a photomask with a pellicle assembly attached is also referred to as a "photomask with a pellicle assembly".

[0003] Generally speaking, the surface flatness of the adhesive layer of the pellicle assembly is worse than that of the photomask. Therefore, in order to prevent the generation of gas paths, when the pellicle assembly is attached to the photomask, a load is applied to the pellicle assembly so that the adhesive layer is bonded to the photomask without a gap. At this time, the softer the adhesive is, the smaller the force can be used to make the surface of the photomask and the surface of the adhesive layer adhere to each other.

[0004] Patent document 1 discloses a protective film assembly using a soft adhesive. The protective film assembly disclosed in Patent document 1 has an adhesive layer attached to the photomask with an attachment load of 0.008kgf to 5kgf including its own weight. The Young's modulus of the adhesive layer is 0.01MPa to 0.10MPa. The tensile bonding strength of the adhesive layer is 0.02N / mm 2 ~0.10N / mm 2 The flatness of the surface of the adhesive layer is 0 μm to 15 μm.

[0005] The adhesive layer of the pellicle assembly disclosed in Patent Document 1 is formed by applying an adhesive to the end surface of the pellicle assembly frame using a dispenser and heating to cure the adhesive. The resulting pellicle assembly is made to contact the adhesive layer with the photomask, and the pellicle assembly is attached to the photomask by the above-mentioned attachment load.

[0006] Patent Document 1: Japanese Patent Application Publication No. 2012-230227 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In Patent Document 1, the surface of the adhesive layer of the pellicle assembly is not planarized before the adhesive layer is attached to the photomask. Therefore, when the pellicle assembly is attached to the photomask, a large number of trapped bubbles may be formed between the surface of the photomask and the surface of the adhesive layer of the pellicle assembly.

[0009] When attaching the pellicle assembly to the photomask, if there are many trapped bubbles between the adhesive layer of the photomask and the pellicle assembly, an air path may be formed when the pellicle assembly is used for extreme ultraviolet (EUV) exposure or deep ultraviolet (DUV) exposure. An air path is a local gap connecting the outside of the pellicle assembly with the inside of the pellicle assembly. Trapped bubbles are local gaps that do not connect the outside of the pellicle assembly with the inside of the pellicle assembly, and become a factor in the expansion during exposure and the formation of an air path. If an air path is formed, foreign matter outside the pellicle assembly may invade the inside of the pellicle assembly.

[0010] In particular, in EUV exposure, EUV is used as exposure light. EUV has a short wavelength and is therefore easily absorbed by gases such as oxygen or nitrogen. Therefore, EUV exposure is performed in a vacuum atmosphere. If the environment in which the photomask with the pellicle assembly is placed is switched from an atmospheric atmosphere to a vacuum atmosphere for EUV exposure, trapped bubbles are likely to expand. Therefore, if the number of trapped bubbles is large when the pellicle assembly is attached to the photomask in an atmospheric atmosphere, a gas path may be easily formed during EUV exposure.

[0011] The present disclosure has been made in view of the above circumstances.

[0012] An embodiment of the present disclosure is to provide a method for manufacturing a pellicle assembly frame with an adhesive layer, a pellicle assembly frame with a protective film, a pellicle assembly, and a pellicle assembly frame with an adhesive layer that can suppress the number of trapped bubbles when attaching a pellicle assembly to a photomask.

[0013] Another embodiment of the present disclosure is to provide a photomask with a pellicle assembly that can suppress the generation of gas paths.

[0014] Solutions to Solve Problems

[0015] Means for solving the above-mentioned problems include the following embodiments.

[0016] <1> A method for manufacturing a pellicle frame with an adhesive layer, the pellicle frame with an adhesive layer comprising a pellicle frame and an adhesive layer formed on the pellicle frame and used for attaching to a photomask,

[0017] The above manufacturing method has the following advantages:

[0018] Step A, preparing a frame precursor, the frame precursor comprising the pellicle assembly frame and a precursor layer formed on the pellicle assembly frame and serving as a precursor of the adhesive layer;

[0019] Step B, configuring a protective film on the surface of the precursor layer to form a frame precursor with a protective film; and

[0020] Step C, subjecting the frame precursor with the protective film to a heat treatment, so as to form the adhesive layer with a flat surface formed by the precursor layer,

[0021] The glass transition temperature of the protective film is higher than the heating temperature in the step C.

[0022] <2> The method for producing a pellicle assembly frame with an adhesive layer according to <1> above, wherein the protective film has a glass transition temperature of greater than 120°C.

[0023] <3> The method for manufacturing a pellicle frame with an adhesive layer according to <1> or <2> above, wherein in the step C, the heat treatment is performed at 80° C. or higher and for 2 hours or longer.

[0024] <4> The method for manufacturing a pellicle assembly frame with an adhesive layer as described in any one of <1> to <3> above, wherein the adhesive layer includes at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, urethane adhesives and olefin adhesives.

[0025] <5> A pellicle assembly frame with a protective film, comprising:

[0026] Protective film assembly frame,

[0027] An adhesive layer formed on the pellicle frame and used for attaching to the photomask, and

[0028] A protective film attached to the surface of the adhesive layer,

[0029] The glass transition temperature of the protective film is greater than 120°C.

[0030] <6> A protective film assembly frame with an adhesive layer, comprising:

[0031] Protective film assembly frame, and

[0032] an adhesive layer formed on the pellicle assembly frame and used for attaching to the photomask,

[0033] The number of local height differences of 3 μm or more on the surface of the adhesive layer is one or less.

[0034] <7> The pellicle assembly frame with an adhesive layer according to <6> above, wherein the adhesive layer includes at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, urethane adhesives, and olefin adhesives.

[0035] <8> A protective membrane assembly comprising:

[0036] The protective film is supported by the protective film assembly frame, and

[0037] The pellicle assembly frame with adhesive layer as described in <6> or <7> above,

[0038] The protective film includes at least one selected from the group consisting of carbon nanotubes, metal silicide and polysilicon.

[0039] <9> A photomask with a pellicle assembly, comprising:

[0040] Photomask, and

[0041] The pellicle assembly described in <8> above attached to the photomask above,

[0042] In the surface of the adhesive layer in contact with the photomask, an area of ​​a gap between the adhesive layer and the photomask is 0.25% or less with respect to an area of ​​the adhesive layer in contact with the photomask.

[0043] Effects of the Invention

[0044] According to the present disclosure, a method for manufacturing a pellicle frame with an adhesive layer, a pellicle frame with a protective film, and a pellicle frame with an adhesive layer are provided, which can suppress the number of trapped bubbles when attaching a pellicle to a photomask.

[0045] According to the present disclosure, a photomask with a pellicle assembly capable of suppressing the generation of a gas path is provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is a schematic cross-sectional view showing a cross section of a pellicle frame with a protective film according to Example 1. DETAILED DESCRIPTION

[0047] In the present disclosure, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0048] In the numerical ranges recorded in stages in the present disclosure, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of the numerical range recorded in other stages. In the numerical ranges recorded in the present disclosure, the upper limit or lower limit recorded in one numerical range can be replaced by the value shown in the embodiments.

[0049] In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment.

[0050] In the present disclosure, when there are a plurality of substances corresponding to each component, the amount of each component means the total amount of the plurality of substances unless otherwise specified.

[0051] In the present disclosure, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.

[0052] In the present disclosure, "(meth)acrylate" means acrylate or methacrylate.

[0053] (1) Method for manufacturing a protective film assembly frame with an adhesive layer

[0054] The manufacturing method of a protective film component frame with an adhesive layer disclosed in the present invention is a method for manufacturing a protective film component frame with an adhesive layer, which comprises a protective film component frame and an adhesive layer formed on the protective film component frame and used for attaching to a photomask. The manufacturing method comprises steps A, B and C. In step A, a frame precursor is prepared. The frame precursor comprises the protective film component frame, and a precursor layer formed on the protective film component frame and serving as a precursor of the adhesive layer. In step B, a protective film is arranged on the surface of the precursor layer to form a frame precursor with a protective film. In step C, the frame precursor with a protective film is subjected to a heat treatment to form the adhesive layer whose surface is flattened by the precursor layer. The glass transition temperature of the protective film is higher than the heating temperature of step C.

[0055] In the present disclosure, the "precursor of the adhesive layer" becomes an adhesive layer if the heat treatment of step C is performed. In the present disclosure, the "glass transition temperature of the protective film" refers to the glass transition temperature of the substrate layer when the protective film is a multilayer structure including a substrate layer and a layer different from the substrate layer (for example, a release layer, a layer that facilitates peeling from the adhesive layer, an antistatic layer, etc.). The "heating temperature of step C" refers to the set temperature of the heating device when a heating device (for example, an oven, a heating plate, etc.) is used to perform the heat treatment. In detail, the "heating temperature of step C" when an oven is used as the heating device is the set temperature in the oven, and the "heating temperature of step C" when a heating plate is used as the heating device is the set temperature of the heating plate.

[0056] Hereinafter, the manufacturing method of the protective film assembly frame with an adhesive layer disclosed in the present invention is also referred to as the "manufacturing method disclosed in the present invention". Hereinafter, step A is also referred to as the "preparation step". Hereinafter, step B is also referred to as the "configuration step". Hereinafter, step C is also referred to as the "flattening step". Hereinafter, the glass transition temperature is also referred to as "Tg".

[0057] Since the manufacturing method of the present disclosure has the above-described configuration, it is possible to suppress the number of trapped bubbles when the pellicle is attached to the photomask.

[0058] This effect is presumed to be due to the following reasons, but the present invention is not limited thereto.

[0059] In the manufacturing method disclosed in the present invention, the glass transition temperature of the protective film is higher than the heating temperature of process C. That is, the occurrence of strain of the protective film caused by the heating of process C is suppressed. Therefore, in process C, the strain of the protective film is not easily transferred to the surface of the adhesive layer in the present invention. As a result, the surface of the adhesive layer in the present invention is easier to become flat compared to the case of using a protective film whose Tg is below the heating temperature of process C. In other words, the number of local height differences on the surface of the adhesive layer in the present invention is less than that of using a protective film whose Tg is below the heating temperature of process C in an atmospheric atmosphere. It is speculated that as a result, the manufacturing method disclosed in the present invention can suppress the number of trapped bubbles when the protective film assembly is attached to the photomask. Therefore, if the protective film assembly frame with an adhesive layer obtained in the manufacturing method disclosed in the present invention is used as a component of the protective film assembly, it is not easy to generate an air path during exposure. In addition, since there are fewer trapped bubbles, the bonding surface with the photomask becomes uniform. Therefore, the strain of the photomask can be suppressed. Furthermore, since there are fewer trapped bubbles, a wide bonding area can be ensured. Therefore, it is possible to suppress the pellicle from peeling off when the photomask moves during exposure.

[0060] The method for measuring the number of local height differences on the surface of the adhesive layer is the same as the method described in Examples.

[0061] In the manufacturing method of the present disclosure, the preparation step, the placement step, and the planarization step are performed in this order.

[0062] (1.1) Protective film assembly frame with adhesive layer

[0063] The manufacturing method disclosed herein is a method for manufacturing a pellicle assembly frame with an adhesive layer.

[0064] The pellicle frame with adhesive layer is a component of the pellicle, and includes a pellicle frame and an adhesive layer for attaching to a photomask. The adhesive layer is formed on the pellicle frame.

[0065] The protective film assembly will be described later.

[0066] (1.1.1) Protective film assembly frame

[0067] The pellicle assembly frame is a rectangular frame. Specifically, the pellicle assembly frame is a rectangular cylinder. The pellicle assembly frame has a through hole. The through hole represents a space through which light passing through the pellicle passes in order to reach the photomask. The pellicle will be described later.

[0068] The pellicle assembly frame has one end surface on which the adhesive layer is provided and another end surface that supports the pellicle.

[0069] The pellicle assembly frame may have a vent hole having a filter. The vent hole connects the internal space of the pellicle assembly with the external space of the pellicle assembly when the pellicle assembly frame is attached to the photomask. The so-called "internal space of the pellicle assembly" refers to the space surrounded by the pellicle assembly and the photomask. The so-called "external space of the pellicle assembly" refers to the space not surrounded by the pellicle assembly and the photomask. The filter is arranged between the internal space of the pellicle assembly and the external space of the pellicle assembly in a manner to prevent foreign matter from passing through.

[0070] The rectangular shape may be a square or a rectangle. The so-called "rectangle" refers to a right-angled quadrilateral. The so-called "square" refers to a shape in which the lengths of the four sides constituting the rectangle are equal. The "rectangle" refers to a shape other than a square in the rectangle.

[0071] Hereinafter, one end surface of the pellicle frame where the adhesive layer is provided is also referred to as the “end surface for exposure substrate”, and the other end surface of the pellicle frame supporting the pellicle is also referred to as the “end surface for pellicle”.

[0072] The material of the protective film assembly frame is not particularly limited, and examples thereof include metals, resins, and ceramic materials. As a metal, it can be a pure metal or an alloy. Pure metals are composed of single metal elements. As pure metals, for example, aluminum and titanium can be mentioned. Alloys are composed of multiple metal elements, or of metal elements and non-metallic elements. As alloys, stainless steel, magnesium alloys, steel, carbon steel, Invar alloys, etc. can be mentioned. As resins, polyethylene can be mentioned. As ceramic materials, silicon nitride (SiN), silicon carbide (SiC), aluminum oxide (Al2O3), etc. can be mentioned.

[0073] The protective film assembly frame can be a single piece or an assembly. A single piece is obtained by cutting a raw material plate. The so-called "assembly" is a combination of multiple components. Methods for integrating multiple components include methods using known adhesives, methods using fastening components, etc. Fastening components include bolts, nuts, screws, rivets or pins.

[0074] In the case where the protective film assembly frame is an assembly, the materials of the multiple components may be different. In the case where the protective film assembly frame is an assembly, it is preferred that the Young's modulus of the component constituting the end face of the photomask is 60 GPa or less, and the Young's modulus of the component constituting the end face of the protective film (hereinafter referred to as "film support frame component") is 90 GPa or more. Thus, the assembly of the protective film assembly frame can suppress the deformation of the protective film assembly frame caused by the strain of the film support frame component caused by the tension of the protective film.

[0075] Examples of materials having a Young's modulus of 60 GPa or less include magnesium, magnesium alloys, polyethylene terephthalate (PET) resins, and resins, etc. Examples of materials having a Young's modulus of 90 GPa or more include titanium, titanium alloys, and silicon.

[0076] The Young's modulus is measured by a tensile test (JIS G0567J). However, when the pellicle assembly frame is made of resin, the Young's modulus is measured by a three-point bending test (JIS K7171). Whether the pellicle assembly frame is made of resin is determined by whether thermal decomposition occurs at 550°C.

[0077] (1.1.2) Adhesive layer

[0078] The adhesive layer is formed on the pellicle frame. Specifically, the adhesive layer is formed on the end surface of the pellicle frame for the exposure substrate.

[0079] The adhesive layer is a gel-like viscoelastic body. The adhesive layer preferably has viscosity and cohesion. The so-called "viscosity" refers to the liquid-like property of contacting and wetting the photomask as an adherend. The so-called "cohesion" refers to the solid-like property of resisting peeling from the photomask.

[0080] The Tg of the adhesive layer is preferably greater than -25°C and less than 10°C. Thus, the adhesive layer has adhesion in the operating temperature range of the pellicle (for example, 20°C or higher) and is less likely to be peeled off from the photomask even when exposed to a high temperature environment.

[0081] From the viewpoint of being less likely to peel from the photomask even when exposed to a high temperature environment, the lower limit of Tg of the adhesive layer is preferably higher than -25°C, more preferably -22°C or higher, further preferably -20°C or higher, and most preferably -18°C or higher.

[0082] From the viewpoint of imparting adhesiveness at room temperature, the upper limit of Tg of the adhesive layer is preferably less than 10°C, more preferably 5°C or lower, and further preferably 0°C or lower.

[0083] The method for measuring Tg of the adhesive layer is in accordance with JIS K 7112. Specifically, Tg of the adhesive layer was measured using a differential scanning calorimeter (DSC) at a temperature increase rate of 20° C. / min under nitrogen.

[0084] The adhesive layer is formed by an adhesive composition. As the adhesive composition constituting the adhesive layer, there is no particular limitation, and examples thereof include acrylic adhesives, silicone adhesives, styrene butadiene adhesives, carbamate adhesives, olefin adhesives, and the like. Among them, from the viewpoint of reducing the amount of outgassing generated by the protective film assembly, the adhesive layer preferably includes at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, carbamate adhesives, and olefin adhesives, more preferably includes an acrylic adhesive, and further preferably an acrylic adhesive. Details about the acrylic adhesive will be described later.

[0085] The thickness of the adhesive layer is not particularly limited, but is preferably 10 μm to 500 μm, more preferably 100 μm to 400 μm, and further preferably 200 μm to 300 μm. When the thickness of the adhesive layer is within the above range, the amount of outgassing from the adhesive layer is less likely to have an effect.

[0086] The method for measuring the thickness of the adhesive layer is the same as in the example.

[0087] (1.2) Preparation process

[0088] The manufacturing method disclosed in the present invention has a preparation step.

[0089] In the preparation step, a frame precursor is prepared. The frame precursor includes a pellicle frame and a precursor layer which is a precursor of an adhesive layer. The precursor layer is formed on the pellicle frame. Specifically, the precursor layer is formed on the end surface of the pellicle frame for the exposure substrate.

[0090] The method for preparing the frame precursor is not particularly limited, and examples thereof include a method of applying a coating composition to a pellicle frame to form a precursor layer on the photomask end surface of the pellicle frame.

[0091] (1.2.1) Coating composition

[0092] The coating composition includes a composition containing a compound selected from various polymers, solvents, crosslinking agents, catalysts, initiators, etc. according to the type of adhesive layer. The coating composition is a precursor of the adhesive composition. That is, if the coating composition is cured, it becomes the above-mentioned adhesive composition.

[0093] (1.2.2) Coating

[0094] The method for applying the coating composition to the end surface for photomask of the pellicle frame is not particularly limited, and examples thereof include a method using a dispenser.

[0095] The area to which the coating composition is applied is preferably only the central portion of each side between the four corners of the end face of the photomask, rather than the entire surface of the end face of the photomask. In other words, the area to which the coating composition is applied preferably does not include the edge portion of the through-hole side of the protective film assembly frame on each side between the four corners and the edge portion on the side opposite to the through-hole side of the protective film assembly frame. Thus, when the protective film assembly is attached to the photomask, the adhesive layer is less likely to overflow to the inner and outer peripheral wall sides of the protective film assembly frame compared to the case where the coating composition is applied to the entire surface of the end face of the photomask. Therefore, the adhesive layer is less likely to be exposed. As a result, the amount of outgassing can be further reduced.

[0096] The thickness of the precursor layer may be any thickness as long as the thickness of the adhesive layer is within the above range.

[0097] (1.3) Drying process

[0098] The manufacturing method of the present disclosure may include a drying step. When the manufacturing method of the present disclosure includes a drying step, the preparation step, the drying step, the placement step, and the planarization step are performed in this order.

[0099] In the drying process, the frame precursor is dried. In order to make it easy to apply the coating composition to the end face of the photomask of the protective film assembly frame, the coating composition may contain a solvent. By performing the drying process, most of the solvent contained in the precursor layer of the frame precursor will evaporate before performing the flattening process. As a result, it is easy to obtain an adhesive layer with a flattened surface.

[0100] The heating temperature for the drying treatment is preferably lower than the heating temperature for the planarization step and can be appropriately selected depending on the type of the coating composition, but is preferably 40 to 120°C, more preferably 50 to 110°C, and further preferably 60 to 100°C.

[0101] The heating time for the drying treatment can be appropriately selected depending on the heating temperature for the drying treatment and the type of the coating composition, and is preferably 10 minutes to 5 hours, more preferably 20 minutes to 4 hours, and even more preferably 30 minutes to 3 hours.

[0102] The method of drying the precursor layer is not particularly limited, and examples thereof include a method using an oven, etc. In the method using an oven, a precursor frame is placed in the oven, and the precursor frame itself is dried, thereby drying the precursor layer.

[0103] When the precursor layer is heated in an oven, the set temperature in the oven is the same as the temperature range exemplified above as the heating temperature for the drying process. The set temperature in the oven means the temperature inside the oven. The time for heating the precursor layer in the oven is the same as the time range exemplified above as the heating time for the drying process.

[0104] (1.4) Configuration process

[0105] The manufacturing method disclosed herein includes a placement step.

[0106] In the disposing step, a protective film is disposed on the surface of the precursor layer of the frame precursor to form a frame precursor with a protective film.

[0107] (1.4.1) Protective film

[0108] In the planarization process, the flat surface of the planarization article can be transferred to the surface of the precursor layer by bringing the flat surface of the planarization article into contact with the surface of the precursor layer of the frame precursor with the protective film through the protective film. At this time, the protective film easily separates the frame precursor with the protective film from the planarization article. The protective film protects at least the surface of the precursor layer or the adhesive layer that contacts the photomask. The protective film can be peeled off relative to the adhesive layer.

[0109] The shape of the protective film is not particularly limited as long as it is a shape that conforms to the shape of the pellicle assembly frame. The protective film may have an opening similarly to the pellicle assembly frame.

[0110] The thickness of the protective film is not particularly limited, but is preferably 5 μm to 500 μm, and more preferably 30 μm to 200 μm.

[0111] The protective film preferably includes a substrate layer and a release layer, and may include other layers (eg, an antistatic layer) different from the substrate layer and the release layer as necessary. The layer structure of the protective film is not particularly limited, and may include two or more layers.

[0112] The substrate layer contains a resin having a glass transition temperature higher than the heating temperature of the planarization process. As the resin constituting the substrate layer, it can be appropriately selected according to the heating temperature of the planarization process, for example, polyester resins (for example, polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), etc.), olefin resins, polyvinyl chloride, vinyl acetate resins, polycarbonate, polyphenylene sulfide, amide resins (for example, polyamide (nylon), wholly aromatic polyamide (aramid), etc.), polyimide resins, polyether ether ketone (PEEK), fluorine resins, etc. As olefin resins, resins with α-olefins (for example, polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), ethylene-propylene copolymers, ethylene-vinyl acetate copolymers (EVA), etc.) as monomer components can be cited.

[0113] The release layer is formed of a release agent. Examples of the release agent include silicone-based release agents and fluorine-based release agents.

[0114] The Tg of the protective film (i.e., the Tg of the substrate layer) is preferably higher than 120° C. The Tg of a commonly used protective film made of polyethylene terephthalate (PET) is lower than 100° C. A PET protective film generally includes a substrate layer made of PET and a release layer formed on one surface of the substrate layer.

[0115] Examples of protective films having a Tg greater than 120° C. include PEN protective films, polyamide (aramid), polyimide, polyamide-imide, polyetheretherketone resin (PEEK), polyphenylene sulfide, polyethersulfone, polycarbonate, polyarylate, polysulfone, polytetrafluoroethylene, etc. The PEN protective film has a base material layer formed of PEN.

[0116] From the viewpoint of both volatilizing the residue of the precursor layer in a short time and reducing the number of trapped bubbles, the lower limit of the Tg of the protective film is more preferably 130°C or more, further preferably 140°C or more, and particularly preferably 150°C or more. The upper limit of the Tg of the protective film is not particularly limited, but is preferably 200°C or less, and more preferably 180°C or less. From these viewpoints, the Tg of the protective film is preferably 130°C or more and 200°C or less, more preferably 140°C or more and 200°C or less, and further preferably 150°C or more and 180°C or less.

[0117] Examples of the material of the base material layer of the protective film having a Tg of 120° C. to 200° C. include PEN, polyamide (aramid), PEEK, polyphenylene sulfide, polycarbonate, polyarylate, polysulfone, and polytetrafluoroethylene.

[0118] Examples of the material of the base material layer of the protective film having a Tg of 140° C. to 200° C. include PEN, PEEK, polycarbonate, polyarylate, and polysulfone.

[0119] The method for measuring Tg of the protective film is the same as the method described in Examples.

[0120] The temperature difference between the Tg of the protective film and the heating temperature of the planarization step is greater than 0° C., preferably 5° C. or more, more preferably 10° C. or more, and further preferably 20° C. or more. If the temperature difference is 5° C. or more, the generation of strain in the protective film caused by heating in the planarization step can be more reliably suppressed.

[0121] “The temperature difference between Tg of the protective film and the heating temperature in the planarization step” refers to a value obtained by subtracting the heating temperature (° C.) in the planarization step from the Tg (° C.) of the protective film.

[0122] (1.4.2) Configuration

[0123] The method of placing the protective film on the surface of the precursor layer of the frame precursor is not particularly limited, and examples thereof include a method of placing the precursor frame on the protective film, a method of placing the protective film on the precursor frame, etc. After placing the protective film on the surface of the precursor layer of the frame precursor, pressure (load) may be uniformly applied to the entire precursor layer.

[0124] (1.5) Planarization process

[0125] The manufacturing method disclosed herein includes a planarization step.

[0126] In the planarization step, the frame precursor with the protective film is subjected to a heat treatment to form an adhesive layer with a planarized surface from the precursor layer of the precursor frame. That is, a pellicle frame with the protective film is obtained.

[0127] The conditions for the heat treatment in the planarization step can be appropriately selected depending on the type of the coating composition, etc., as long as the heating temperature is lower than the Tg of the protective film, but are preferably 80° C. or higher and 2 hours or longer.

[0128] From the viewpoint of volatilizing the residue of the precursor layer, the heating temperature of the heat treatment is more preferably 80°C to 200°C, further preferably 90°C to 190°C, and particularly preferably 100°C to 180°C.

[0129] The heating time of the heat treatment can be appropriately selected depending on the heating temperature of the heat treatment and the type of the coating composition, and is preferably 2 to 48 hours, more preferably 3 to 36 hours, further preferably 4 to 24 hours, and further preferably 10 to 24 hours.

[0130] The thickness of the precursor layer immediately after the coating composition is applied usually varies depending on the location of the precursor layer. In the planarization process, it is preferred to heat the precursor layer while it is in contact with the flat surface of the planarization article via a protective film. Thus, the surface of the adhesive layer can be further planarized.

[0131] Hereinafter, the article for flattening which is brought into contact with the precursor frame with a protective film is referred to as a "first contact article".

[0132] There is no particular limitation on the method of making the precursor layer of the precursor frame with a protective film contact the flat surface of the flattening article via the protective film, and for example, an inversion method, a loading method, and the like can be cited. In the loading method, a frame precursor with a protective film is placed on the flat surface of the flattening article. In the inversion method, a flattening article is placed on the frame precursor with a protective film. Whether it is the loading method or the inversion method, the flattening article can be further brought into contact with the protective film end surface of the protective film assembly frame of the precursor frame with a protective film. Among them, from the viewpoint of making it easy to heat the precursor layer when heating using a heating plate, the loading method is preferred.

[0133] When the flat surface is brought into contact with the precursor layer via the protective film, the pressure (load) can be uniformly applied to the entire precursor layer. The pressure (load) uniformly applied to the entire precursor layer is not particularly limited, but is preferably 10 g / cm2 from the perspective of reducing the strain of the protective film assembly frame. 2 ~1000g / cm 2 , more preferably 100 g / cm 2 ~800g / cm 2 , more preferably 300g / cm 2 ~600g / cm 2 .

[0134] The TIR value of the flat surface of the flattening article is less than 10 μm. As a result, the TIR value of the adhesive layer can be made less than 10 μm. That is, the number of local height differences on the surface of the adhesive layer can be reduced. From the viewpoint of forming an adhesive layer with a lower TIR value, the TIR value of the flat surface of the flattening article is preferably less than 5 μm, more preferably less than 3 μm, and the closer to 0 μm, the better. As the flattening article, for example, a glass substrate can be cited. In the flattening process, it is preferred to perform a heat treatment in a state where the flat surface of the glass substrate is in contact with the surface of the precursor layer via a protective film.

[0135] There is no particular limitation on the method of heat-treating the precursor frame with the protective film in a state where the precursor layer is in contact with the flat surface via the protective film, and examples thereof include a method using an oven, a method using a heating plate, and a method of contacting a heated flattening article. In the method using an oven, a first contact article is placed in the oven, and the first contact article itself is heated, thereby heat-treating the precursor frame with the protective film. In the method using a heating plate, for example, the first contact article is placed on a heating plate in such a manner that the flattening article that contacts the precursor layer of the first contact article via the protective film contacts the plate of the heating plate, and the precursor layer is heated by the flattening article, thereby heat-treating the precursor frame with the protective film. In the method of contacting the heated flat surface, for example, a heated flattening article is prepared, and the first contact article is placed on the flattening article to heat the precursor layer, thereby heat-treating the precursor frame with the protective film.

[0136] When an oven is used, the set temperature in the oven is the same as the temperature range exemplified above as the heating temperature for the heat treatment. The set temperature in the oven means the temperature inside the oven. The time for heating the precursor layer using the oven is the same as the time range exemplified above as the heating time for the heat treatment.

[0137] When a hot plate is used, the set temperature of the hot plate is in the same temperature range as the heating temperature of the heat treatment described above. The set temperature of the hot plate indicates the surface temperature of the hot plate. The time for heating the precursor layer using the hot plate is in the same time range as the heating time of the heat treatment described above.

[0138] In the flattening process, in order to further promote flattening, before the aforementioned frame precursor with a protective film is subjected to a heat treatment, the precursor layer of the precursor frame with a protective film may be brought into contact with the heated flat surface via the protective film. The method of bringing the precursor layer of the precursor frame with a protective film into contact with the heated flat surface via the protective film is not particularly limited, and hot pressing and the like may be cited. From the viewpoint of easy flattening, the heating temperature of the heated flat surface is the same as the temperature range exemplified as the heating temperature of the heat treatment, and the heating time may be set to be 10 seconds or more.

[0139] (1.6) Peeling process

[0140] The manufacturing method disclosed herein generally includes a stripping step, which is performed after the planarization step.

[0141] In the peeling step, the protective film is peeled off from the pellicle assembly frame with the protective film. Thus, the pellicle assembly frame with the adhesive layer can be obtained.

[0142] Examples of a method for peeling the protective film from the pellicle frame with the protective film include a method of peeling the protective film by applying a mechanical force in a direction of peeling from the pellicle frame.

[0143] (1.7) Acrylic adhesive

[0144] Hereinafter, an acrylic adhesive will be described as an example of the adhesive composition.

[0145] The acrylic pressure-sensitive adhesive contains a copolymer (hereinafter referred to as a "(meth)acrylate alkyl ester copolymer").

[0146] (1.7.1) (Meth) alkyl acrylate copolymer

[0147] The alkyl (meth)acrylate copolymer preferably comprises

[0148] (Meth) alkyl acrylate monomer, and

[0149] A copolymer of a monomer having a functional group reactive with at least one of an isocyanate group, an epoxy group and an acid anhydride (hereinafter referred to as a "functional group-containing monomer").

[0150] The acrylic adhesive contains an alkyl (meth)acrylate copolymer, so that the pellicle is not easily peeled off from the photomask even when exposed to a high temperature environment (for example, a temperature environment of 60° C. or higher), and the generation of residual adhesive can be suppressed.

[0151] The term “adhesive residue” refers to a state where at least a portion of the adhesive layer remains on the photomask after the pellicle assembly is peeled off from the photomask.

[0152] The weight average molecular weight (Mw) of the (meth)acrylic acid alkyl ester copolymer is preferably 30,000 to 2.5 million, more preferably 50,000 to 1.5 million, and even more preferably 70,000 to 1.2 million.

[0153] If the upper limit of the weight average molecular weight (Mw) of the (meth) alkyl acrylate copolymer is 2.5 million or less, even if the solid content concentration of the coating composition is increased, the solution viscosity can be controlled to a range that is easy to process. The upper limit of the weight average molecular weight (Mw) of the (meth) alkyl acrylate copolymer is preferably 2.5 million or less, more preferably 1.5 million or less, and further preferably 1.2 million or less.

[0154] If the lower limit of the weight average molecular weight (Mw) of the (meth) alkyl ester copolymer is 30,000 or more, the pellicle assembly is less likely to be peeled off from the photomask even when exposed to a high temperature environment (e.g., 60° C.), and the generation of residual adhesive can be suppressed. The lower limit of the weight average molecular weight (Mw) of the (meth) alkyl ester copolymer is preferably 30,000 or more, more preferably 50,000 or more, and even more preferably 70,000 or more.

[0155] The weight average molecular weight (Mw) of the (meth)acrylic acid alkyl ester copolymer is measured by GPC (gel permeation chromatography).

[0156] For example, generally speaking, the higher the monomer concentration during the polymerization reaction, the greater the weight average molecular weight (Mw), and the less the amount of the polymerization initiator or the lower the polymerization temperature, the greater the weight average molecular weight (Mw). The weight average molecular weight (Mw) can be controlled by adjusting the monomer concentration, the amount of the polymerization initiator, and the polymerization temperature.

[0157] The number average molecular weight (Mn) of the (meth)acrylic acid alkyl ester copolymer is preferably 5,000 to 500,000, more preferably 8,000 to 300,000, further preferably 10,000 to 200,000, and most preferably 20,000 to 200,000.

[0158] If the upper limit of the number average molecular weight (Mn) of the (meth) alkyl acrylate copolymer is 500,000 or less, even if the solid content concentration of the coating composition is increased, the solution viscosity can be controlled to a range that is easy to process. The upper limit of the number average molecular weight (Mn) of the (meth) alkyl acrylate copolymer is preferably 500,000 or less, more preferably 300,000 or less, and further preferably 200,000 or less. If the lower limit of the number average molecular weight (Mn) of the (meth) alkyl acrylate copolymer is 5,000 or more, the protective film assembly is less likely to be peeled off from the photomask even if exposed to a high temperature environment (for example, 60°C), and the generation of residual glue can be suppressed. The lower limit of the number average molecular weight (Mn) of the (meth) alkyl acrylate copolymer is preferably 5,000 or more, more preferably 8,000 or more, further preferably 10,000 or more, and most preferably 20,000 or more.

[0159] The method for measuring the number average molecular weight (Mn) of the alkyl (meth)acrylate copolymer is the same as the method for measuring the weight average molecular weight (Mw) of the alkyl (meth)acrylate copolymer described above.

[0160] The "weight average molecular weight (Mw) / number average molecular weight (Mn)" (hereinafter referred to as "Mw / Mn") of the alkyl (meth)acrylate copolymer is preferably 1.0 to 10.0, more preferably 2.5 to 9.0, further preferably 2.5 to 8.0, and most preferably 3.0 to 7.0.

[0161] When Mw / Mn is within the above range, the copolymer can be easily produced and the generation of residual adhesive can be suppressed.

[0162] If the upper limit of Mw / Mn is 10.0 or less, the generation of adhesive residue can be suppressed. The upper limit of Mw / Mn is preferably 10.0 or less, more preferably 9.0 or less, further preferably 8.0 or less, and most preferably 7.0 or less.

[0163] If the lower limit of Mw / Mn is 1.0 or more, the copolymer can be easily produced. The lower limit of Mw / Mn is preferably 1.0 or more, more preferably 2.0 or more, further preferably 2.5 or more, and most preferably 3.0 or more.

[0164] The alkyl (meth)acrylate monomer preferably includes an alkyl (meth)acrylate monomer having an alkyl group having 1 to 14 carbon atoms. Examples of the alkyl (meth)acrylate monomer having an alkyl group having 1 to 14 carbon atoms include a (meth)acrylate monomer of a linear aliphatic alcohol and a (meth)acrylate monomer of a branched aliphatic alcohol.

[0165] Examples of the (meth)acrylate monomer of a linear aliphatic alcohol include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and lauryl (meth)acrylate.

[0166] Examples of the (meth)acrylate monomer of a branched aliphatic alcohol include isobutyl (meth)acrylate, isopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and isononyl (meth)acrylate. These may be used alone or in combination of two or more.

[0167] Among these, the (meth)acrylic acid alkyl ester monomer preferably has at least one of an alkyl group having 1 to 3 carbon atoms and an alicyclic alkyl group.

[0168] Hereinafter, an alkyl (meth)acrylate monomer having at least one of an alkyl group and an alicyclic alkyl group having 1 to 3 carbon atoms is referred to as a “high Tg monomer.” “Tg” is a glass transition temperature.

[0169] In order to further reduce the amount of outgassing, the (meth)acrylic acid alkyl ester monomer is more preferably an alkyl acrylate monomer having an alkyl group or an alicyclic alkyl group with a carbon number of 1 to 3, and is further preferably an alkyl acrylate monomer having an alkyl group with a carbon number of 1 to 3. In the case of an alkyl acrylate monomer having an alicyclic alkyl group, the alicyclic alkyl group preferably has 5 to 10 carbon atoms from the viewpoint of easy availability.

[0170] When the alkyl (meth)acrylate monomer contains a high Tg monomer, the pellicle is less likely to be peeled off from the photomask even when exposed to a high temperature atmosphere.

[0171] Specifically, examples of the high Tg monomer include methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, cyclohexyl acrylate, dicyclopentanyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, cyclohexyl methacrylate, and dicyclopentanyl methacrylate.

[0172] The content of the alkyl (meth)acrylate monomer is preferably 80 to 99.5 parts by mass, more preferably 85 to 99.5 parts by mass, and even more preferably 87 to 99.5 parts by mass, based on 100 parts by mass of the total amount of monomers constituting the copolymer.

[0173] When the content of the alkyl (meth)acrylate monomer is within a range of 80 parts by mass to 99.5 parts by mass, appropriate adhesive force can be achieved.

[0174] The functional group-containing monomer is a monomer that can be copolymerized with the (meth)acrylic acid alkyl ester monomer. The functional group-containing monomer has a functional group reactive with at least one of an isocyanate group, an epoxy group, and an acid anhydride.

[0175] Examples of the functional group-containing monomer include a carboxyl group-containing monomer, a hydroxyl group-containing monomer, and an epoxy group-containing monomer.

[0176] Examples of the carboxyl group-containing monomer include (meth)acrylic acid, itaconic acid, (meth)acryloitaconic acid, maleic acid, and crotonic acid.

[0177] Examples of the hydroxyl group-containing monomer include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.

[0178] Examples of the epoxy group-containing monomer include glycidyl (meth)acrylate and the like.

[0179] These may be used alone or in combination of two or more.

[0180] In particular, from the perspectives of copolymerizability and versatility, the functional group-containing monomer preferably includes a hydroxyl group-containing (meth)acrylic acid having a hydroxyalkyl group having 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate, or glycidyl (meth)acrylate as an epoxy group-containing monomer.

[0181] The content of the functional group-containing monomer is, for example, preferably 0.5 to 20 parts by mass relative to 100 parts by mass of the total amount of monomers constituting the copolymer.

[0182] From the viewpoint of improving the adhesive strength of the adhesive layer, the lower limit of the content of the functional group-containing monomer is more preferably 1 part by mass or more, further preferably 2 parts by mass or more, and particularly preferably 3 parts by mass or more, relative to 100 parts by mass of the total amount of monomers constituting the (meth)acrylate alkyl ester copolymer.

[0183] From the viewpoint of achieving appropriate adhesive strength of the adhesive layer, the upper limit of the content of the functional group-containing monomer is more preferably 15 parts by mass or less, and further preferably 10 parts by mass or less, based on 100 parts by mass of the total amount of monomers constituting the (meth)acrylate alkyl ester copolymer.

[0184] (1.7.2) Aggregation method

[0185] The polymerization method of the (meth)acrylic acid alkyl ester copolymer is not particularly limited, and examples thereof include solution polymerization, bulk polymerization, emulsion polymerization, and various radical polymerizations.

[0186] The (meth)acrylate copolymer obtained by these polymerization methods may be any of a random copolymer, a block copolymer, a graft copolymer, and the like.

[0187] (1.7.3) Polymerization solvent

[0188] The reaction solution contains a polymerization solvent.

[0189] In solution polymerization, as a polymerization solvent, for example, propyl acetate, ethyl acetate, toluene, etc. can be used. Thus, the viscosity of the copolymer solution can be adjusted. As a result, when polymerization is performed, the thickness and width of the coating composition can be easily controlled.

[0190] Examples of the diluting solvent include propyl acetate, acetone, ethyl acetate, and toluene.

[0191] The viscosity of the copolymer solution is preferably 1000 Pa·s or less, more preferably 500 Pa·s or less, and even more preferably 200 Pa·s or less.

[0192] The viscosity of the copolymer solution is the viscosity of the copolymer solution at a temperature of 25° C. and can be measured using an E-type viscometer.

[0193] (1.7.4) Solution polymerization

[0194] As an example of solution polymerization, there can be mentioned a method in which a polymerization initiator is added to a mixed solution of monomers under a stream of an inert gas such as nitrogen, and a polymerization reaction is carried out at 50° C. to 100° C. for 4 to 30 hours.

[0195] Examples of the polymerization initiator include azo-based polymerization initiators and peroxide-based polymerization initiators. Examples of the azo-based polymerization initiator include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2-methylpropionic acid) dimethyl ester, and 4,4'-azobis(4-cyanovaleric acid). Examples of the peroxide-based polymerization initiator include benzoyl peroxide.

[0196] The content of the polymerization initiator is preferably 0.01 to 2.0 parts by mass relative to 100 parts by mass of the total amount of all monomers constituting the alkyl (meth)acrylate copolymer.

[0197] In solution polymerization, in addition to the polymerization initiator, a chain transfer agent, an emulsifier, etc. may be added to the mixed solution of the monomers. As the chain transfer agent, the emulsifier, etc., known ones may be appropriately selected and used.

[0198] The amount of the polymerization initiator remaining in the adhesive layer is preferably small, because this can reduce the amount of outgassing generated during exposure.

[0199] Methods for reducing the amount of polymerization initiator remaining in the adhesive layer include: a method of reducing the amount of polymerization initiator added when polymerizing the (meth)acrylate alkyl ester copolymer to the necessary minimum; a method of using a polymerization initiator that is easily thermally decomposed; a method of heating the adhesive at a high temperature for a long time during the adhesive coating and drying process to decompose the polymerization initiator during the drying process, etc.

[0200] The 10-hour half-life temperature is used as an indicator of the thermal decomposition rate of the polymerization initiator. The so-called "half-life" refers to the time until the polymerization initiator is decomposed by half. The 10-hour half-life temperature refers to the temperature at which the half-life is 10 hours.

[0201] As the polymerization initiator, it is preferred to use a polymerization initiator with a low 10-hour half-life temperature. The lower the 10-hour half-life temperature, the easier it is for the polymerization initiator to thermally decompose. As a result, it is not easy to remain in the adhesive layer.

[0202] The 10-hour half-life temperature of the polymerization initiator is preferably 80° C. or lower, more preferably 75° C. or lower.

[0203] Examples of azo polymerization initiators having a low 10-hour half-life temperature include 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) (10-hour half-life temperature: 30°C), 2,2'-azobisisobutyronitrile (10-hour half-life temperature: 65°C), 2,2-azobis(2,4-dimethylvaleronitrile) (10-hour half-life temperature: 51°C), dimethyl 2,2'-azobis(2-methylpropionate) (10-hour half-life temperature: 66°C), and 2,2'-azobis(2-methylbutyronitrile) (10-hour half-life temperature: 67°C).

[0204] Examples of peroxide-based polymerization initiators having a low 10-hour half-life temperature include dibenzoyl peroxide (10-hour half-life temperature: 74° C.) and dilauroyl peroxide (10-hour half-life temperature: 62° C.).

[0205] (1.7.5) Cross-linking agent

[0206] The acrylic adhesive preferably contains a reaction product of an alkyl (meth)acrylate copolymer and a crosslinking agent. This can improve the cohesive force of the obtained adhesive layer, suppress residual adhesive when the pellicle assembly is peeled off from the photomask, and improve the adhesive strength at high temperatures (for example, a temperature environment of 60°C or higher).

[0207] The cross-linking agent has at least one of an isocyanate group, an epoxy group, and an acid anhydride.

[0208] Examples of the crosslinking agent include monofunctional epoxy compounds, polyfunctional epoxy compounds, acid anhydride compounds, metal salts, metal alkoxides, aldehyde compounds, non-amino resin amino compounds, urea compounds, isocyanate compounds, metal chelate compounds, melamine compounds, and aziridine compounds.

[0209] Among them, the crosslinking agent is more preferably at least one of a monofunctional epoxy compound, a polyfunctional epoxy compound, an isocyanate compound and an acid anhydride compound, and more preferably an acid anhydride compound, from the viewpoint of excellent reactivity with the functional group component possessed by the (meth)acrylate copolymer.

[0210] Examples of the monofunctional epoxy compound include glycidyl (meth)acrylate, glycidyl acetate, butyl glycidyl ether, and phenyl glycidyl ether.

[0211] Examples of the polyfunctional epoxy compound include neopentyl glycol diglycidyl ether, polyethylene glycol diglycidyl ether, bisphenol A diglycidyl ether, bisphenol F diglycidyl ether, phthalic acid diglycidyl ester, dimer acid diglycidyl ester, isocyanuric acid triglycidyl ester, diglycerol triglycidyl ether, sorbitol tetraglycidyl ether, N,N,N',N'-tetraglycidyl meta-xylene diamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and N,N,N',N'-tetraglycidyl diaminodiphenylmethane.

[0212] Examples of the acid anhydride-based compound include aliphatic dicarboxylic acid anhydrides and aromatic polycarboxylic acid anhydrides.

[0213] Examples of the aliphatic dicarboxylic anhydride include maleic anhydride, hexahydrophthalic anhydride, hexahydro-4-methylphthalic anhydride, bicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, 2-methylbicyclo[2.2.1]heptane-2,3-dicarboxylic anhydride, and tetrahydrophthalic anhydride.

[0214] Examples of the aromatic polycarboxylic acid anhydride include phthalic anhydride and trimellitic anhydride.

[0215] Examples of the isocyanate compound include xylylene diisocyanate, hexamethylene diisocyanate, toluene diisocyanate, and multimers, derivatives, and polymers thereof, etc. These may be used alone or in combination of two or more.

[0216] The crosslinking agent may be a product. Examples of the crosslinking agent product include "RIKACID MH-700G" manufactured by Shin Nippon Rika Co., Ltd.

[0217] The adhesive layer contains a reaction product of the copolymer and a cross-linking agent, and the content of the cross-linking agent is preferably 0.01 to 3.00 parts by mass based on 100 parts by mass of the total amount of monomers constituting the copolymer.

[0218] The content of the crosslinking agent is preferably 0.01 to 3.00 parts by mass based on 100 parts by mass of the total amount of the monomers constituting the copolymer, more preferably 0.10 to 3.00 parts by mass, and even more preferably 0.1 to 2.00 parts by mass from the viewpoint of obtaining an adhesive that is less likely to produce adhesive residue.

[0219] If the upper limit of the content of the crosslinking agent is less than 3.00 parts by mass, the crosslinking density of the (meth) alkyl acrylate copolymer will not become too large. Therefore, it is believed that the adhesive absorbs the stress applied to the photomask, and the effect of the adhesive layer on the flatness of the photomask is alleviated. The upper limit of the content of the crosslinking agent is preferably less than 2.00 parts by mass, more preferably less than 1.00 parts by mass.

[0220] On the other hand, when the lower limit of the content of the crosslinking agent is 0.01 parts by mass or more, the crosslinking density does not become too low, so that workability in the production process is maintained and adhesive residue is less likely to be generated when the pellicle is peeled from the photomask.

[0221] When the content of the cross-linking agent is within the range of 0.01 parts by mass to 3.00 parts by mass, a pellicle in which the generation of residual adhesive is further suppressed can be obtained.

[0222] (1.7.6) Catalyst

[0223] The coating composition may further contain a catalyst, thereby further accelerating the curing of the alkyl (meth)acrylate copolymer.

[0224] As the catalyst, for example, an amine catalyst can be mentioned. As the amine catalyst, octanoate of (1,8-diazabicyclo-(5.4.0)undecene-7), triethylenediamine, etc. can be mentioned. The amine catalyst can be a product of San-Apro (Strain) such as "DBU", "DBN", "U-CAT", "U-CAT SA1", "U-CAT SA102", etc.

[0225] The content of the catalyst is preferably 0.01 to 3.00 parts by mass, more preferably 0.10 to 1.00 parts by mass, based on 100 parts by mass of the alkyl (meth)acrylate copolymer.

[0226] (1.7.7) Surface modifiers

[0227] The coating composition preferably does not contain a surface modifier, thereby being able to suppress the amount of outgassing.

[0228] (1.7.8) Additives

[0229] The coating composition may contain additives such as fillers, pigments, diluents, antioxidants, tackifiers, etc. as necessary. These additives may be used alone or in combination of two or more.

[0230] (1.7.9) Dilution solvent

[0231] The coating composition may contain a diluent solvent. Thus, the viscosity of the coating composition can be adjusted. As a result, when the coating composition is applied to the end surface of the photomask of the pellicle assembly frame, the thickness and width of the coating composition can be easily controlled.

[0232] Examples of the diluting solvent include propyl acetate, acetone, ethyl acetate, and toluene.

[0233] The viscosity of the coating composition is preferably 50 Pa·s or less, more preferably 10 Pa·s to 40 Pa·s, and further preferably 20 Pa·s to 30 Pa·s.

[0234] The viscosity of the coating composition is the viscosity of the coating composition when the temperature is 25° C., and can be measured using an E-type viscometer.

[0235] (2) Protective film assembly frame with protective film

[0236] The pellicle assembly frame with protective film disclosed in the present invention comprises a pellicle assembly frame, an adhesive layer for attaching to a photomask, and a protective film. The adhesive layer is formed on the pellicle assembly frame. The protective film is attached to the surface of the adhesive layer. The glass transition temperature of the protective film is greater than 120°C.

[0237] Since the pellicle frame with a protective film of the present disclosure has the above-described configuration, the number of trapped bubbles when the pellicle is attached to a photomask can be reduced.

[0238] This effect is presumed to be due to the following reasons, but the present invention is not limited thereto.

[0239] The protective film assembly frame with a protective film disclosed in the present invention can be suitably manufactured by the manufacturing method of the protective film assembly frame with an adhesive layer disclosed in the present invention. The heating temperature of the flattening process of the manufacturing method of the protective film assembly frame with an adhesive layer disclosed in the present invention is usually below 120°C. Therefore, if the glass transition temperature of the protective film is greater than 120°C, strain of the protective film is not likely to occur during the manufacturing process. As a result, when the protective film is peeled off from the protective film assembly frame with a protective film, the surface of the adhesive layer tends to become flat. In detail, the number of local height differences on the surface of the adhesive layer tends to be less than 1. Therefore, it is speculated that the number of trapped bubbles when the protective film assembly is attached to the photomask can be suppressed.

[0240] The pellicle frame, adhesive layer, and protective film of the pellicle frame with a protective film may be the same as those exemplified as the pellicle frame, adhesive layer, and protective film in the method for manufacturing the pellicle frame with an adhesive layer.

[0241] (3) Protective film assembly frame with adhesive layer

[0242] The pellicle assembly frame with an adhesive layer disclosed in the present invention comprises a pellicle assembly frame and an adhesive layer for attaching to a photomask. The adhesive layer is formed on the pellicle assembly frame. The number of local height differences of 3 μm or more on the surface of the adhesive layer is one or less.

[0243] The method for measuring "the number of local height differences of 3 μm or more" is the same as the method described in Examples.

[0244] Since the pellicle frame with an adhesive layer of the present disclosure has the above-described configuration, the number of trapped bubbles when the pellicle is attached to a photomask can be reduced.

[0245] This effect is presumed to be due to the following reasons, but the present invention is not limited thereto.

[0246] The fact that the number of local height differences of 3 μm or more on the surface of the adhesive layer is 1 or less indicates that the surface of the adhesive layer is flat. Therefore, it is estimated that the number of trapped bubbles when the pellicle assembly is attached to the photomask can be suppressed compared to the case where the number of local height differences of 3 μm or more on the surface of the adhesive layer is 2 or more.

[0247] The number of local height differences of 3 μm or more on the surface of the adhesive layer is 1 or less, and preferably 0 from the viewpoint of further reducing the number of trapped bubbles when the pellicle is attached to the photomask.

[0248] As a method for making the number of local height differences of 3 μm or more on the surface of the adhesive layer fall within the above range, for example, there is a method of manufacturing a pellicle frame with an adhesive layer by the method of manufacturing a pellicle frame with an adhesive layer disclosed in the present invention.

[0249] The pellicle frame and the adhesive layer of the pellicle frame with an adhesive layer may be the same as those exemplified as the pellicle frame and the adhesive layer in the method for manufacturing the pellicle frame with an adhesive layer.

[0250] Among them, from the viewpoint of reducing the amount of outgassing generated by the protective film assembly, the adhesive layer preferably contains at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, urethane adhesives and olefin adhesives, more preferably contains an acrylic adhesive, and even more preferably an acrylic adhesive.

[0251] (4) Protective film assembly

[0252] The pellicle assembly of the present disclosure comprises a pellicle supported by the pellicle assembly frame and the pellicle assembly frame with an adhesive layer of the present disclosure. The pellicle is supported by the pellicle assembly frame. Specifically, the pellicle is supported by the pellicle end surface of the pellicle assembly frame.

[0253] The pellicle prevents foreign matter from adhering to the surface of the photomask and allows exposure light to pass through during exposure. Foreign matter includes dust. Examples of exposure light include deep ultraviolet (DUV: Deep UltraViolet) light and EUV. EUV refers to light with a wavelength of 2 nm or more and 30 nm or less.

[0254] The pellicle covers the entire opening of one end face (the pellicle end face) of the through hole of the pellicle assembly frame. The pellicle may be directly supported by one end face of the pellicle assembly frame or may be supported via a membrane adhesive layer. The membrane adhesive layer may be a cured product of a known adhesive.

[0255] The thickness of the pellicle membrane is preferably from 1 nm to 400 nm, and more preferably from 1 nm to 70 nm in order to easily increase the transmittance under EUV exposure.

[0256] The material of the protective film is not particularly limited, and examples thereof include carbon-based materials, SiN, polysilicon, fluororesins, and the like. Carbon-based materials include carbon nanotubes (hereinafter referred to as "CNTs"). Among them, in order to easily improve the transmittance under EUV exposure, the material of the protective film preferably includes at least one selected from the group consisting of CNTs, metal silicides, and polysilicon, and more preferably includes CNTs. CNTs may be single-walled CNTs or multi-walled CNTs. The above-mentioned metal silicide is preferably any one of molybdenum nitride silicide (MoSiN) and molybdenum silicide (MoSi).

[0257] The protective film may be a non-woven fabric structure, which is formed, for example, from fiber-shaped CNTs.

[0258] The pellicle membrane may be indirectly supported by the pellicle membrane assembly frame via the pellicle membrane adhesive layer, or may be directly supported by the pellicle membrane assembly frame.

[0259] Examples of the adhesive constituting the adhesive layer for a pellicle include acrylic resin adhesives, epoxy resin adhesives, polyimide resin adhesives, silicone resin adhesives, inorganic adhesives, double-sided adhesive tapes, polyolefin adhesives, and hydrogenated styrene adhesives.

[0260] Among them, the pellicle adhesive is preferably at least one selected from the group consisting of silicone resin adhesives, acrylic resin adhesives, hydrogenated styrene adhesives, and epoxy resin adhesives from the viewpoint of ease of coating and curing.

[0261] In the present disclosure, the adhesive for a pellicle is a concept that includes not only adhesives but also tacky agents.

[0262] The thickness of the adhesive layer for a pellicle is not particularly limited. The thickness of the adhesive layer for a pellicle is, for example, 10 μm or more and 1 mm or less.

[0263] (5) Photomask with protective film assembly

[0264] The photomask with pellicle assembly of the present disclosure comprises a photomask and the pellicle assembly of the present disclosure. The pellicle assembly is attached to the photomask. The area of ​​the gap between the adhesive layer and the photomask on the surface of the adhesive layer in contact with the photomask is 0.25% or less relative to the area of ​​the adhesive layer in contact with the photomask.

[0265] The method for measuring the area of ​​the gap between the adhesive layer and the photomask is the same as the method described in Examples.

[0266] “In the surface of the adhesive layer in contact with the photomask, the area of ​​the gap between the adhesive layer and the photomask is less than 0.25% relative to the area of ​​the adhesive layer in contact with the photomask” means that there are very few trapped bubbles. The photomask with a protective film assembly disclosed in the present invention has the above-mentioned structure, so the generation of air paths can be suppressed. In addition, since there are few trapped bubbles, the bonding surface toward the photomask becomes uniform, thereby suppressing the strain of the photomask and ensuring a wide bonding area, thereby suppressing the peeling of the protective film assembly when the photomask moves during exposure.

[0267] On the surface of the adhesive layer in contact with the photomask, the area of ​​the gap between the adhesive layer and the photomask is 0.25% or less, preferably 0% to 0.10%, more preferably 0% to 0.05% of the area of ​​the adhesive layer in contact with the photomask, the lower the better.

[0268] The photomask is the original plate of the circuit pattern. The photomask has a pattern. The pellicle assembly is attached to the side of the photomask with the pattern.

[0269] The photomask may not be stacked in the order of the support substrate, the reflective layer, and the absorber layer, for example. The absorber layer absorbs a portion of the light (e.g., EUV), thereby forming a desired image on a sensing substrate (e.g., a semiconductor substrate with a photoresist film). As the reflective layer, a multilayer film of molybdenum (Mo) and silicon (Si) may be cited. The material of the absorber layer may be a material with high absorption of EUV, etc. As the material with high absorption of EUV, etc., chromium (Cr), tantalum nitride, etc. may be cited.

[0270] The photomask with a pellicle assembly disclosed herein is used in an exposure device.

[0271] The exposure device includes a light source, a photomask with a pellicle assembly of the present disclosure, and an optical system. The light source emits exposure light. The optical system guides the exposure light emitted by the light source to the photomask. The photomask with a pellicle assembly is configured in such a way that the exposure light emitted by the light source passes through the pellicle and irradiates the photomask.

[0272] The exposure device can form a fine pattern (for example, a line width of less than 32 nm) using EUV or the like. In addition, even when using EUV in which poor resolution caused by foreign matter is likely to become a problem, pattern exposure with reduced poor resolution caused by foreign matter can be performed.

[0273] The exposure light is preferably DUV or EUV. EUV has a short wavelength and is easily absorbed by gases such as oxygen or nitrogen. Therefore, exposure using EUV light is performed in a vacuum environment.

[0274] Example

[0275] Hereinafter, the present disclosure will be described in further detail using examples, but the present invention is not limited to these examples.

[0276] [1] Preparation

[0277] The materials used in Examples and Comparative Examples are as follows.

[0278] <Alkyl (meth)acrylate monomer>

[0279] EA: Ethyl acrylate (Tg: -24℃)

[0280] <Functional group-containing monomers>

[0281] ·4-HBA: 4-Hydroxybutyl acrylate

[0282] HEMA: 2-Hydroxyethyl Methacrylate

[0283] ·GMA: Glycidyl Methacrylate

[0284] <Cross-linking agent>

[0285] ・RIKACID MH-700G manufactured by Shin Nippon Rika Co., Ltd.

[0286] <Polymerization solvent>

[0287] Propyl acetate

[0288] <Polymerization initiator>

[0289] ·AIBN: 2,2'-azobisisobutyronitrile (10-hour half-life temperature: 65°C)

[0290] <Catalyst>

[0291] Amine catalyst: "U-CAT SA-102" manufactured by San-Apro Co., Ltd. (chemical formula: octanoate of (1,8-diazabicyclo-(5.4.0)undecene-7))

[0292] [2] Example 1

[0293] [2.1] Preparation process

[0294] The alkyl (meth)acrylate copolymer is prepared by a well-known method.

[0295] Specifically, a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping device and a nitrogen inlet pipe was prepared. A polymerization solvent (180 parts by mass) was added to the reaction vessel, and a mixture of EA / 4-HBA / HEMA / GMA / polymerization initiator (423.4 parts by mass) was charged at a mass ratio of 378 / 12.6 / 21 / 8.4 / 3.4. The reaction solution was reacted at 85° C. for 6 hours and further at 95° C. for 2 hours under a nitrogen atmosphere to obtain an acrylic copolymer solution (weight average molecular weight: 119,000) having a non-volatile component (copolymer) concentration of 70% by mass.

[0296] A crosslinking agent (0.28 parts by mass) and a catalyst (0.93 parts by mass) were added to the obtained acrylic copolymer solution (143 parts by mass), and the mixture was stirred and mixed to obtain a coating composition (acrylic adhesive).

[0297] like Figure 1 As shown, an anodized aluminum pellicle frame (external dimensions: 149 mm×115 mm, frame height H: 4.5 mm, frame width W: 2 mm) is prepared as the pellicle frame 11. The prepared coating composition is applied to the photomask end surface S11A of the pellicle frame 11 by a dispenser to form a precursor layer formed of the coating composition. Thus, a frame precursor is obtained.

[0298] [2.2] Drying process

[0299] The frame precursor was dried under drying conditions of 100° C. for 2 hours.

[0300] [2.3] Configuration process

[0301] A PEN protective film was prepared as the protective film 21. The PEN protective film had a two-layer structure of a base layer (material: polyethylene naphthalate) and a release layer (material: silicone-based). The thickness of the base layer was 75 μm.

[0302] A glass substrate was prepared as a flat plate, and the TIR value of the flat surface of the flat plate was 5 μm.

[0303] The protective film 21 is disposed on the surface of the precursor layer of the dried frame precursor to obtain a frame precursor with a protective film.

[0304] [2.4] Planarization process

[0305] Next, the placement method is implemented. Specifically, the precursor layer of the frame precursor with the protective film is oriented downward (in the direction of gravity), and the protective film assembly frame with the precursor layer is placed on the flat plate. The precursor layer of the frame precursor with the protective film is in contact with the flat surface of the flat plate via the protective film 21. At this time, the protective film is 1.6 g / cm 2 The pressure (load) is applied in such a way that the pressure (load) acts uniformly on the entire precursor layer of the pellicle assembly frame with the precursor layer. Thus, a first contact article is obtained.

[0306] As a heating device, an oven ("DRC623FB19A" manufactured by ADVANTEC) is prepared. The first contact article is placed in the oven. The first contact article is heated as a whole in the oven under the heating conditions of 120°C for 16 hours. Thus, the flat surface of the flat plate is transferred to the surface of the precursor layer, and the precursor layer is cured at the same time. That is, the adhesive layer 12 with a flat surface is formed by the precursor layer.

[0307] Next, the first contact object is taken out of the heating device, and the flat plate is removed from the first contact object. Thus, the pellicle assembly frame 20 with a protective film is obtained.

[0308] Next, protective film 21 was removed from pellicle frame 20 with protective film, thereby obtaining pellicle frame 10 with adhesive layer. Adhesive layer 12 composed of the adhesive composition had a thickness of 0.2 mm.

[0309] [3] Example 2 and Example 3

[0310] The pellicle frame 10 with an adhesive layer was obtained in the same manner as in Example 1 except that the temperature and time of the heating conditions in the planarization step were changed to the conditions in Table 1.

[0311] [4] Comparative Example 1

[0312] The pellicle frame 10 with an adhesive layer was obtained in the same manner as in Example 1 except that the PEN protective film was changed to a PET protective film as the protective film 21 .

[0313] The PET protective film has a two-layer structure of a base layer (material: polyethylene terephthalate) and a release layer (material: silicone-based). The thickness of the base layer is 75 μm.

[0314] [5] Measurement method

[0315] The number of local height differences on the surface S12 of the adhesive layer 12, the thickness of the adhesive layer 12, and the Tg of the protective film 21 were measured by the following method. Table 1 shows the results of the measurement of the number of local height differences on the surface S12 of the adhesive layer 12.

[0316] [5.1] Determination of the number of local height differences

[0317] The number of local height differences of the surface S12 of the adhesive layer 12 is calculated by measuring the height differences at each measurement point of the surface S12 of the adhesive layer 12 and using the measured height differences.

[0318] The height difference at each measuring point of the surface S12 of the adhesive layer 12 is measured as follows.

[0319] The protective film assembly frame 10 with an adhesive layer is placed on the platform in such a manner that the end surface S11B of the protective film assembly frame 10 with an adhesive layer is opposite to the platform. A 3D displacement meter (manufactured by Keyence Corporation, "WI5000", sensor head "WI-004") is used to measure the height of each of the 204 measurement points on the surface S12 of the adhesive layer 12 from the platform. The 204 measurement points include 4 points at the four corners of the end surface S11A for the photomask and 200 points on the four sides between the four corners. In principle, the 200 points represent the total of points set at intervals of 2.5 mm from one point in the four corners toward another point in the four corners on each side between the four corners. However, if, among the 200 points, one point in the four corners (hereinafter referred to as a "corner point") and the interval between the points adjacent to the corner point (hereinafter referred to as an "angle interval") are less than 2.5 mm, the points adjacent to the corner point are points set so that the angle interval is less than 2.5 mm. If the measurement points are not 204 points when the above-mentioned 2.5 mm interval and angle interval are used due to the different size of the pellicle assembly frame 11, the measurement points are determined by considering the 2.5 mm interval and the above-mentioned angle interval.

[0320] The least square plane calculated using the measured values ​​of the heights of 204 points is derived. The height difference between each measuring point and the least square plane is calculated. The positive and negative signs of each height difference of multiple measuring points located on the opposite side of the platform side relative to the least square plane are set to "positive (+)". The positive and negative signs of each height difference of multiple measuring points located on the platform side relative to the least square plane are set to "negative (-)". The height difference with positive and negative signs calculated in this way is used as the height difference of each measuring point on the surface S12 of the adhesive layer 12.

[0321] Next, based on the height differences of each measurement point, the Δ height differences between adjacent measurement points of the 204 points are calculated. The Δ height difference represents a value obtained by subtracting the height difference of a point adjacent to the arbitrary point in the clockwise direction from the height difference of an arbitrary point among the 204 points.

[0322] In principle, the number of local height differences indicates the number of Δ height differences (referred to as "Δ height differences (large)") whose absolute value of Δ height differences is greater than 3μm among the 204 Δ height differences. However, when the 204 Δ height differences are arranged in a row according to the arrangement of the 204 measurement points, if the Δ height difference (large) continues for more than 2 consecutive times, the number of consecutive multiple Δ height differences (large) is counted as 1 local height difference. For example, when the Δ height differences arranged in a row based on the above method are 2μm, -4μm, 1μm, 3μm, and 1μm, the number of local height differences is 2. When the Δ height differences arranged in a row are 2μm, -4μm, 5μm, 3μm, and 1μm, the number of local height differences is 1.

[0323] [5.2] Method for measuring the thickness of the adhesive layer

[0324] The thickness of the adhesive layer was determined as follows.

[0325] The pellicle assembly frame is placed on the platform in such a manner that the pellicle end face of the pellicle assembly frame with the adhesive layer faces the platform. The height of the 6 measurement points on any one side between the four corners of the photomask end face is measured from the platform using a 3D displacement meter (manufactured by KEYENCE Corporation, "WI5000", sensor head "WI-004"). In the width direction of the pellicle assembly frame (the short side direction of one side of the pellicle assembly frame), 4 of the 6 measurement points are points coated with the adhesive layer, and 2 of the 6 measurement points are points not coated with the adhesive layer.

[0326] In this embodiment, the adhesive layer is formed only in the center of each side between the four corners of the end face of the photomask, and is not formed on the edge of each side between the four corners on the through-hole side of the pellicle assembly frame and the edge on the side opposite to the through-hole side of the pellicle assembly frame. Therefore, in this embodiment, the four points located in the center of the width direction of the pellicle assembly among the six measurement points are set as the positions where the adhesive layer is formed on the end face of the photomask. The remaining two points located at the two edges in the width direction of the pellicle assembly among the six measurement points are set as the positions where the adhesive layer is not formed on the end face of the photomask.

[0327] Using the measured values ​​of the heights of the six points, calculate the height difference between the highest point (the point where the adhesive layer is the thickest) among the four points coated with the adhesive layer and the lowest point among the two points not coated with the adhesive layer. For this calculation method, the same consideration method as that for each measurement point on the surface S12 of the above-mentioned adhesive layer 12 (every 2.5 mm interval and angular interval) is used to measure the length direction of the protective film assembly (the long side direction of one side of the protective film assembly frame). For the remaining three sides between the four corners of the end face of the photomask, the height differences are also calculated in the same way. The average value of all the height differences of the four sides calculated in this way is set as the thickness of the adhesive layer.

[0328] [5.3] Method for measuring the TIR value of the flat surface of a flat plate

[0329] The flat plate was placed on the platform in such a manner that the surface opposite to the flat surface of the flat plate was facing the platform. A 3D displacement meter (manufactured by KEYENCE Corporation, "WI5000", sensor head "WI-004") was used to measure the height of each of the 204 measurement points on the flat surface of the flat plate from the platform. The 204 measurement points were measured in the same way as the measurement points for measuring the height of the surface S12 of the adhesive layer 12 described above.

[0330] The least square plane calculated using the measured values ​​of the heights of 204 points is derived. The height difference between each measuring point and the least square plane is calculated. The positive and negative signs of each height difference of multiple measuring points located on the opposite side of the platform side relative to the least square plane are set to "positive (+)". The positive and negative signs of each height difference of multiple measuring points located on the platform side relative to the least square plane are set to "negative (-)". The height difference with positive and negative signs calculated in this way is used as the height difference of each measuring point on the surface S12 of the adhesive layer 12. The difference between the maximum height difference and the minimum height difference in each measuring point is used as the TIR value.

[0331] [6] Evaluation Method

[0332] The number of gas paths, the number of trapped bubbles, the ratio of trapped bubbles, and the area of ​​trapped bubbles were measured by the following method. The measurement results of the number of gas paths, the number of trapped bubbles, the ratio of trapped bubbles, and the area of ​​trapped bubbles are shown in Table 1.

[0333] [6.1] Number of gas paths and number of trapped bubbles

[0334] A transparent quartz substrate is prepared. The transparent quartz substrate has a first main surface and a second main surface opposite to the first main surface.

[0335] The pellicle frame 10 with an adhesive layer is placed on the first main surface of the transparent quartz substrate. The adhesive layer 12 of the pellicle frame 10 with an adhesive layer is brought into contact with the first main surface of the transparent quartz substrate. Thus, a second contact article is obtained.

[0336] A glass substrate (model: "HOYA 6025 quartz substrate", mass: 320 g) was placed on the pellicle end surface S11B of the pellicle assembly frame 11, and a weight (mass: 2 kg) was placed on the glass substrate. After 20 seconds from the time the weight was placed on the glass substrate, the glass substrate and the weight were removed from the pellicle end surface S11B of the pellicle assembly frame 11.

[0337] The second contact article was placed on the stage of an optical microscope ("VHX-6000" manufactured by KEYENCE Corporation) such that the second principal surface of the transparent quartz substrate of the second contact article was on the upper side (the side opposite to the gravity direction).

[0338] The entire surface of the contact surface between the adhesive layer 12 of the pellicle frame 10 with an adhesive layer and the first main surface of the quartz substrate was observed through the transparent quartz substrate using an optical microscope. The observation magnification of the optical microscope was 20 times.

[0339] The number of gas paths and the number of retained bubbles in the contact surface between the adhesive layer 12 and the first main surface of the transparent quartz substrate were counted.

[0340] The allowable range of the number of gas paths is 0. The allowable range of the number of trapped bubbles is 10 or less.

[0341] [6.2] Retention bubble area

[0342] Using the software "VHX" included with the optical microscope, the total area of ​​the plurality of trapped bubbles existing in the contact surface between the adhesive layer 12 and the first main surface of the quartz substrate and the total area of ​​the contact surface between the adhesive layer 12 and the first main surface of the quartz substrate were measured.

[0343] The total area of ​​a plurality of retained bubbles existing in the contact surface between the adhesive layer 12 and the first main surface of the quartz substrate is defined as a “retained bubble area”.

[0344] The ratio of the retained bubble area to the total area of ​​the contact surface between the adhesive layer 12 and the first main surface of the quartz substrate is referred to as a “retained bubble ratio”.

[0345] The permissible range of the retained bubble ratio is 0.25% or less.

[0346] [Table 1]

[0347]

[0348] In Table 1, "acrylic" means an acrylic adhesive. "Tg" means a glass transition temperature. "Tg of a protective film" means a glass transition temperature of a base material layer included in the protective film.

[0349] The manufacturing method of the protective film assembly frame with an adhesive layer of Examples 1 to 3 includes step A (i.e., preparation step), step B (i.e., configuration step) and step C (i.e., planarization step), and the glass transition temperature (Tg) of the protective film 21 is higher than the heating temperature of the planarization step.

[0350] Therefore, the number of retained bubbles in Examples 1 to 3 is 3 or less. From these results, it can be seen that the methods of manufacturing the pellicle frame with an adhesive layer in Examples 1 to 3 can suppress the number of retained bubbles when attaching the pellicle to the photomask.

[0351] Pellicle frame 20 with protective film of Comparative Example 1 includes pellicle frame 11, adhesive layer 12, and protective film 21. However, the glass transition temperature of protective film 21 of Comparative Example 1 does not exceed 120°C. Therefore, the number of retained bubbles of Comparative Example 1 is 13.

[0352] The pellicle assembly frame 20 with a protective film of Examples 1 to 3 includes a pellicle assembly frame 11, an adhesive layer 12, and a protective film 21. The glass transition temperature of the protective film 21 of Examples 1 to 3 is greater than 120° C. Therefore, the number of trapped bubbles in Examples 1 to 3 is 3 or less. From this result, it can be seen that the pellicle assembly frame 20 with a protective film of Examples 1 to 3 can suppress the number of trapped bubbles when the pellicle assembly is attached to the photomask.

[0353] Pellicle frame 10 with adhesive layer of Comparative Example 1 includes pellicle frame 11 and adhesive layer 12. However, the number of local height differences of 3 μm or more on surface S12 of adhesive layer 12 of Comparative Example 1 is not less than 1. Therefore, the number of trapped bubbles in Comparative Example 1 is 13.

[0354] The pellicle assembly frame 10 with an adhesive layer of Examples 1 to 3 includes a pellicle assembly frame 11 and an adhesive layer 12. The number of local height differences of 3 μm or more in the surface S12 of the adhesive layer 12 of Examples 1 to 3 is 0. When the number of local height differences of 3 μm or more in the surface S12 of the adhesive layer 12 is 1 or less, it means that the surface S12 of the adhesive layer 12 is flat. According to this result, the pellicle assembly frame 10 with an adhesive layer of Examples 1 to 3 can suppress the number of trapped bubbles when the pellicle assembly is attached to the photomask.

[0355] The disclosed contents of Japanese Patent Application No. 2022-047178 filed on March 23, 2022 are incorporated into this specification by reference in their entirety.

[0356] All documents, patent applications, and technical standards described in this specification are incorporated herein by reference to the same extent as if each document, patent application, and technical standard was specifically and individually described as being incorporated by reference.

Claims

1. A method for manufacturing a pellicle assembly frame with an adhesive layer, the pellicle assembly frame with an adhesive layer comprising a pellicle assembly frame and an adhesive layer formed on the pellicle assembly frame and used for attaching to a photomask, The manufacturing method has the following features: Step A, preparing a frame precursor, the frame precursor comprising the pellicle assembly frame and a precursor layer formed on the pellicle assembly frame and serving as a precursor of the adhesive layer; Step B, disposing a protective film on the surface of the precursor layer to form a frame precursor with a protective film; as well as Step C, subjecting the frame precursor with the protective film to a heat treatment to form the adhesive layer with a flat surface from the precursor layer, The glass transition temperature of the protective film is higher than the heating temperature in the step C. 2 . The method for manufacturing a pellicle assembly frame with an adhesive layer according to claim 1 , wherein the protective film has a glass transition temperature greater than 120° C. 3 . The method for manufacturing a pellicle frame with an adhesive layer according to claim 1 , wherein in the step C, the heat treatment is performed at 80° C. or higher and for 2 hours or longer.

4. The method for manufacturing a pellicle assembly frame with an adhesive layer according to claim 1 or 2, wherein the adhesive layer comprises at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, urethane adhesives, and olefin adhesives.

5. A protective film assembly frame with a protective film, comprising: Protective film assembly frame, an adhesive layer formed on the pellicle frame and used for attaching to the photomask, and a protective film attached to the surface of the adhesive layer, The glass transition temperature of the protective film is greater than 120°C.

6. A protective film assembly frame with an adhesive layer, comprising: Protective film assembly frame, and an adhesive layer formed on the pellicle assembly frame and used for attaching to the photomask, The number of local height differences of 3 μm or more on the surface of the adhesive layer is one or less. 7 . The pellicle assembly frame with an adhesive layer according to claim 6 , wherein the adhesive layer comprises at least one selected from the group consisting of acrylic adhesives, silicone adhesives, styrene butadiene adhesives, urethane adhesives, and olefin adhesives.

8. A protective membrane assembly, comprising: A pellicle supported by a pellicle assembly frame, and The protective film assembly frame with an adhesive layer according to claim 6 or 7, The protective film includes at least one selected from the group consisting of carbon nanotubes, metal silicide, and polysilicon.

9. A photomask with a pellicle assembly, comprising: Photomask, and The pellicle assembly according to claim 8 attached to the photomask, On the surface of the adhesive layer in contact with the photomask, an area of ​​a gap between the adhesive layer and the photomask is 0.25% or less relative to an area of ​​the adhesive layer in contact with the photomask.