Composition for forming resist underlayer film having fluorene skeleton
By using a resist underlying film composition containing a fluorene structure in EB or EUV lithography, combining a crosslinker and a curing catalyst, the problem of resist patterns LWR and LER is solved, significantly improving pattern consistency and semiconductor components performance.
Patent Information
- Application Number
- CN202380028506.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-23
- Publication Date
- 2024-11-01
AI Technical Summary
In EB or EUV lithography, the LWR (line width unevenness) and LER (side wall roughness) of the resist pattern are serious problems, affecting component performance, and it is difficult to effectively improve the prior art.
Using a resist underlayer film composition containing a fluorene structure and a solvent, a resist underlayer film with excellent properties is formed by combining a crosslinking agent and a curing catalyst to improve LWR and LER.
The LWR of the resist pattern in EB or EUV lithography is significantly improved, the shape consistency and performance of the pattern are improved, and the manufacturing quality of semiconductor components is enhanced.
Smart Images

Figure BDA0005048857290000021 
Figure BDA0005048857290000022 
Figure BDA0005048857290000031
Abstract
Description
Technical Field
[0001] The present invention relates to a composition for forming a resist underlayer film for EB (electron beam) or EUV (extreme ultraviolet) lithography, a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for manufacturing a semiconductor element, and a method for patterning. Background Art
[0002] In semiconductor devices such as LSI (semiconductor integrated circuit), it is necessary to form fine patterns as the degree of integration increases, and the minimum pattern size has reached 100 nm or less in recent years.
[0003] The formation of fine patterns in such semiconductor devices has been achieved by shortening the wavelength of the light source of the exposure device and improving the resist material. Currently, the liquid immersion exposure method is implemented, which uses ArF (argon fluoride) excimer laser with a wavelength of 193nm, which is deep ultraviolet light, as the light source and performs exposure through water. Regarding the resist material, various ArF-compatible resist materials based on acrylic resin have been developed.
[0004] In addition, as a next-generation exposure technology, research has been conducted on the EB exposure method using an electron beam (EB: Electron beam) or the EUV (extreme ultraviolet) exposure method using soft X-rays with a wavelength of 13.5nm as a light source. The pattern size has been reduced to less than 30nm and is further developing towards miniaturization.
[0005] However, as the pattern size becomes smaller, the roughness of the sidewalls of the resist pattern (LER; Line edge roughness) and the unevenness of the width of the resist pattern (LWR: Line width roughness) become more serious, and there is an increasing concern that they will have an adverse effect on device performance. Although studies have been conducted to suppress these by optimizing exposure equipment, resist materials, and process conditions, sufficient results have not been obtained. In addition, LWR is related to LER, and LER can also be improved by improving LWR.
[0006] As a method for solving the above-mentioned problems, there is a document that discloses a method for improving the LWR and LER by treating the resist pattern with an aqueous solution containing a specific ionic surfactant in the cleaning step after the development process to suppress the defects caused by the development process (defects such as the generation of residues or pattern collapse), while dissolving the unevenness of the resist pattern (refer to Patent Document 1).
[0007] [Prior art literature]
[0008] [Patent Document]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 2007-213013 Summary of the invention
[0010] [Problems to be solved by the invention]
[0011] The object of the present invention is to provide a composition for forming a resist underlayer film for EB or EUV lithography, a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for manufacturing a semiconductor element, and a pattern forming method, which can improve the LWR of a resist pattern in EB or EUV lithography.
[0012] [Methods for solving the problem]
[0013] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved, and have completed the present invention having the following gist.
[0014] That is, the present invention includes the following aspects.
[0015] [1]. A composition for forming a resist underlayer film for EB or EUV lithography, comprising: a polymer containing a fluorene structure and a solvent.
[0016] [2] The composition for forming a resist underlayer film for EB or EUV lithography according to [1], wherein the polymer comprises a partial structure represented by the following formula (1),
[0017] [Chemistry 1]
[0018]
[0019] In formula (1), X 1 represents a divalent organic group having a fluorene structure,
[0020] Z 1 and Z 2 Each independently represents a single bond, -O-, -C(=O)O- or -OC m H 2m -O-, m represents an integer from 1 to 6,
[0021] A 1 , A 2 , A 3 , A 4 , A 5 and A 6 each independently represents a hydrogen atom, a methyl group or an ethyl group,
[0022] * indicates a connection key.
[0023] [3] The composition for forming a resist underlayer film for EB or EUV lithography as described in [2], wherein X in the formula (1) 1 represents a divalent organic group represented by the following formula (1-A) or (1-B),
[0024] [Chemistry 2]
[0025]
[0026] In formula (1-A) and (1-B), R 1 , R 2 , R 5 and R 6 each independently represents a hydroxyl group, an acyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms, and the acyl group, alkoxy group, alkoxycarbonyl group, alkyl group, aryl group, alkenyl group, and alkynyl group may have one or more groups selected from an amino group, a nitro group, a cyano group, a hydroxyl group, a glycidyl group, and a carboxyl group,
[0027] R 3 and R 4 each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms,
[0028] m1 and m2 each independently represent an integer from 0 to 4,
[0029] n1 and n2 each independently represent 0 or 1,
[0030] When n1 is 0, o1 represents an integer from 0 to 4; when n1 is 1, o1 represents an integer from 0 to 6.
[0031] When n2 is 0, o2 represents an integer from 0 to 4; when n2 is 1, o2 represents an integer from 0 to 6.
[0032] R 1 ~R 6 When there are multiple R 1 ~R 6 They may be the same or different.
[0033] One R 5 With an R 6 can form an -O- bond together,
[0034] * indicates a connection key.
[0035] [4] The composition for forming a resist underlayer film for EB or EUV lithography according to [2] or [3], wherein the polymer further comprises at least one of a partial structure represented by the following formula (2-1) and a partial structure represented by the following formula (2-2),
[0036] [Chemistry 3]
[0037]
[0038] In formula (2-1), X 11 represents a group represented by any one of the following formulae (2-1-1) to (2-1-3),
[0039] Z 11 and Z 12 Each independently represents a single bond or a divalent group represented by the following formula (2-1-4),
[0040] In formula (2-2), Q 1 represents a single bond or a divalent organic group, p1 and p2 each independently represent 0 or 1,
[0041] [Chemistry 4]
[0042]
[0043] In formulas (2-1-1) to (2-1-3), R 11 ~R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group, or a phenyl group, wherein the phenyl group may be substituted with at least one monovalent group selected from an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms, and R 11 With R 12 can be combined to form a ring with 3 to 6 carbon atoms, R 13 With R 14 can be bonded to each other to form a ring having 3 to 6 carbon atoms, * represents a bond, *1 represents a bond bonded to a carbon atom, and *2 represents a bond bonded to a nitrogen atom,
[0044] [Chemistry 5]
[0045]
[0046] In the formula (2-1-4), m1 represents an integer of 1 to 4, m2 represents 0 or 1, *3 represents a bond to a nitrogen atom, and *4 represents a bond.
[0047] [5] The resist underlayer film forming composition for EB or EUV lithography according to any one of [1] to [4], further comprising a crosslinking agent.
[0048] [6] The resist underlayer film forming composition for EB or EUV lithography according to any one of [1] to [5], further comprising a curing catalyst.
[0049] [7] The composition for forming a resist underlayer film for EB or EUV lithography according to any one of [1] to [6], which is used for forming a resist underlayer film for EB or EUV lithography having a film thickness of 10 nm or less.
[0050] [8] A resist underlayer film for EB or EUV lithography, which is a cured product of the resist underlayer film-forming composition for EB or EUV lithography according to any one of [1] to [7].
[0051] [9]. A semiconductor processing substrate comprising:
[0052] A semiconductor substrate and the resist underlayer film for EB or EUV lithography described in [8].
[0053]
[10] . A method for manufacturing a semiconductor device, comprising:
[0054] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography described in any one of [1] to [7]; and
[0055] A step of forming a resist film on the resist underlayer film.
[0056]
[11] . A pattern forming method comprising:
[0057] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography described in any one of [1] to [7];
[0058] forming a resist film on the resist underlayer film;
[0059] irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; and
[0060] A step of etching the resist underlayer film using the resist pattern as a mask.
[0061] [Effects of the invention]
[0062] According to the present invention, a composition for forming a resist underlayer film for EB or EUV lithography, a resist underlayer film for EB or EUV lithography, a substrate for semiconductor processing, a method for manufacturing a semiconductor element, and a pattern forming method can be provided, which can improve the LWR of a resist pattern in EB or EUV lithography. DETAILED DESCRIPTION
[0063] The present inventors have studied methods for improving LWR by methods other than the cleaning step and have found that a resist underlayer film formed from a resist underlayer film-forming composition containing a polymer having a fluorene structure is effective in improving the LWR of a resist pattern in EB or EUV lithography.
[0064] (Composition for forming a resist underlayer film for EB or EUV lithography)
[0065] The resist underlayer film-forming composition for EB or EUV lithography of the present invention (hereinafter sometimes simply referred to as “resist underlayer film-forming composition”) contains a polymer including a fluorene structure and a solvent.
[0066] <Polymer containing fluorene structure>
[0067] The polymer including a fluorene structure is not particularly limited as long as it includes a fluorene structure.
[0068] The fluorene structure refers to the following structure.
[0069]
Chemistry 6
[0070]
[0071] The polymer containing a fluorene structure preferably contains a partial structure represented by the following formula (1) from the viewpoint of favorably obtaining the effects of the present invention.
[0072]
Chemistry 7
[0073]
[0074] (In formula (1), X 1 represents a divalent organic group having a fluorene structure,
[0075] Z 1 and Z 2 Each independently represents a single bond, -O-, -C(=O)O- or -OC m H 2m -O- (m represents an integer from 1 to 6),
[0076] A 1 , A 2 , A 3 , A 4 , A 5 and A 6 each independently represents a hydrogen atom, a methyl group or an ethyl group,
[0077] * indicates a connection key)
[0078] X in formula (1) 1From the viewpoint of facilitating the effects of the present invention, it is preferably a divalent organic group represented by the following formula (1-A) or (1-B).
[0079]
Chemistry 8
[0080]
[0081] (In formula (1-A) and (1-B), R 1 , R 2 , R 5 and R 6 each independently represents a hydroxyl group, an acyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms, wherein the acyl group, alkoxy group, alkoxycarbonyl group, alkyl group, aryl group, alkenyl group, and alkynyl group may have one or more groups selected from an amino group, a nitro group, a cyano group, a hydroxyl group, a glycidyl group, and a carboxyl group,
[0082] R 3 and R 4 each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms,
[0083] m1 and m2 each independently represent an integer of 0 to 4,
[0084] n1 and n2 each independently represent 0 or 1,
[0085] When n1 is 0, o1 represents an integer from 0 to 4; when n1 is 1, o1 represents an integer from 0 to 6.
[0086] When n2 is 0, o2 represents an integer from 0 to 4; when n2 is 1, o2 represents an integer from 0 to 6.
[0087] R 1 ~R 6 When there are multiple R 1 ~R 6 They may be the same or different.
[0088] One R 5 With an R 6 can form an -O- bond together,
[0089] * indicates a connection key).
[0090] R 1 , R 2 , R 5 and R 6Each independently represents a hydroxyl group, an acyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms. However, the acyl group, alkoxy group, alkoxycarbonyl group, alkyl group, aryl group, alkenyl group, and alkynyl group may have one or more groups selected from an amino group, a nitro group, a cyano group, a hydroxyl group, a glycidyl group, and a carboxyl group.
[0091] Examples of the acyl group having 1 to 6 carbon atoms include formyl, acetyl, propionyl, butyryl, isobutyryl, valeryl, and isovaleryl.
[0092] Examples of the alkoxy group having 1 to 6 carbon atoms include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, sec-butoxy, n-pentoxy, neopentoxy, n-hexyloxy, isohexyloxy and 3-methylpentyloxy.
[0093] Examples of the alkoxycarbonyl group having 1 to 6 carbon atoms include methoxycarbonyl, ethoxycarbonyl, n-propoxycarbonyl, isopropoxycarbonyl, n-butoxycarbonyl, isobutoxycarbonyl, sec-butoxycarbonyl, tert-butoxycarbonyl, n-pentyloxycarbonyl and n-hexyloxycarbonyl.
[0094] The alkyl group having 1 to 10 carbon atoms includes, for example, straight-chain alkyl groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl; branched-chain alkyl groups such as isopropyl, sec-butyl, tert-butyl, isopentyl, neopentyl, 1-methylpentyl, isohexyl, 1-propylbutyl, 2-ethylhexyl, and isononyl; and cyclic alkyl groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, p-tert-butylcyclohexyl, and adamantyl.
[0095] Examples of the aryl group having 6 to 20 carbon atoms include phenyl, naphthyl, biphenyl, anthracenyl, phenanthrenyl, and pyrenyl.
[0096] Examples of the alkenyl group having 2 to 20 carbon atoms include ethenyl, propenyl, butenyl and the like.
[0097] Examples of the alkynyl group having 2 to 10 carbon atoms include ethynyl, propynyl, butynyl, pentynyl, hexynyl, heptynyl, octynyl, nonynyl, decynyl, butadiynyl, pentadiynyl, hexadiynyl, heptadiynyl, octadiynyl, nonadiynyl and decadiynyl.
[0098] R 3 and R 4 Each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms.
[0099] Examples of the alkylene group having 1 to 10 carbon atoms include methylene, ethylene, 1,3-propylene, 1-methylethylene, 1,4-butylene, 1-ethylethylene, 1-methylpropylene, 2-methylpropylene, 1,5-pentylene, 1-methylbutylene, 2-methylbutylene, 1,1-dimethylpropylene, 1,2-dimethylpropylene, 1-ethylpropylene, 2-ethylpropylene, 1,6-hexylene, 1,4-cyclohexylene, 1,8-octylene, 2-ethyloctylene, 1,9-nonylene, and 1,10-decylene.
[0100] Z 1 and Z 2 Among them -OC m H 2m -C in -O m H 2m The - group may be straight chain or branched.
[0101] In formula (1), “*-Z 1 -X 1 -Z 2 -*", the following structures can be listed.
[0102]
Chemistry 9
[0103]
[0104]
Chemistry 10
[0105]
[0106]
Chemistry 11
[0107]
[0108] In the above structure, * represents a connecting bond.
[0109] The polymer including a fluorene structure may further include at least one of the partial structure represented by the following formula (2-1) and the partial structure represented by the following formula (2-2).
[0110]
Chemistry 12
[0111]
[0112] (In formula (2-1), X 11 represents a group represented by any one of the following formulae (2-1-1) to (2-1-3),
[0113] Z 11 and Z 12 Each independently represents a single bond or a divalent group represented by the following formula (2-1-4),
[0114] In formula (2-2), Q 1 represents a single bond or a divalent organic group, p1 and p2 each independently represent 0 or 1,
[0115] * indicates a connection key)
[0116]
Chemistry 13
[0117]
[0118] (In formulas (2-1-1) to (2-1-3), R 11 ~R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group, or a phenyl group, wherein the phenyl group may have at least one monovalent substituent selected from an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms, and R 11 With R 12 can be combined to form a ring with 3 to 6 carbon atoms, R 13 With R 14 They can be bonded to form a ring with 3 to 6 carbon atoms, * represents a bond, *1 represents a bond bonded to a carbon atom, and *2 represents a bond bonded to a nitrogen atom)
[0119]
Chemistry 14
[0120]
[0121] (In formula (2-1-4), m1 represents an integer of 1 to 4, m2 represents 0 or 1, *3 represents a bond to the nitrogen atom, and *4 represents a bond)
[0122] Specific examples of the alkyl group having 1 to 10 carbon atoms include, for example, in formulas (1-A) and (1-B), R 1 , R 2 , R 5 and R 6 The alkyl group is listed in the description.
[0123] The alkenyl group having 2 to 10 carbon atoms includes, for example, in formula (1-A) and (1-B), R 1 , R 2 , R 5 and R 6 The alkenyl group is listed in the description.
[0124] The alkynyl group having 2 to 10 carbon atoms includes, for example, in formula (1-A) and (1-B), R 1 , R2 , R 5 and R 6 The alkynyl groups listed in the description are:
[0125] Q 1 There are no particular limitations on the divalent organic group as long as it is a divalent organic group, and examples thereof include divalent organic groups having 1 to 20 carbon atoms. Examples of the divalent organic group having 1 to 10 carbon atoms include alkylene groups having 1 to 10 carbon atoms which may be interrupted by oxygen atoms or sulfur atoms.
[0126] Examples of the alkylene group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom include the alkylene group represented by the following (Q1-1).
[0127]
Chemistry 15
[0128]
[0129] (In formula (Q1-1), Q 11 and Q 12 Each independently represents a single bond, an oxygen atom or a sulfur atom, k, m and n each independently represent an integer of 0 to 10, and k+m+n represents an integer of 1 to 10, but when k is 0, Q 11 represents a single bond, when n is 0, Q 12 Indicates a single key)
[0130] When k, m and n are 1 or more respectively, -C k H 2k -、-C m H 2m -and-C n H 2n - represents an alkylene group. The alkylene group may be a straight chain or a branched chain.
[0131] Q 1 It may be a group represented by the following formula (T).
[0132]
Chemistry 16
[0133]
[0134] (In the formula (T), T represents a single bond, an oxygen atom, a sulfur atom, a carbonyl group, or an alkylene group having 1 to 10 carbon atoms which may have a substituent,
[0135] R 22 and R 23 each independently represents an alkyl group having 1 to 10 carbon atoms which may have a substituent,
[0136] n12 and n13 each independently represent an integer of 0 to 4,
[0137] R 22When there are two or more of them, two or more Rs 22 may be the same or different,
[0138] R 23 When there are two or more of them, two or more Rs 23 may be the same or different,
[0139] * represents a linking bond)
[0140] Examples of the substituent of the alkylene group having 1 to 10 carbon atoms which may have a substituent in T of formula (T) include a fluorine atom. The number of substituents in the alkylene group having 1 to 10 carbon atoms may be one or two or more.
[0141] R in formula (T) 22 and R 23 Examples of the substituent of the alkyl group having 1 to 10 carbon atoms which may have a substituent include a fluorine atom. The number of substituents in the alkyl group having 1 to 10 carbon atoms may be one or two or more.
[0142] For formula (2-1), the following structures may be cited, for example.
[0143]
Chemical formula 17
[0144]
[0145]
Chemical formula 18
[0146]
[0147]
Chemical formula 19
[0148]
[0149]
Chemical formula 20
[0150]
[0151]
Chemical formula 21
[0152]
[0153] In the above structures, * represents a linking bond.
[0154] Q in formula (2-2) 1 may be the following structures, for example.
[0155]
Chemical formula 22
[0156]
[0157]
[0158] In the above structures, * represents a linking bond.
[0159] The polymer including the fluorene structure may further have an aliphatic ring at the terminal whose carbon-carbon bond may be interrupted by a heteroatom. The aliphatic ring may have a substituent.
[0160] The polymer containing a fluorene structure is, for example, a linear polymer. Among the linear polymers containing a fluorene structure, it is preferred that the polymers have an aliphatic ring at both ends.
[0161] Examples of the substituent on the aliphatic ring which may have a substituent and whose carbon-carbon bond may be interrupted by a heteroatom include a hydroxyl group, a carboxyl group, an alkyl group having 1 to 6 carbon atoms, an acyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, and an alkoxycarbonyl group having 2 to 6 carbon atoms.
[0162] Examples of the number of members of the aliphatic ring include a 3-membered ring to a 10-membered ring.
[0163] The aliphatic ring may be monocyclic or polycyclic.
[0164] The aliphatic ring may be a saturated aliphatic ring or an unsaturated aliphatic ring.
[0165] The total number of carbon atoms in the aliphatic ring which may have a substituent and in which the carbon-carbon bond may be interrupted by a heteroatom may be 6 to 15, for example.
[0166] When the aliphatic ring in which the carbon-carbon bond of the polymer including the fluorene structure may be interrupted by a heteroatom is represented by a monovalent organic group, for example, it can be represented by the following formula (Z).
[0167]
Chemistry 23
[0168]
[0169] (In the formula (Z), Z represents a monovalent organic group obtained by removing one hydrogen atom from an aliphatic ring which may have a substituent and whose carbon-carbon bond may be interrupted by a heteroatom, and * represents a connecting bond)
[0170] Examples of Z in formula (Z) include the following structures.
[0171]
Chemistry 24
[0172]
[0173]
Chemistry 25
[0174]
[0175]
Chemistry 26
[0176]
[0177] In the above structure, * represents a connecting bond.
[0178] The molecular weight of the polymer including a fluorene structure is not particularly limited, but the weight average molecular weight measured by gel permeation chromatography (hereinafter sometimes referred to as GPC) is preferably 1,500 to 100,000, more preferably 2,000 to 50,000.
[0179] <<Method for producing a polymer containing a fluorene structure>>
[0180] The polymer including a fluorene structure can be produced using, for example, a monomer including a fluorene structure.
[0181] The method for producing the polymer including a fluorene structure is not particularly limited, and examples thereof include the following methods (i) to (vi).
[0182] (i): A method of reacting a dihydroxy compound represented by the following formula (A1-1) with a diepoxy compound having two epoxy groups.
[0183] (ii): A method of reacting a dihydroxy compound represented by the following formula (A1-1), a diepoxy compound having two epoxy groups, and a monocarboxyl compound having one carboxyl group.
[0184] (iii): A method of reacting a diepoxy compound represented by the following formula (A1-2) with a dicarboxyl compound having two carboxyl groups.
[0185] (iv): A method of reacting a diepoxy compound represented by the following formula (A1-2) with a dicarboxyl compound having two carboxyl groups and a monocarboxyl compound having one carboxyl group.
[0186] (v): A method of reacting a diepoxy compound represented by the following formula (A1-2) with a dihydroxy compound having two hydroxyl groups that can react with an epoxy group.
[0187] (vi): A method of reacting a diepoxy compound represented by the following formula (A1-2), a dihydroxy compound having two hydroxyl groups reactive with an epoxy group, and a monocarboxyl compound having one carboxyl group.
[0188] Furthermore, in (i) and (ii), a dihydroxy compound having two hydroxyl groups other than the dihydroxy compound represented by formula (A1-1) may be used in combination.
[0189] In addition, in (i) and (ii), a dicarboxyl compound having two carboxyl groups may be used in combination.
[0190] In (iii) and (iv), a diepoxy compound having two epoxy groups other than the diepoxy compound represented by formula (A1-2) may be used in combination.
[0191] In addition, in (iii) and (iv), a dihydroxy compound having two hydroxyl groups can also be used in combination.
[0192] In (v) and (vi), a diepoxy compound having two epoxy groups other than the diepoxy compound represented by the formula (A1-2) can also be used in combination.
[0193] In addition, in (v) and (vi), a dicarboxylic acid compound having two carboxyl groups can also be used in combination.
[0194] By using a monocarboxylic acid compound, the residue after removing the carboxyl group from the monocarboxylic acid compound can be introduced into the terminal of the polymer.
[0195] When producing the polymer, the hydroxyl group in the reaction is preferably a phenolic hydroxyl group. The phenolic hydroxyl group means a hydroxyl group directly bonded to an aromatic hydrocarbon ring. Examples of the aromatic hydrocarbon ring include a benzene ring, a naphthalene ring, and an anthracene ring.
[0196] In the polymerization reaction, a catalyst can also be used to promote the reaction. The catalyst is, for example, tetrabutylammonium bromide , ethyltriphenylammonium bromide such quaternary salts, and quaternary ammonium salts such as benzyltriethylammonium chloride. The amount of the catalyst used can be appropriately selected within the range of 0.1 to 10% by mass based on the total mass of the polymer raw materials used in the reaction. The temperature and time of the polymerization reaction can be selected from the most suitable conditions in the range of, for example, 80 to 160 °C and 2 to 50 hours.
[0197]
Chemical formula 27
[0198] HO-Z 1 -X 1 -Z 2 -OH (A1-1)
[0199]
[0200] (In the formula (A1-1), X 1 , Z 1 and Z 2 are respectively the same as X 1 , Z 1 and Z 2 in the formula (1) in meaning,
[0201] In the formula (A1-2), X 1 , Z 1 and Z 2 are respectively the same as X 1 , Z 1 and Z 2 in the formula (1) in meaning, and A x each independently represents a hydrogen atom, a methyl group or an ethyl group)
[0202] In formula (A1-1), X 1 preferably represents a divalent organic group represented by formula (1-A) or (1-B).
[0203] In formula (A1-1), Z 1 and Z 2 are preferably single bonds.
[0204] Examples of the compound represented by formula (A1-1) include the following compounds.
[0205]
Chemical formula 28
[0206]
[0207]
Chemical formula 29
[0208]
[0209] Examples of the compound represented by formula (A1-2) include the following compounds.
[0210]
Chemical formula 30
[0211]
[0212]
Chemical formula 31
[0213]
[0214] Examples of the diepoxide compound include the compound represented by the following formula (B1).
[0215]
Chemical formula 32
[0216]
[0217] (In formula (B1), X 11 , Z 11 and Z 12 have the same meanings as X 11 , Z 11 and Z 12 in formula (2-1), respectively, and A y each independently represents a hydrogen atom, a methyl group or an ethyl group)
[0218] Examples of the compound represented by formula (B1) include the following compounds.
[0219]
Chemical formula 33
[0220]
[0221]
Chemical formula 34
[0222]
[0223]
Chemical 35
[0224]
[0225]
Chemical 36
[0226]
[0227]
Chemical 37
[0228]
[0229]
Chemical 38
[0230]
[0231] Examples of the diepoxide compound having two epoxy groups other than the diepoxide compound represented by the formula (A1-2) include the following diepoxide compounds.
[0232]
Chemical 39
[0233]
[0234]
Chemical 40
[0235]
[0236]
Chemical 41
[0237]
[0238] Examples of the dicarboxylic acid compound having two carboxyl groups include the compound represented by the following formula (C1).
[0239]
Chemical 42
[0240]
[0241] (In the formula (C1), Q 1 has the same meaning as Q in the formula (2-2) 1 )
[0242] Examples of the dihydroxy compound having two hydroxyl groups capable of reacting with an epoxy group include the compound represented by the following formula (C2).
[0243]
Chemical 43
[0244] HO-Q 1 -OH (C2)
[0245] (In the formula (C2), Q 1 has the same meaning as Q in the formula (2-2)1 Same meaning)
[0246] Examples of the compound represented by formula (C1) include the following compounds.
[0247]
Chemistry 44
[0248]
[0249]
Chemistry 45
[0250]
[0251] Examples of the compound represented by formula (C2) include the following compounds.
[0252]
Chemistry 46
[0253]
[0254] In addition, as the monomer for producing the polymer containing a fluorene structure, the following compounds can also be used.
[0255]
Chemistry 47
[0256]
[0257] Examples of the monocarboxyl compound having one carboxyl group include a compound represented by the following formula (D1).
[0258]
Chemistry 48
[0259]
[0260] (In formula (D1), Z has the same meaning as Z in formula (Z))
[0261] Examples of the compound represented by formula (D1) include the following compounds.
[0262]
Chemistry 49
[0263]
[0264]
Chemistry 50
[0265]
[0266]
Chemistry 51
[0267]
[0268] There is no particular restriction on the proportion of the fluorene structure in the polymer containing the fluorene structure. The proportion of the monomer containing the fluorene structure relative to the total monomers used to produce the polymer containing the fluorene structure is preferably 10 mol% to 90 mol%, more preferably 20 mol% to 80 mol%, and particularly preferably 30 mol% to 70 mol%.
[0269] Here, regarding the monomer, for example, in the above-mentioned production method examples (i) to (iv), the following compounds correspond to the monomer.
[0270] ·Dihydroxy compound represented by formula (A1-1)
[0271] Diepoxide compounds with two epoxy groups
[0272] · Diepoxy compound represented by formula (A1-2)
[0273] Dicarboxyl compounds with two carboxyl groups
[0274] ·Dihydroxy compounds with two hydroxyl groups
[0275] Monocarboxyl compounds with one carboxyl group
[0276] The content of the polymer containing a fluorene structure in the resist underlayer film-forming composition is not particularly limited, but is preferably 30 to 95% by mass, more preferably 50 to 90% by mass, and particularly preferably 60 to 85% by mass based on the film constituent components.
[0277] The film-constituting components refer to components obtained by removing volatile components (solvent) from the resist film-forming composition.
[0278] <Cross-linking agent>
[0279] The resist underlayer film-forming composition preferably contains a crosslinking agent from the viewpoint of favorably obtaining the effects of the present invention.
[0280] The cross-linking agent contained as an optional component in the resist underlayer film-forming composition has, for example, a functional group that reacts independently.
[0281] Examples of the crosslinking agent include hexamethoxymethylmelamine, tetramethoxymethylbenzoguanamine, 1,3,4,6-tetrakis(methoxymethyl)glycoluril (tetramethoxymethyl glycoluril) (POWDERLINK [registered trademark] 1174), 1,3,4,6-tetrakis(butoxymethyl)glycoluril, 1,3,4,6-tetrakis(hydroxymethyl)glycoluril, 1,3-bis(hydroxymethyl)urea, 1,1,3,3-tetrakis(butoxymethyl)urea, and 1,1,3,3-tetrakis(methoxymethyl)urea.
[0282] In addition, the crosslinking agent may also be a nitrogen-containing compound having 2 to 6 substituents represented by the following formula (1d) bonded to nitrogen atoms in one molecule as described in International Publication No. 2017 / 187969.
[0283]
Chemical Formula 52
[0284]
[0285] (In formula (1d), R 1 represents methyl or ethyl, and * represents a bonding site bonded to the nitrogen atom)
[0286] The nitrogen-containing compound having 2 to 6 substituents represented by the formula (1d) in one molecule may be a glycoluril derivative represented by the following formula (1E).
[0287]
Chemical Formula 53
[0288]
[0289] (In formula (1E), the four Rs 1 each independently represent methyl or ethyl, and R 2 and R 3 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group)
[0290] Examples of the glycoluril derivative represented by the formula (1E) may include compounds represented by the following formulas (1E-1) to (1E-6).
[0291]
Chemical Formula 54
[0292]
[0293] The nitrogen-containing compound having 2 to 6 substituents represented by the formula (1d) in one molecule can be obtained by reacting a nitrogen-containing compound having 2 to 6 substituents represented by the following formula (2d) bonded to nitrogen atoms in one molecule with at least one compound represented by the following formula (3d).
[0294]
Chemical Formula 55
[0295]
[0296] (In formulas (2d) and (3d), R 1 represents methyl or ethyl, R 4 represents an alkyl group having 1 to 4 carbon atoms, and * represents a bonding site bonded to the nitrogen atom)
[0297] The glycoluril derivative represented by the formula (1E) can be obtained by reacting the glycoluril derivative represented by the following formula (2E) with at least one compound represented by the formula (3d).
[0298] A nitrogen-containing compound having 2 to 6 substituents represented by the formula (2d) in one molecule, for example, a glycoluril derivative represented by the following formula (2E).
[0299]
Chemical 56
[0300]
[0301] (In the formula (2E), R 2 and R 3 each independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, or a phenyl group, and R 4 each independently represent an alkyl group having 1 to 4 carbon atoms)
[0302] Examples of the glycoluril derivative represented by the formula (2E) include compounds represented by the following formulas (2E-1) to (2E-4). In addition, examples of the compound represented by the formula (3d) include compounds represented by the following formulas (3d-1) and (3d-2).
[0303]
Chemical 57
[0304]
[0305]
Chemical 58
[0306]
[0307] Regarding the relevant content of the nitrogen-containing compound having 2 to 6 substituents represented by the formula (1d) bonded to the nitrogen atom in one molecule, the entire disclosure of WO2017 / 187969 is incorporated herein by reference in the present invention.
[0308] In addition, the above crosslinking agent may also be a crosslinkable compound represented by the following formula (G-1) or formula (G-2) described in International Publication No. 2014 / 208542.
[0309]
Chemical 59
[0310]
[0311] (In the formula, Q 1 represents a single bond or an m1-valent organic group, R 1 and R 4 each represent an alkyl group having 2 to 10 carbon atoms, or an alkyl group having 2 to 10 carbon atoms having an alkoxy group having 1 to 10 carbon atoms, R 2 and R 5 each represent a hydrogen atom or a methyl group, R 3 and R 6respectively represent an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms,
[0312] n1 represents an integer of 1≤n1≤3, n2 represents an integer of 2≤n2≤5, n3 represents an integer of 0≤n3≤3, n4 represents an integer of 0≤n4≤3, and 3≤(n1+n2+n3+n4)≤6,
[0313] n5 represents an integer of 1≤n5≤3, n6 represents an integer of 1≤n6≤4, n7 represents an integer of 0≤n7≤3, n8 represents an integer of 0≤n8≤3, and 2≤(n5+n6+n7+n8)≤5,
[0314] m1 represents an integer from 2 to 10)
[0315] The crosslinking compound represented by the above formula (G-1) or (G-2) may be a compound obtained by reacting a compound represented by the following formula (G-3) or (G-4) with a hydroxyl-containing ether compound or an alcohol having 2 to 10 carbon atoms.
[0316]
Chemistry 60
[0317]
[0318] (Where Q 2 Represents a single bond or an m2-valent organic group, R 8 , R 9 , R 11 and R 12 represent hydrogen atoms or methyl groups, R 7 and R 10 represents an alkyl group having 1 to 10 carbon atoms or an aryl group having 6 to 40 carbon atoms,
[0319] n9 represents an integer of 1≤n9≤3, n10 represents an integer of 2≤n10≤5, n11 represents an integer of 0≤n11≤3, n12 represents an integer of 0≤n12≤3, and 3≤(n9+n10+n11+n12)≤6,
[0320] n13 represents an integer of 1≤n13≤3, n14 represents an integer of 1≤n14≤4, n15 represents an integer of 0≤n15≤3, n16 represents an integer of 0≤n16≤3, and 2≤(n13+n14+n15+n16)≤5,
[0321] m2 represents an integer from 2 to 10)
[0322] The compounds represented by the above formula (G-1) and formula (G-2) can be exemplified as follows.
[0323]
Chemistry 61
[0324]
[0325]
Chemistry 62
[0326]
[0327]
Chemistry 63
[0328]
[0329]
Chemistry 64
[0330]
[0331]
Chemistry 65
[0332]
[0333] The compounds represented by formula (G-3) and formula (G-4) can be exemplified as follows.
[0334]
Chemistry 66
[0335]
[0336]
Chemistry 67
[0337]
[0338] In the formula, Me represents a methyl group.
[0339] The entire disclosure of International Publication No. 2014 / 208542 is incorporated herein by reference.
[0340] When the crosslinking agent is used, the content ratio of the crosslinking agent in the resist underlayer film-forming composition is, for example, 1 mass % to 50 mass %, preferably 5 mass % to 40 mass % based on the polymer containing a fluorene structure.
[0341] <Curing catalyst>
[0342] As the curing catalyst contained as an optional component in the resist underlayer film-forming composition, either a thermal acid generator or a photoacid generator may be used, and it is preferred to use a thermal acid generator.
[0343] Examples of the thermal acid generator include sulfonic acid compounds and carboxylic acid compounds such as p-toluenesulfonic acid, trifluoromethanesulfonic acid, pyridinium p-toluenesulfonate (pyridinium p-toluenesulfonate), pyridinium phenolsulfonate, pyridinium p-hydroxybenzenesulfonate (pyridinium p-phenolsulfonate), pyridinium trifluoromethanesulfonate, salicylic acid, camphorsulfonic acid, 5-sulfosalicylic acid, 4-chlorobenzenesulfonic acid, 4-hydroxybenzenesulfonic acid, benzenedisulfonic acid, 1-naphthalenesulfonic acid, citric acid, benzoic acid, and hydroxybenzoic acid.
[0344] Examples of the photoacid generator include onium salt compounds, sulfonyl imide compounds, and disulfonyldiazomethane compounds.
[0345] Examples of the onium salt compound include iodonium salt compounds such as diphenyliodonium hexafluorophosphate, diphenyliodonium trifluoromethanesulfonate, diphenyliodonium nonafluoro-n-butanesulfonate, diphenyliodonium perfluoro-n-octanesulfonate, diphenyliodonium camphorsulfonate, bis(4-tert-butylphenyl)iodonium camphorsulfonate, and bis(4-tert-butylphenyl)iodonium trifluoromethanesulfonate; and sulfonium salt compounds such as triphenylsulfonium hexafluoroantimonate, triphenylsulfonium nonafluoro-n-butanesulfonate, triphenylsulfonium camphorsulfonate, and triphenylsulfonium trifluoromethanesulfonate.
[0346] Examples of the sulfonyl imide compound include N-(trifluoromethanesulfonyloxy)succinimide, N-(nonafluoro-n-butanesulfonyloxy)succinimide, N-(camphorsulfonyloxy)succinimide, and N-(trifluoromethanesulfonyloxy)naphthalimide.
[0347] Examples of the disulfonyldiazomethane compound include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane, bis(2,4-dimethylbenzenesulfonyl)diazomethane, and methylsulfonyl-p-toluenesulfonyldiazomethane.
[0348] The curing catalyst may be used alone or in combination of two or more.
[0349] When a curing catalyst is used, the content ratio of the curing catalyst is, for example, 0.1 mass % to 50 mass %, preferably 1 mass % to 30 mass % based on the cross-linking agent.
[0350] <Solvent>
[0351] The solvent is preferably an organic solvent used in a general semiconductor lithography step solution. Specifically, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, cycloheptanone, 4-methyl-2-pentanol, methyl 2-hydroxyisobutyrate, 2- Ethyl hydroxyisobutyrate, ethyl ethoxylate, 2-hydroxyethyl acetate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, 2-heptanone, methoxycyclopentane, anisole, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide and N,N-dimethylacetamide. These solvents may be used alone or in combination of two or more.
[0352] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, ethyl lactate, butyl lactate and cyclohexanone are preferred, and propylene glycol monomethyl ether and propylene glycol monomethyl ether acetate are particularly preferred.
[0353] <Other ingredients>
[0354] A surfactant may be further added to the resist underlayer film-forming composition in order to prevent pinholes, streaks, and the like from being generated and to further improve coating properties on surface unevenness.
[0355] Examples of the surfactant include polyoxyethylene alkyl ethers such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, polyoxyethylene cetyl ether, and polyoxyethylene oleyl ether, polyoxyethylene alkyl allyl ethers such as polyoxyethylene octylphenol ether and polyoxyethylene nonylphenol ether, polyoxyethylene-polyoxypropylene block copolymers, sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan monooleate, sorbitan trioleate, and sorbitan tristearate, and sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan trioleate, and polyoxyethylene sorbitan tristearate. Nonionic surfactants such as polyoxyethylene sorbitan fatty acid esters such as sorbitan tristearate, FTOP EF301, EF303, EF352 (manufactured by Tochem Products Co., Ltd., trade name), MEGAFA CF171, F173, R-30 (manufactured by DIC Corporation, trade name), Fluorad FC430, FC431 (manufactured by Sumitomo 3M Co., Ltd., trade name), Asahiguard AG710, Surflon S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by Asahi Glass Co., Ltd., trade name), and the like, fluorine-based surfactants, organosiloxane polymer KP341 (manufactured by Shin-Etsu Chemical Co., Ltd.), and the like.
[0356] The amount of these surfactants blended is not particularly limited, but is usually 2.0 mass % or less, preferably 1.0 mass % or less, based on the total solid content of the resist underlayer film-forming composition.
[0357] These surfactants may be added alone or in combination of two or more.
[0358] The film constituting components contained in the resist underlayer film-forming composition, that is, the components excluding the solvent, are, for example, 0.01% by mass to 10% by mass of the resist underlayer film-forming composition.
[0359] The composition for forming a resist underlayer film for EB or EUV lithography is preferably used for forming a resist underlayer film for EB or EUV lithography having a film thickness of 10 nm or less.
[0360] (Resist underlayer film for EB or EUV lithography)
[0361] The resist underlayer film for EB or EUV lithography (hereinafter sometimes simply referred to as “resist underlayer film”) of the present invention is a cured product of the resist underlayer film-forming composition for EB or EUV lithography.
[0362] The resist underlayer film can be produced by, for example, applying the resist underlayer film-forming composition for EB or EUV lithography on a semiconductor substrate and firing the coating.
[0363] Examples of the semiconductor substrate to which the resist underlayer film-forming composition is applied include silicon wafers, germanium wafers, and compound semiconductor wafers such as gallium arsenide, indium phosphide, gallium nitride, indium nitride, and aluminum nitride.
[0364] In the case of using a semiconductor substrate having an inorganic film formed on the surface, the inorganic film can be formed by, for example, ALD (atomic layer deposition) method, CVD (chemical vapor deposition) method, reactive sputtering method, ion plating method, vacuum evaporation method, spin coating method (spin-on glass method: SOG). Examples of the inorganic film include polysilicon film, silicon oxide film, silicon nitride film, borophosphosilicate glass (BPSG, Boro-PhosphoSilicate Glass) film, titanium nitride film, titanium oxynitride film, tungsten film, gallium nitride film, and gallium arsenide film.
[0365] On such a semiconductor substrate, the resist underlayer film forming composition of the present invention is applied by a suitable coating method such as a spin coater or a coater. Then, a heating means such as a hot plate is used to bake to form a resist underlayer film. The baking conditions can be appropriately selected from a baking temperature of 100°C to 400°C and a baking time of 0.3 minutes to 60 minutes. In a suitable case, the baking temperature is 120°C to 350°C and the baking time is 0.5 minutes to 30 minutes. In a further preferred case, the baking temperature is 150°C to 300°C and the baking time is 0.8 minutes to 10 minutes.
[0366] The thickness of the resist underlayer film is, for example, 0.001 μm (1 nm) to 10 μm, 0.002 μm (2 nm) to 1 μm, 0.005 μm (5 nm) to 0.5 μm (500 nm), 0.001 μm (1 nm) to 0.05 μm (50 nm), 0.002 μm (2 nm) to 0.05 μm (50 nm), 0.003 μm (3 nm) to 0.05 μm (50 nm), 0.004 μm (4 nm) to 0.05 μm (50 nm), 0.005 μm (5 nm) to 0.05 μm (50 nm), nm), 0.003μm (3nm) ~ 0.03μm (30nm), 0.003μm (3nm) ~ 0.02μm (20nm), 0.005μm (5nm) ~ 0.02μm (20nm), 0.005μm (5nm) ~ 0.02μ m (20nm), 0.003μm (3nm) ~ 0.01μm (10nm), 0.005μm (5nm) ~ 0.01μm (10nm), 0.003μm (3nm) ~ 0.006μm (6nm), or 0.005μm (5nm).
[0367] The method for measuring the film thickness of the resist underlayer film in this specification is as follows.
[0368] ·Measurement device name: Ellipsometry film thickness measurement device RE-3100 (SCREEN Co., Ltd.)
[0369] SWE (Single Wavelength Ellipsometer) Mode
[0370] Arithmetic average of 8 points (e.g., 8 points at 1 cm intervals in the X direction of the wafer)
[0371] (Substrates for semiconductor processing)
[0372] The semiconductor processing substrate of the present invention comprises: a semiconductor substrate and the resist underlayer film for EB or EUV lithography of the present invention.
[0373] Examples of the semiconductor substrate include the above-mentioned semiconductor substrates.
[0374] The resist underlayer film is disposed on, for example, a semiconductor substrate.
[0375] (Semiconductor device manufacturing method, pattern forming method)
[0376] The method for manufacturing a semiconductor device of the present invention comprises at least the following steps.
[0377] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography of the present invention; and
[0378] · Step of forming a resist film on the resist underlayer film
[0379] The pattern forming method of the present invention comprises at least the following steps.
[0380] A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography of the present invention,
[0381] · Step of forming a resist film on the resist underlayer film
[0382] · a step of irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; and
[0383] ・Step of etching the resist lower layer film using the resist pattern as a mask
[0384] Usually, a resist film is formed on the resist underlayer film.
[0385] The thickness of the resist film is preferably below 200 nm, more preferably below 150 nm, more preferably below 100 nm, and particularly preferably below 80 nm. In addition, the thickness of the resist film is preferably above 10 nm, more preferably above 20 nm, and particularly preferably above 30 nm.
[0386] The method for forming the resist film is not particularly limited.
[0387] The resist film formed on the resist underlayer film by, for example, coating and firing by a known method is not particularly limited as long as it can be sensitive to EB or EUV used for irradiation. Either a negative photoresist or a positive photoresist can be used.
[0388] In addition, in this specification, the EB-sensitive resist is also referred to as a photoresist.
[0389] As photoresists, there are known positive photoresists formed of phenolic resin and 1,2-naphthoquinone diazosulfonic acid ester; chemically amplified photoresists formed of a binder having a group that decomposes by acid to increase the alkali dissolution rate and a photoacid generator; chemically amplified photoresists formed of a low molecular compound that decomposes by acid to increase the alkali dissolution rate of the photoresist, an alkali-soluble binder, and a photoacid generator; chemically amplified photoresists formed of a binder having a group that decomposes by acid to increase the alkali dissolution rate, a low molecular compound that decomposes by acid to increase the alkali dissolution rate of the photoresist, and a photoacid generator; resists containing metal elements, etc. Examples thereof include V146G manufactured by JSR Corporation, APEX-E manufactured by Shipley, PAR710 manufactured by Sumitomo Chemical Co., Ltd., and AR2772 and SEPR430 manufactured by Shin-Etsu Chemical Co., Ltd. In addition, fluorine atom-containing polymer photoresists described in, for example, Proc. SPIE, Vol. 3999, 330-334 (2000), Proc. SPIE, Vol. 3999, 357-364 (2000), or Proc. SPIE, Vol. 3999, 365-374 (2000) can be mentioned.
[0390] In addition, WO2019 / 188595, WO2019 / 187881, WO2019 / 187803, WO2019 / 167737, WO2019 / 167725, WO2019 / 187445, WO2019 / 167419, WO2019 / 123842, WO2019 / 054282, WO2019 / 058945, WO2019 / 058890, WO2019 / 039290, WO2019 / 044259, WO2019 / 044231, WO2019 / 026549, WO2018 / 193954, WO2019 / 172054, W O2019 / 021975, WO2018 / 230334, WO2018 / 194123, Japanese Special Opening 2018-180525, WO2018 / 190088, Japanese Special Opening 2018-070596, Japanese Special Opening 2018-028090, Japanese Special Opening 2016-153409, Japanese Special Opening 2016-130240, Japanese Special Opening 2016-108325, Japanese Special Opening 2016-047920, Japanese Special Opening 2016-035570, Japan Special opening 2016-035567, Japanese special opening 2016-035565, Japanese special opening 2019-101417, Japanese special opening 2019-117373, Japan Special Opening 2019-052294, Japanese Special Opening 2019-008280, Japanese Special Opening 2019-008279, Japanese Special Opening 2019-003176, Japanese Special Opening 2019-003175, Japanese Special Opening 2018-197853, Japanese Special Opening 2019-191298, Japanese Special Opening 2019-06 1217, Japan’s special opening 2018-045152, Japan’s special opening 2018-022039, Japan’s special opening 2016-090441, Japan’s special opening 2015- 10878, Japan’s special opening 2012-168279, Japan’s special opening 2012-022261, Japan’s special opening 2012-022258, Japan’s special opening 2011 -043749, Japanese Patent Application Laid-Open No. 2010-181857, Japanese Patent Application Laid-Open No. 2010-128369, WO2018 / 031896, Japanese Patent Application Laid-Open No. 2019-113855, WO2017 / 156388, WO2017 / 066319, Japanese Patent Application Laid-Open No. 2018-41099, WO2016 / 065120, WO2015 / 026482, Japanese Patent Application Laid-Open No. 2016-29498, Japanese Patent Application Laid-Open No. 2011-253185, etc., so-called resist compositions such as high-resolution patterning compositions based on organic metal solutions, and metal-containing resist compositions, but are not limited thereto.
[0391] Examples of the resist composition include the following compositions.
[0392] The active light-sensitive or radiation-sensitive resin composition comprises a compound represented by the following general formula (21) and a resin A having a repeating unit containing an acid-degradable group, wherein the polar group of the acid-degradable group is protected by a protective group that can be removed by the action of an acid.
[0393]
Chemistry 68
[0394]
[0395] In the general formula (21), m represents an integer of 1-6.
[0396] R 1 and R 2 Each independently represents a fluorine atom or a perfluoroalkyl group.
[0397] L 1 Represents -O-, -S-, -COO-, -SO 2 -, or -SO 3 -.
[0398] L 2 represents an alkylene group which may have a substituent or a single bond.
[0399] W 1 It represents a cyclic organic group which may have a substituent.
[0400] M + Represents a cation.
[0401] A metal-containing film-forming composition for extreme ultraviolet or electron beam lithography contains: a compound having a metal-oxygen covalent bond and a solvent, wherein the metal element constituting the compound belongs to the 3rd to 7th periods of the 3rd to 15th groups of the periodic table.
[0402] The radiation sensitive resin composition contains a polymer having a first structural unit represented by the following formula (31) and a second structural unit containing an acid dissociable group represented by the following formula (32), and an acid generator.
[0403]
Chemistry 69
[0404]
[0405] (In formula (31), Ar is a group obtained by removing (n+1) hydrogen atoms from an aromatic hydrocarbon having 6 to 20 carbon atoms, and R 1 is a hydroxyl group, a sulfonyl group or a monovalent organic group having 1 to 20 carbon atoms, n is an integer of 0 to 11, and when n is 2 or more, a plurality of R 1 Can be the same or different, R2 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group. In formula (32), R 3 is a monovalent group having 1 to 20 carbon atoms including the above acid dissociable group, Z is a single bond, an oxygen atom or a sulfur atom, R 4 is a hydrogen atom, a fluorine atom, a methyl group or a trifluoromethyl group)
[0406] The resist composition contains an acid generator and a resin (A1) including a structural unit having a cyclic carbonate structure, a structural unit represented by the following formula, and a structural unit having an acid-labile group.
[0407]
Chemistry 70
[0408]
[0409] [Where R 2 represents an alkyl group having 1 to 6 carbon atoms which may have a halogen atom, a hydrogen atom or a halogen atom, and X 1 Represents a single bond, -CO-O-* or -CO-NR 4 -*, * represents the connecting bond of -Ar, R 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and Ar represents an aromatic hydrocarbon group having 6 to 20 carbon atoms which may have one or more groups selected from a hydroxyl group and a carboxyl group.]
[0410] As the resist film, for example, the following can be mentioned.
[0411] A resist film comprising a base resin comprising a repeating unit represented by the following formula (a1) and / or a repeating unit represented by the following formula (a2), and a repeating unit which generates an acid bonded to a polymer main chain by exposure.
[0412]
Chemistry 71
[0413]
[0414] (In formula (a1) and formula (a2), R A are each independently a hydrogen atom or a methyl group, R 1 and R 2 Each independently represents a tertiary alkyl group having 4 to 6 carbon atoms, R 3 are each independently a fluorine atom or a methyl group, m is an integer from 0 to 4, and X 1 is a single bond, a phenylene group or a naphthylene group, an ester bond, a lactone ring, or a linking group having 1 to 12 carbon atoms and containing at least one selected from a phenylene group and a naphthylene group, 2 is a single bond, an ester bond or an amide bond)
[0415] Examples of the resist material include the following.
[0416] A resist material containing a polymer having a repeating unit represented by the following formula (b1) or formula (b2).
[0417]
Chemical 72
[0418]
[0419] (In formula (b1) and formula (b2), R A is a hydrogen atom or a methyl group, X 1 is a single bond or an ester group, X 2 is a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms or an arylene group having 6 to 10 carbon atoms. Part of the methylene groups constituting the alkylene group may be substituted with an ether group, an ester group or a group containing a lactone ring. In addition, at least one hydrogen atom contained in X 2 is substituted with a bromine atom, X 3 is a single bond, an ether group, an ester group, a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms. Part of the methylene groups constituting the alkylene group may be substituted with an ether group or an ester group, Rf 1 ~Rf 4 are each independently a hydrogen atom, a fluorine atom or a trifluoromethyl group, and at least one of them is a fluorine atom or a trifluoromethyl group. In addition, Rf 1 and Rf 2 may combine together to form a carbonyl group, R 1 ~R 5 are each independently a linear, branched or cyclic alkyl group having 1 to 12 carbon atoms, a linear, branched or cyclic alkenyl group having 2 to 12 carbon atoms, an alkynyl group having 2 to 12 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aralkyl group having 7 to 12 carbon atoms, an aryloxyalkyl group having 7 to 12 carbon atoms. Part or all of the hydrogen atoms of these groups may be substituted with a hydroxyl group, a carboxyl group, a halogen atom, a side oxygen group, a cyano group, an acylamino group, a nitro group, a sultone group, a sulfone group or a group containing a sulfonium salt. Part of the methylene groups constituting these groups may be substituted with an ether group, an ester group, a carbonyl group, a carbonate group or a sulfonate group. In addition, R 1 may also bond to R 2 and form a ring together with the sulfur atom to which it is bonded)
[0420] A resist material containing a base resin, the base resin containing a polymer having a repeating unit represented by the following formula (a).
[0421]
Chemical 73
[0422]
[0423] (In formula (a), R A is a hydrogen atom or a methyl group, R 1 is a hydrogen atom or an acid-labile group, R 2is a linear, branched or cyclic alkyl group having 1 to 6 carbon atoms, or a halogen atom other than bromine, X 1 is a single bond or a linear, branched or cyclic alkylene group having 1 to 12 carbon atoms which may contain an ester group or a lactone ring, X 2 is -O-, -O-CH 2 -, or -NH-, m is an integer of 1 to 4, u is an integer of 0 to 3, provided that m + u is an integer of 1 to 4)
[0424] A resist composition that generates an acid upon exposure and whose solubility in a developer changes by the action of the acid, comprising: a substrate component (A) whose solubility in a developer changes by the action of an acid, and a fluorine additive component (F) that exhibits decomposability with respect to an alkali developer
[0425] The fluorine additive component (F) contains a fluororesin component (F1) having a structural unit (f1) containing an alkali-dissociable group and a structural unit (f2) containing a group represented by the following general formula (f2-r-1).
[0426]
Chemical formula 74
[0427]
[0428] [In formula (f2-r-1), Rf 21 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a hydroxyl group, a hydroxyalkyl group or a cyano group, n” is an integer of 0 to 2, and * is a linking bond]
[0429] The structural unit (f1) contains a structural unit represented by the following general formula (f1-1) or a structural unit represented by the following general formula (f1-2).
[0430]
Chemical formula 75
[0431]
[0432] [In formulas (f1-1) and (f1-2), R are each independently a hydrogen atom, an alkyl group having 1 to 5 carbon atoms or a halogenated alkyl group having 1 to 5 carbon atoms, X is a divalent linking group having no acid-dissociable moiety, A aryl is a divalent aromatic cyclic group which may have a substituent. X 01 is a single bond or a divalent linking group, R 2 are each independently an organic group having a fluorine atom]
[0433] Coatings, coating solutions and coating compositions include, for example, the following.
[0434] A coating comprising a metal oxy-hydroxy network having an organic ligand through a metal-carbon bond and / or a metal carboxylate bond.
[0435] An inorganic oxygen / hydroxyl based composition.
[0436] A coating solution comprising: an organic solvent; a first organic metal composition, which is a compound of formula R z SnO (2-(z / 2)-(x / 2)) (OH) x (where 0<z≤2 and 0<(z+x)≤4), formula R'nSnX 4- n (here, n=1 or 2) or a mixture thereof, wherein R and R' are independently a hydrocarbon group having 1 to 31 carbon atoms, and X is a ligand having a hydrolyzable bond to Sn or a combination thereof; and a hydrolyzable metal compound represented by the formula MX'v (here, M is a metal selected from Groups 2 to 16 of the periodic table, v=a number from 2 to 6, and X' is a ligand having a hydrolyzable MX bond or a combination thereof).
[0437] The coating solution comprises an organic solvent and a material of the formula RSnO (3 / 2 -x / 2) The first organometallic compound is represented by (OH)x (wherein 0<x<3), and the solution contains about 0.0025M to about 1.5M of tin, and R is an alkyl or cycloalkyl group having 3 to 31 carbon atoms, and the alkyl or cycloalkyl group is bonded to tin at a secondary or tertiary carbon atom.
[0438] An aqueous precursor solution for forming an inorganic pattern comprises a mixture of water, metal suboxide cations, polyatomic inorganic anions, and a radiation-sensitive ligand containing a peroxide group.
[0439] EB or EUV irradiation is performed through a mask (reticle) for forming a predetermined pattern. The resist underlayer film-forming composition of the present invention is suitable for EB (electron beam) or EUV (extreme ultraviolet light: 13.5 nm) irradiation, and is preferably suitable for EUV (extreme ultraviolet light) exposure.
[0440] The irradiation energy of EB and the exposure amount of EUV are not particularly limited.
[0441] After EB or EUV irradiation and before development, baking (PEB: Post Exposure Bake) may be performed.
[0442] The baking temperature is not particularly limited, but is preferably 60°C to 150°C, more preferably 70°C to 120°C, and particularly preferably 75°C to 110°C.
[0443] The baking time is not particularly limited, but is preferably 1 second to 10 minutes, more preferably 10 seconds to 5 minutes, and particularly preferably 30 seconds to 3 minutes.
[0444] For development, for example, an alkaline developer can be used.
[0445] The development temperature may be, for example, 5°C to 50°C.
[0446] The development time may be, for example, 10 seconds to 300 seconds.
[0447] Alkaline developer can be used, for example, inorganic bases such as sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, ammonia water, etc., primary amines such as ethylamine, n-propylamine, secondary amines such as diethylamine, di-n-butylamine, tertiary amines such as triethylamine, methyldiethylamine, alcohol amines such as dimethylethanolamine, triethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, quaternary ammonium salts of choline, cyclic amines such as pyrrole and piperidine, etc., aqueous solutions of alkalis. In addition, in the aqueous solution of the above-mentioned alkalis, alcohols such as isopropyl alcohol, nonionic surfactants such as the like can also be added in appropriate amounts for use. Among these, suitable developer is an aqueous solution of quaternary ammonium salt, more preferably an aqueous solution of tetramethylammonium hydroxide and an aqueous solution of choline. In addition, surfactants, etc. can also be added to these developers. It is also possible to use an organic solvent such as butyl acetate instead of an alkali developer for development, so that the method of partially developing the photoresist where the alkali dissolution rate is not improved.
[0448] Next, the resist underlayer film is etched using the formed resist pattern as a mask. The etching may be dry etching or wet etching, with dry etching being preferred.
[0449] When the inorganic film is formed on the surface of the semiconductor substrate used, the surface of the inorganic film is exposed, and when the inorganic film is not formed on the surface of the semiconductor substrate used, the surface of the semiconductor substrate is exposed. Then, the semiconductor substrate is processed by a known method (dry etching method, etc.) to manufacture a semiconductor device.
[0450] Example
[0451] Next, the present invention will be described in detail with reference to examples, but the present invention is not limited to these examples.
[0452] The weight average molecular weight of the polymers shown in the following synthesis examples is the result of measurement by gel permeation chromatography (hereinafter referred to as GPC). The measurement was performed using a GPC apparatus manufactured by Tosoh Corporation, and the measurement conditions and the like were as follows.
[0453] GPC columns: ShodexKF803L, ShodexKF802, ShodexKF801 [registered trademark] (Showa Denko K.K.)
[0454] Column temperature: 40℃
[0455] Solvent: Tetrahydrofuran (THF)
[0456] Flow rate: 1.0 ml / min
[0457] Standard sample: Polystyrene (manufactured by Tosoh Corporation)
[0458] <Synthesis Example 1>
[0459] In a reaction vessel, 5.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Chemicals Corporation), 5.32 g of 9,9-bis(4-hydroxyphenyl)fluorene (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.96 g of adamantane carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.21 g of tetrabutylammonium bromide (manufactured by ACROS Organics) were added to 79.00 g of propylene glycol monomethyl ether and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the mixture was reacted at 105 °C for 24 hours to obtain a polymer solution. This polymer solution did not become cloudy even when cooled to room temperature and had good solubility in propylene glycol monomethyl ether. As a result of GPC analysis, the polymer in the obtained solution had a weight-average molecular weight of 8000 in terms of standard polystyrene. The polymer obtained in this synthesis example has structural units represented by the following formulas (1a), (2a), and (3a).
[0460] [Chemical Formula 76]
[0461]
[0462] <Synthesis Example 2>
[0463] In a reaction vessel, 10.00 g of 9,9-bis(4-glycidyloxyphenyl)fluorene (manufactured by Osaka Gas Chemical Co., Ltd., trade name: Ogsol PG), 5.32 g of 3,3'-dithiobispropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), 1.16 g of adamantane carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.25 g of tetrabutylammonium bromide (manufactured by ACROS Organics) were added to 35.58 g of propylene glycol monomethyl ether and dissolved. After replacing the atmosphere in the reaction vessel with nitrogen, the mixture was reacted at 105 °C for 24 hours to obtain a polymer solution. This polymer solution did not become cloudy even when cooled to room temperature and had good solubility in propylene glycol monomethyl ether. As a result of GPC analysis, the polymer in the obtained solution had a weight-average molecular weight of 9000 in terms of standard polystyrene. The polymer obtained in this synthesis example has structural units represented by the following formulas (1b), (2b), and (3a).
[0464] [Chemical Formula 77]
[0465]
[0466] <Synthesis Example 3>
[0467] In a reaction vessel, 5.00 g of 3',6'-bis(2-oxiranylmethoxy)spiro[9H-fluorene-9,9'-[9H]xanthene] (manufactured by Taoka Chemical Industry Co., Ltd., trade name: TBIS-RXG), 1.82 g of 3,3'-dithiobispropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), 0.55 g of adamantane carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.25 g of tetrabutylammonium bromide (manufactured by ACROSS Corporation) were added to 30.00 g of propylene glycol monomethyl ether and dissolved. After replacing the nitrogen in the reaction vessel, the mixture was reacted at 105 °C for 24 hours to obtain a polymer solution. The polymer solution did not become cloudy even when cooled to room temperature and had good solubility in propylene glycol monomethyl ether. As a result of GPC analysis, the polymer in the obtained solution had a weight-average molecular weight of 8000 in terms of standard polystyrene. The polymer obtained in this synthesis example has structural units represented by the following formulas (1c), (2b), and (3a).
[0468] [Chemical Formula 78]
[0469]
[0470] <Comparative Synthesis Example 1>
[0471] In a reaction vessel, 3.00 g of monoallyl diglycidyl isocyanurate (manufactured by Shikoku Kasei Kogyo Co., Ltd.), 1.91 g of 3,3'-dithiobispropionic acid (manufactured by Sakai Chemical Industry Co., Ltd., trade name: DTDPA), 0.57 g of adamantane carboxylic acid (manufactured by Tokyo Chemical Industry Co., Ltd.), and 0.14 g of tetrabutylammonium bromide (manufactured by ACROSS Corporation) were added to 6.87 g of propylene glycol monomethyl ether and dissolved. After replacing the nitrogen in the reaction vessel, the mixture was reacted at 105 °C for 8 hours to obtain a polymer solution. The polymer solution did not become cloudy even when cooled to room temperature and had good solubility in propylene glycol monomethyl ether. As a result of GPC analysis, the polymer in the obtained solution had a weight-average molecular weight of 5000 in terms of standard polystyrene. The polymer obtained in this synthesis example has structural units represented by the following formulas (1b), (2a), and (3a).
[0472] [Chemical Formula 79]
[0473]
[0474] <Example 1>
[0475] 0.02 g of tetramethoxymethyl glycoluril (manufactured by Cytec Industries, Japan), 0.003 g of pyridinium phenolsulfonate, 44.5 g of propylene glycol monomethyl ether and 4.99 g of propylene glycol monomethyl ether acetate were added to 0.43 g (solid content: 16.4 wt%) of the polymer solution obtained in Synthesis Example 1 and dissolved. The mixture was then filtered using a polyethylene microfilter having a pore size of 0.05 μm to form a resist underlayer film-forming composition for lithography.
[0476] <Example 2>
[0477] 0.02 g of tetramethoxymethyl glycoluril (manufactured by Cytec Industries, Japan), 0.003 g of pyridinium phenolsulfonate, 44.6 g of propylene glycol monomethyl ether and 4.99 g of propylene glycol monomethyl ether acetate were added and dissolved in 0.47 g (solid content: 17.8 wt%) of the polymer solution obtained in Synthesis Example 2. The mixture was then filtered using a polyethylene microfilter having a pore size of 0.05 μm to form a resist underlayer film-forming composition for lithography.
[0478] <Example 3>
[0479] 0.02 g of tetramethoxymethyl glycoluril (manufactured by Cytec Industries, Japan), 0.003 g of pyridinium phenolsulfonate, 44.6 g of propylene glycol monomethyl ether and 4.99 g of propylene glycol monomethyl ether acetate were added and dissolved in 0.47 g of the polymer solution obtained in Synthesis Example 3 (solid content: 18.3 wt%), and then filtered using a polyethylene microfilter with a pore size of 0.05 μm to form a resist underlayer film-forming composition for lithography.
[0480] <Comparative Example 1>
[0481] 0.02 g of tetramethoxymethyl glycoluril (manufactured by Cytec Industries, Japan), 0.003 g of pyridinium phenolsulfonate, 44.6 g of propylene glycol monomethyl ether and 4.99 g of propylene glycol monomethyl ether acetate were added and dissolved in 0.47 g of the polymer solution obtained in the above-mentioned comparative synthesis example 1 (solid content: 18.0 wt%), and then filtered using a polyethylene microfilter with a pore size of 0.05 μm to form a resist underlayer film-forming composition for lithography.
[0482] [Dissolution test of photoresist solvent]
[0483] The resist underlayer film-forming compositions of Example 1, Example 2, Example 3 and Comparative Example 1 were applied to the silicon wafer of the semiconductor substrate by a spin coater. The silicon wafer was placed on a hot plate and baked at 205° C. for 1 minute to form a resist underlayer film (film thickness 5 nm). These resist underlayer films were immersed in ethyl lactate and propylene glycol monomethyl ether, solvents used for photoresists, respectively, and it was confirmed that they were insoluble in these solvents.
[0484] [Formation of positive resist pattern using electron beam lithography apparatus]
[0485] The compositions for forming the resist underlayer film of Example 1, Example 2, Example 3 and Comparative Example 1 were respectively coated on a silicon wafer using a spin coater. The silicon wafer was baked on a hot plate at 205°C for 60 seconds to obtain a resist underlayer film with a film thickness of 5 nm. A positive resist solution for EUV (containing a methacrylic acid polymer) was spin-coated on the resist underlayer film and heated at 130°C for 60 seconds to form an EUV resist film. The resist film was exposed under predetermined conditions using an electron beam drawing device (ELS-G130). After exposure, it was baked (PEB) at 100°C for 60 seconds, cooled to room temperature on a cooling plate, and developed with an alkaline developer (2.38% TMAH) to form a resist pattern with a line width and spacing of CD 25nm / 50nm spacing. The length of the resist pattern was measured using a scanning electron microscope (manufactured by Hitachi High Technologies Co., Ltd., CG4100). The LWR of the critical dimension (CD dimension) of 25 nm in the formation of the above-mentioned resist pattern was compared.
[0486] Table 1
[0487]
[0488] All of Examples 1, 2, and 3 showed better LWR than Comparative Example 1.
Claims
1. A composition for forming a resist underlayer film for EB or EUV lithography, comprising: a polymer having a fluorene structure and a solvent.
2. The resist underlayer film forming composition for EB or EUV lithography according to claim 1, wherein the polymer comprises a partial structure represented by the following formula (1): In formula (1), X 1 represents a divalent organic group having a fluorene structure, Z 1 and Z 2 Each independently represents a single bond, -O-, -C(=O)O- or -OC m H 2m -O-, m represents an integer from 1 to 6, A 1 , A 2 , A 3 , A 4 , A 5 and A 6 each independently represents a hydrogen atom, a methyl group or an ethyl group, * indicates a connection key.
3. The resist underlayer film-forming composition for EB or EUV lithography according to claim 2, wherein X in the formula (1) 1 represents a divalent organic group represented by the following formula (1-A) or (1-B), In formula (1-A) and (1-B), R 1 , R 2 , R 5 and R 6 each independently represents a hydroxyl group, an acyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alkoxycarbonyl group having 1 to 6 carbon atoms, an alkyl group having 1 to 10 carbon atoms, an aryl group having 6 to 20 carbon atoms, an alkenyl group having 2 to 20 carbon atoms, or an alkynyl group having 2 to 10 carbon atoms, and the acyl group, alkoxy group, alkoxycarbonyl group, alkyl group, aryl group, alkenyl group, and alkynyl group may have one or more groups selected from an amino group, a nitro group, a cyano group, a hydroxyl group, a glycidyl group, and a carboxyl group, R 3 and R 4 each independently represents a single bond or an alkylene group having 1 to 10 carbon atoms, m1 and m2 each independently represent an integer from 0 to 4, n1 and n2 each independently represent 0 or 1, When n1 is 0, o1 represents an integer from 0 to 4; when n1 is 1, o1 represents an integer from 0 to 6. When n2 is 0, o2 represents an integer from 0 to 4; when n2 is 1, o2 represents an integer from 0 to 6. R 1 ~R 6 When there are multiple R 1 ~R 6 They may be the same or different. One R 5 With an R 6 can form an -O- bond together, * indicates a connection key.
4. The resist underlayer film forming composition for EB or EUV lithography according to claim 2, wherein the polymer further comprises at least one of a partial structure represented by the following formula (2-1) and a partial structure represented by the following formula (2-2), In formula (2-1), X 11 represents a group represented by any one of the following formulae (2-1-1) to (2-1-3), Z 11 and Z 12 Each independently represents a single bond or a divalent group represented by the following formula (2-1-4), In formula (2-2), Q 1 represents a single bond or a divalent organic group, p1 and p2 each independently represent 0 or 1, In formulas (2-1-1) to (2-1-3), R 11 ~R 15 each independently represents a hydrogen atom, an alkyl group having 1 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkenyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, an alkynyl group having 2 to 10 carbon atoms which may be interrupted by an oxygen atom or a sulfur atom, a benzyl group, or a phenyl group, wherein the phenyl group may be substituted with at least one monovalent group selected from an alkyl group having 1 to 6 carbon atoms, a halogen atom, an alkoxy group having 1 to 6 carbon atoms, a nitro group, a cyano group, and an alkylthio group having 1 to 6 carbon atoms, and R 11 With R 12 can be combined with each other to form a ring with 3 to 6 carbon atoms, R 13 With R 14 can be bonded to each other to form a ring having 3 to 6 carbon atoms, * represents a bond, *1 represents a bond bonded to a carbon atom, and *2 represents a bond bonded to a nitrogen atom, In the formula (2-1-4), m1 represents an integer of 1 to 4, m2 represents 0 or 1, *3 represents a bond to a nitrogen atom, and *4 represents a bond. 5 . The resist underlayer film forming composition for EB or EUV lithography according to claim 1 , further comprising a crosslinking agent. 6 . The resist underlayer film forming composition for EB or EUV lithography according to claim 1 , further comprising a curing catalyst. 7 . The composition for forming a resist underlayer film for EB or EUV lithography according to claim 1 , which is used for forming a resist underlayer film for EB or EUV lithography having a film thickness of 10 nm or less. 8 . A resist underlayer film for EB or EUV lithography, which is a cured product of the resist underlayer film-forming composition for EB or EUV lithography according to claim 1 .
9. A semiconductor processing substrate comprising: A semiconductor substrate and the resist underlayer film for EB or EUV lithography according to claim 8.
10. A method for manufacturing a semiconductor device, comprising: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography according to any one of claims 1 to 7; and A step of forming a resist film on the resist underlayer film.
11. A pattern forming method, comprising: A step of forming a resist underlayer film on a semiconductor substrate using the resist underlayer film-forming composition for EB or EUV lithography according to any one of claims 1 to 7; forming a resist film on the resist underlayer film; irradiating the resist film with EB or EUV, and then developing the resist film to obtain a resist pattern; and A step of etching the resist underlayer film using the resist pattern as a mask.