Capacitance reduction in semiconductor devices

By using plasma enhanced atomic layer deposition technology in semiconductor equipment, the reaction stream is diluted to form air gaps, which solves the problem of high capacitance in the middle layer of the prior art, and the formation of low dielectric constant air gaps is achieved, reducing parasitic capacitance and improving Equipment performance.

CN118891698APending Publication Date: 2024-11-01LAM RES CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380028358.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-27
Filing Date
2023-03-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to effectively form a low dielectric constant air gap in semiconductor devices, resulting in an increase in the capacitance in the layer and affecting the performance of the equipment.

Method used

Using plasma enhanced atomic layer deposition (PEALD) technology, air gaps are formed in holes and trench structures by diluting the reaction stream, preferentially depositing dielectric materials on top of the features, thus forming a closed low-dial constant air gap between features .

Benefits of technology

The in-layer capacitance in semiconductor devices has been successfully reduced, parasitic capacitance has been reduced, equipment performance has been improved, and the appropriate position and size of the air gap has been achieved by controlling process parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891698A_ABST
    Figure CN118891698A_ABST
Patent Text Reader

Abstract

Methods of forming air gaps in hole and trench structures using plasma enhanced atomic layer deposition (PEALD) are disclosed. The method may be used to form a buried void, i.e., a void that is lower than the top of an adjacent feature. In some embodiments, the methods are used to reduce in-layer capacitance in a semiconductor device.
Need to check novelty before this filing date? Find Prior Art

Description

Incorporated by Reference

[0001] The PCT application form is filed concurrently with this specification as a part of this application. Each application identified in the concurrently filed PCT application form to which this application claims the benefit or priority is incorporated herein by reference in its entirety and for all purposes. Background Art

[0002] Air is a ferroelectric with a dielectric constant, k, close to unity. Air gaps can be formed in semiconductor device structures to provide ultra-low-k materials separating conductors.

[0003] The background description provided here is for the purpose of generally presenting the context of the present disclosure. The work of the presently designated inventors is neither explicitly nor implicitly admitted to be prior art against the present disclosure to the extent that it is described in this background section and to aspects of the specification that could not be determined as prior art at the time of filing the application. Summary of the invention

[0004] A method for forming air gaps in hole and trench structures is disclosed. The method can be used to form buried voids. A buried void is a void that is below the top of an adjacent feature. The method includes plasma enhanced deposition of a dielectric material using a diluted reactant stream during a plasma operation. In some embodiments, the method includes diluting a reactive gas species during a plasma conversion operation of a plasma enhanced atomic layer deposition (PEALD) process. This results in a lack of reactive ions and / or radicals at the bottom of the feature, resulting in non-conformal growth that preferentially deposits near the top of the feature. Repeating this sequence results in the formation of an air gap.

[0005] One aspect of the present disclosure relates to a method, comprising: providing a structure including features and open gaps between the features, the open gaps including sidewalls and a bottom surface; and performing multiple plasma enhanced atomic layer deposition (PEALD) cycles, each cycle comprising: exposing the structure to a dose of a silicon-containing precursor so that the silicon-containing precursor is adsorbed on the sidewalls and the bottom surface of the open gaps; and exposing the adsorbed silicon-containing precursor to a plasma generated by a process gas including a co-reactant and one or more dilution gases so that the co-reactant reacts with the adsorbed silicon-containing precursor and forms a dielectric material, wherein the dielectric material is preferentially formed near the top of the open gap, wherein the volume flow rate ratio of the one or more dilution gases to the co-reactant is at least 5:1.

[0006] In some embodiments, the method further comprises closing the open gap with the deposited dielectric material, thereby forming a closed air gap between the features. In some embodiments, the top of the closed air gap is lower than the top of the feature. In some embodiments, the top of the closed air gap is at least 5 nanometers lower than the top of the feature.

[0007] In some embodiments, the method further comprises purging the chamber containing the structure between step (a) and step (b). In some embodiments, the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 10:1. In some embodiments, the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 20:1. In some embodiments, the volume flow rate ratio of the one or more dilution gases to the co-reactants is between 5:1 and 50:1. In some embodiments, the co-reactant is an oxygen-containing gas. In some embodiments, the co-reactant is nitrous oxide (N2O) and / or oxygen (O2). In some embodiments, the co-reactant is nitrogen (N2). In some embodiments, the duration of (a) in each cycle is at least twice the duration of (b). In some embodiments, the open gap has a first area and the closed air gap occupies at least 80% of the first area. In some embodiments, the closed air gap occupies at least 90% of the first area.

[0008] Another aspect of the present disclosure relates to a method comprising: providing a structure including features and open gaps between the features, the open gaps having a first area and including sidewalls and a bottom surface; and performing multiple plasma enhanced atomic layer deposition (PEALD) cycles to preferentially deposit a dielectric material on top of the open gaps to form closed air gaps between the features, each cycle comprising: exposing the structure to a dose of a silicon-containing precursor so that the silicon-containing precursor is adsorbed on the sidewalls and bottom surfaces of the open gaps; and exposing the adsorbed silicon-containing precursor to a plasma generated by a process gas including a co-reactant and one or more dilution gases so that the co-reactant reacts with the adsorbed silicon-containing precursor and forms the dielectric material, wherein the closed air gaps are formed without etching or inhibiting operations, and the closed air gaps occupy at least 80% of the first area.

[0009] In some embodiments, the enclosed air gap occupies at least 90% of the first area. In some embodiments, the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 10: 1. In some embodiments, the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 20: 1.

[0010] This and other aspects are further described below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 A process flow diagram showing an exemplary method of forming an air gap.

[0012] Figure 2 Schematic cross-sectional view of a feature before and after air gap formation is included.

[0013] Figure 3 is a process flow diagram for performing a single plasma enhanced atomic layer deposition cycle as part of a method of forming an air gap.

[0014] Figure 4 is an example of a gas and plasma RF timing at a plasma enhanced atomic layer deposition (PEALD) station that may be implemented according to embodiments described herein.

[0015] Figure 5 Includes examples of cross-sectional schematics of a feature before and after air gap formation.

[0016] Figure 6 Included are examples of cross-sectional schematics of a feature with air gaps before and after planarization.

[0017] Figure 7 is a schematic diagram of an embodiment of an atomic layer deposition (ALD) processing station that can be used to perform the methods described herein.

[0018] Figure 8 is a schematic diagram of an embodiment of a multi-station processing tool that can be used to perform the methods described herein. DETAILED DESCRIPTION

[0019] In the following description, numerous specific details are set forth to provide a thorough understanding of the embodiments presented. The disclosed embodiments may be implemented without some or all of these specific details. In other cases, well-known processing operations are not described in detail to avoid unnecessarily obscuring the disclosed embodiments. Although the disclosed embodiments will be described in conjunction with specific embodiments, it should be understood that they are not intended to limit the disclosed embodiments.

[0020] Methods for forming air gaps in hole and trench structures are disclosed. An air gap is a closed space in a hole, trench, or other recess containing air. In some embodiments, the method is used to reduce intra-layer capacitance in a semiconductor device. The method includes plasma enhanced deposition of a dielectric material using a dilute reactant stream during plasma operation.

[0021] In some embodiments, the method includes diluting the reactive gas species during the plasma conversion operation of a plasma enhanced atomic layer deposition (PEALD) process. This can result in a lack of reactive ions and / or free radicals at the bottom of the feature, resulting in non-conformal growth that is preferentially deposited near the top of the feature. Repeating this sequence results in the formation of air gaps. As discussed further below, the conformality of the process and the position of the air gap can be controlled by various parameters, including reactive species chemistry, gas flow ratio, pressure, and plasma power. Air gaps in appropriate locations throughout different structures and feature sizes can be formed.

[0022] Figure 1 1 is a flow chart showing an exemplary method 100 for forming an air gap. First, in operation 101, a structure having an open gap between features is provided. The structure may be a hole or trench structure or other structure between two features that will form an air gap, and the two features may be conductive features, dielectric features, semiconductor features, etc. Examples of structures are as follows: Figure 2 As shown, further discussed below.

[0023] In some embodiments, the method is used to reduce the intra-layer capacitance in semiconductor devices. However, they can also be used to form air gaps in any appropriate environment, including forming air gaps in metal films or layers and forming air gaps in MEMS devices. Examples of semiconductor structures include interconnects, wires, or other conductive features. The method can also be implemented in any situation where a dielectric film between features covers the air gap. Examples of structures include 3D NAND structures (e.g., slits), DRAM structures (e.g., bitline structures), metal lines in back-end-of-line (BEOL) processes, and logic gates.

[0024] The structure is characterized as having two or more adjacent features with an open gap between the features. In many implementations, the feature is a conductive feature, and the air gap formed provides a very low-k dielectric and reduced parasitic capacitance. However, the sidewall surface of the feature may include any suitable material, including conductive, dielectric or semiconductor materials or any combination of these materials. For example, the structure may be a copper (Cu) wire coated with a silicon carbide (SiC) film. The size of the structure depends on the specific application. For example, an incoming DRAM structure may have a gap of 25-50nm wide and 300-800nm ​​deep, and an incoming 3D NAND structure may be 50-100nm wide and 5-14 microns deep. However, the method described herein is not limited to any specific structure size, feature composition or sidewall surface. In some embodiments, the method can be implemented in applications where it is difficult to implement other technologies for forming air gaps (such as deposition and removal of sacrificial materials). The structure is typically provided to a deposition chamber.

[0025] Next, an optional conformal or bottom-up deposition of material in the structure is performed in operation 103. The material may be the same or different than the material that will be formed on top of the structure in a subsequent operation. The material may be deposited to achieve a particular arrangement and / or geometry of the air gap. For example, if the bottom of the air gap is designed to be above the bottom of the structure, the bottom of the air gap may be formed to have a shape that is substantially the same as the bottom of the structure. can be deposited at the bottom of the structure materials.

[0026] In some embodiments, a conformal liner layer of material is formed. A conformal deposition process such as PEALD may be used for conformal deposition. In some embodiments, operation 103 is omitted.

[0027] In a PEALD process, an adsorbed silicon-containing precursor (or other dielectric precursor) reacts with a co-reactant delivered in a plasma. For example, an oxidizing plasma may be used to form a silicon oxide film. Plasma may refer to a conversion plasma, and the operation of exposing a dielectric precursor to a plasma may be referred to as a plasma conversion operation.

[0028] In operation 105, dielectric material is preferentially deposited on top of the structure by PEALD using a diluted co-reactant stream during a plasma conversion operation. This gas dilution results in a co-reactant-starved conversion, where most of the reactive plasma species are consumed at or near the top of the structure. Few reactive species reach the bottom of the structure, resulting in little growth. The PEALD process preferentially deposits dielectric material on top of the structure. Sidewall growth at the top of the structure closes the structure, leaving an air gap below.

[0029] Figure 2 An example of a structure including features 205 and open gaps 206 on a substrate 201 before and after deposition is shown. Features 205 may be, for example, metal contacts. Open gaps 206 are between features 205 and have sidewall surfaces 215 and bottom surfaces 217. Sidewall surfaces 215 extend from the openings and are connected by bottom surfaces 217. Substrate 201 may be a silicon or other semiconductor wafer, such as a 200-mm wafer, a 300-mm wafer, or a 450-mm wafer, including wafers having one or more layers of material (e.g., dielectric, conductive, or semiconductor material) deposited thereon. The method may also be applied to forming structures with air gaps on other substrates such as glass, plastic, and the like, including in the manufacture of microelectromechanical (MEMS) devices.

[0030] The dielectric material 203 is deposited in the open gap 206 by a PEALD method using a diluted reactive gas. Most of the reactive plasma species are consumed at the top of each feature 205 of the structure. The dielectric material 203 is preferentially deposited at the top of the structure. As deposition occurs, the sidewall surface 217 and the bottom surface 215 of the open gap 206 change, where the deposited material forms the boundary of the open gap 206. The growth of each sidewall of the feature 205 eventually meets, closing the feature at 207. As a result, a closed air gap 208 is formed between the features 205.

[0031] In some embodiments, the deposition process is controlled so that the top of air gap 208 is lower than the top of feature 205, such as Figure 2 shown.

[0032] The air gap formed can occupy a majority of the volume of the gap prior to deposition, for example, at least 60%, at least 70%, at least 80%, at least 90%, or at least 90% of the original gap. This can also be characterized as the percent volume occupied by air relative to the total volume occupied by air and solid material between the features. The area of ​​the original gap can be determined by considering the plane connecting the tops of the features to the tops of the gaps.

[0033] For example, to reduce capacitance between metal lines, a majority (eg, at least 80% or 90%) of the original gap can be air. The top of the air gap can be at least about 5 nm below the top of the feature to allow some margin after subsequent planarization.

[0034] In some embodiments, a thin layer of dielectric material is deposited over the entire feature, including on the bottom and lower sidewall surfaces. This encapsulates the air gap and can be deposited during the PEALD process.

[0035] Air gaps can be formed in large gaps. For example, an entry gap (e.g., a slit or memory hole) in a 3D NAND structure may be between 50-100 nm wide and 5-14 microns deep. Dielectric material may be deposited to a depth of about 500 nm, with the gap below it being empty (filled with air). About 500 nm of dielectric material may be deposited on the feature plane. An entry gap in a DRAM structure may be 25-50 nm wide and 300-800 nm deep. Dielectric material may be deposited to a depth of about 30-50 nm, with the gap below it being empty.

[0036] Although the description herein is with respect to air gaps, the methods described herein may be used to form gaps between features occupied by any gas by performing the methods in an appropriate environment.

[0037] In some embodiments, Figure 1One or more etching and / or inhibiting operations are performed during or before the process shown. However, in some embodiments, air gaps are formed using PEALD without any inhibiting or etching operations during and / or before the PEALD process.

[0038] Operation 105 typically uses multiple PEALD cycles. Figure 3 is a manufacturing flow chart for a single PEALD cycle, which can be used as Figure 1 A portion of operation 105 in is implemented to preferentially deposit dielectric material on a top portion of the structure.

[0039] ALD is a technique for sequentially depositing thin layers of material. The ALD process uses a surface-mediated deposition reaction to deposit films layer by layer in a cycle. For example, an ALD cycle may include the following operations: (i) delivery / adsorption of a precursor, (ii) purging the precursor from the chamber, (iii) delivery of a second reactant, and in the PEALD process, plasma ignition, and (iv) purging byproducts from the chamber.

[0040] In one example of an ALD process, a substrate surface containing many surface active sites is exposed to a gas phase distribution of a first precursor (e.g., a silicon-containing precursor) provided in a certain dosage to a chamber containing the substrate. Molecules of the first precursor are adsorbed onto the substrate surface, including chemically adsorbed species and / or physically adsorbed molecules of the first precursor. It should be understood that when a compound is adsorbed onto the substrate surface as described herein, the adsorption layer may include the compound and derivatives of the compound. For example, the adsorption layer of a silicon-containing precursor may include the silicon-containing precursor and derivatives of the silicon-containing precursor. After the first precursor is dosed, the chamber is then evacuated to remove most or all of the remaining first precursor in the gas phase, so that most or only the adsorbed substances remain. In some embodiments, the chamber may not be completely evacuated. For example, the reactor may be vented so that the partial pressure of the first precursor in the gas phase is low enough to moderate the reaction. A second reactant, such as an oxygen-containing gas, is introduced into the chamber so that some of these molecules react with the first precursor adsorbed on the surface. In some processes, the second reactant reacts immediately with the adsorbed first precursor. In other embodiments, the second reactant reacts only with a temporary application of an activation source such as a plasma. The chamber may then be evacuated again to remove unbound second reactant molecules. As described above, in some embodiments, the chamber may not be completely evacuated. Additional ALD cycles may be used to build up film thickness.

[0041] Steering Figure 3In operation 302, the substrate is exposed to a dielectric precursor to adsorb the precursor onto the surface of the feature. This operation may be self-limiting. In some embodiments, the precursor adsorbs less than all active sites on the surface of the feature. The dielectric precursor is typically a silicon-containing precursor, but other dielectric precursors may be used. Useful silicon-containing precursors are further described below.

[0042] In operation 304, the processing chamber is purged to remove any unadsorbed dielectric precursor. In operation 306, the substrate is exposed to a plasma generated by a diluted co-reactant. Examples include oxygen-containing gases such as oxygen (O2) and / or nitrous oxide (N2O) to form an oxide layer; nitrogen (N2) or ammonia (NH3) to form a nitride layer; carbon-containing reactants to form a carbide layer, etc.

[0043] In operation 308, the process chamber is purged to remove byproducts from the reaction between the dielectric precursor and the co-reactant. Operations 302 to 308 may be repeated for multiple cycles to deposit dielectric material to form an air gap as described above. According to various embodiments, any of the process parameters described below may be constant or varied cycle-to-cycle in multiple PEALD cycles.

[0044] It should be noted that the processes described herein are not limited to a particular reaction mechanism. Figure 1-3 The processes described include all deposition processes using sequential exposure to dielectric precursor and conversion plasma, including those processes that are not strictly self-limiting. The processes include sequences in which one or more gases used to generate the plasma are supplied continuously throughout the process with intermittent plasma ignition.

[0045] The co-reactant in operation 105 or 306 is delivered along with more inert gas such as argon (Ar), hydrogen (H2), and / or helium (He) to dilute it. These inert gases are referred to as diluent gases. An exemplary volume flow rate ratio of inert gas to co-reactant ranges from 100:1 to 5:1. Ratios outside this range may be used depending on the topography of the feature. The ratio may be adjusted to control the placement and size of the air gap, and in some embodiments may be 50:1 to 5:1 or 20:1 to 5:1 to obtain a large gap below the top of the feature.

[0046] In addition to diluting the co-reactant gas, the plasma conversion time can be short to limit the reactive species that can diffuse further into the structure. Figure 4An exemplary timing for depositing silicon oxide material to form an air gap is shown. First, in a batching phase, the structure is exposed to a silicon-containing precursor. This is followed by a post-batch purge (PDP) in which an inert purge gas is supplied. As shown, the plasma conversion operation (labeled as radio frequency (RF) / oxidation) is relatively short, with significantly more diluent gas than the supplied oxidant gas. An RF post-purge is then performed. In some embodiments, the purge and diluent gases may include the same gas flow rate. The silicon-containing precursor may also be supplied with an inert gas, but the dilution is significantly lower than the oxidant. In some embodiments, the duration of the batching phase is at least twice the duration of the plasma conversion phase.

[0047] While extreme dilution of the dielectric precursor formulation can be used for non-conformal deposition and for forming air gaps, it tends to result in high within-wafer non-uniformity. The methods described herein using extreme dilution of plasma co-reactants can result in low non-uniformity, for example, less than 5% non-uniformity.

[0048] The air gap size and placement can be controlled. As described above, in some embodiments, the air gap size does not extend above the height of adjacent features. In some embodiments, the air gap is formed as large as possible while keeping the air gap below the top of the feature.

[0049] In some embodiments, forming an air gap in a gap with a smaller critical dimension (CD) may include using a more non-conformal process (e.g., using a higher co-reactant dilution). In addition to the CD, the feature shape also affects the conditions used to form an air gap of a specific size and location. Forming an air gap in a structure with an overhang may use less dilution than a structure with straight sidewalls. This is because the presence of the overhang can cause non-conformality, thereby promoting preferential deposition on the top of the structure and forming an air gap within the structure. See, e.g. Figure 5 , which shows the overhang 515 in the structure before and after the preferential deposition of dielectric material 503 and the formation of air gap 508.

[0050] Conformality and the size and position of the air gap can be controlled by the dilution, chamber pressure, plasma time, plasma power, and the choice of co-reactants. For example, when using O2 as a co-reactant for depositing oxide, any one or more of reducing dilution, increasing pressure, increasing RF time, and increasing RF power makes the deposition more conformal and can be used to reduce the position of the air gap. These process conditions can result in a smaller air gap with more sidewall deposition. Similarly, any one or more of increasing dilution, reducing pressure, reducing RF time, and reducing RF power can make the deposition more non-conformal and can be used to increase the size of the air gap when using O2.

[0051] When using N2O as the oxidant, any one or more of the following: reducing dilution, reducing pressure, reducing RF time, and reducing RF power, makes the deposition more conformal and can be used to reduce the location of the air gap. These process conditions can result in a smaller air gap with more sidewall deposition. Similarly, any one or more of the following: increasing dilution, increasing pressure, increasing RF time, and increasing RF power, makes the deposition more non-conformal and can be used to increase the size of the air gap when using N2O.

[0052] The air gap location and size can also be controlled by the choice of co-reactant. For example, N2O will result in a less conformal deposition than O2 at the same dilution. Mixtures of co-reactants (e.g., O2 and N2O) can be used.

[0053] To deposit the silicon-containing film, one or more silicon-containing precursors may be used. The silicon-containing precursor may react with a co-reactant to form a silicon-containing film (e.g., SiO2, SiN, SiON, SiC, SiOC, etc.). Silicon-containing precursors suitable for use according to the disclosed embodiments include polysilane (H3Si-(SiH2) n -SiH3), wherein n≥0. Examples of silanes are silane (SiH4), disilane (Si2H6), and organosilanes (e.g., methylsilane, ethylsilane, isopropylsilane, tert-butylsilane, dimethylsilane, diethylsilane, di-tert-butylsilane, allylsilane, sec-butylsilane, tert-hexylsilane (thexylsilane), isoamylsilane (isoamylsilane), tert-butyldisilane, di-tert-butyldisilane, etc.).

[0054] Halogen silanes include at least one halogen group and may or may not include hydrogen and / or carbon groups. Examples of halogen silanes are iodosilanes, bromosilanes, chlorosilanes and fluorosilanes. Specific chlorosilanes are tetrachlorosilane, trichlorosilane, dichlorosilane, monochlorosilane, chloroallyl silane, chloromethylsilane, dichloromethylsilane, chlorodimethylsilane, chloroethylsilane, tert-butylchlorosilane, di-tert-butylchlorosilane, chloroisopropylsilane, chloro-sec-butylsilane, tert-butyldiethylchlorosilane, n-hexyldimethylchlorosilane etc.

[0055] Aminosilanes contain at least one nitrogen atom bonded to a silicon atom, but may also contain hydrogen, oxygen, halogens, and carbon. Examples of aminosilanes are mono-, di-, tri-, and tetra-aminosilanes (H3Si(NH2), H2Si(NH2)2, HSi(NH2)3, and Si(NH2)4, respectively) and substituted mono-, di-, tri-, and tetra-aminosilanes, such as tert-butylaminosilane, methylaminosilane, tert-butylsilylamine, di(tert-butylamino)silane (SiH2(NHC(CH3)3)2(BTBAS), tert-butylsilylcarbamate, SiH(CH3)-(N(CH3)2)2, SiHCl-(N(CH3)2)2, (Si(CH3)2NH)3, and the like. A further example of an aminosilane is trisilylamine (N(SiH3)). In some embodiments, aminosilanes having two or more amine groups attached to a central silicon atom may be used. These may cause less damage than aminosilanes having only a single amine group attached.

[0056] Another example of a silicon-containing precursor includes trimethylsilane (3MS); ethylsilane; butylsilane; pentasilane; octylsilane; heptylsilane; hexasilane; cyclotetrasilane; cycloheptylsilane; cyclohexasilane; cyclooctylsilane; cyclopentasilane; 1,4-dioxa-2,3,5,6-tetrasilcyclohexane; diethoxymethylsilane (DEMS); diethoxysilane (DES); dimethoxymethylsilane; dimethoxysilane (DMOS); methyldiethoxysilane (MDES); methyldimethoxysilane (MDMS); octamethoxydodecyloxane (OMODDS); tert-butoxydisilane; tetramethylcyclotetrasiloxane (TMCTS); tetraoxymethylcyclotetrasiloxane (TOMCTS); triethoxysilane (TES); triethoxysiloxane (TRIES); and trimethoxysilane (TMS or TriMOS).

[0057] In some implementations, the silicon-containing precursor may include siloxane or siloxane containing amino groups. In certain embodiments, the siloxane used herein may have a chemical formula X(R 1 ) a Si-O-Si(R 2 ) b Y, wherein a and b are integers from 0 to 2, X and Y can independently be H or NR 3 R 4 , where R 1 , R 2 , R 3 , and R 4 Each of X and Y is hydrogen, a linear alkyl group, a branched alkyl group, a saturated heterocyclic group, an unsaturated heterocyclic group, or a combination thereof. In certain embodiments, when at least one of X or Y is NR 3 R4 When R 3 With R 4 Together with the atoms to which each of them is attached, a saturated heterocyclic compound is formed. In certain embodiments, the silicon-containing precursor is a pentamethylated siloxane containing an amino group, or a dimethylated siloxane containing an amino group. Examples of siloxanes containing amino groups include: 1-diethylamino 1,1,3,3,3,-pentamethyldisiloxane, 1-diisopropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-dipropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-di-n-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-di-sec-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-N-methylethylamino 1,1,3,3,3,-pentamethyldisiloxane disiloxane, 1-N-methylpropylamino-1,1,3,3,3,-pentamethyldisiloxane, 1N-methylbutylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-tert-butylamino-1,1,3,3,3,-pentamethyldisiloxane, 1-piperidinyl-1,1,3,3,3,-pentamethyldisiloxane, 1-dimethylamino-1,1-dimethyldisiloxane, 1-diethylamino-1,1-dimethyldisiloxane, 1-diisopropylamino-1,1-dimethyldisiloxane 1-dipropylamino-1,1-dimethyldisiloxane, 1-di-n-butylamino-1,1-dimethyldisiloxane, 1-di-sec-butylamino-1,1-dimethyldisiloxane, 1-N-methylethylamino-1,1-dimethyldisiloxane, 1-N-methylpropylamino-1,1-dimethyldisiloxane, 1-N-methylbutylamino-1,1-dimethyldisiloxane, 1-piperidinyl-1,1-dimethyldisiloxane, 1-tert-butylamino-1,1-dimethyldisiloxane, 1-dimethyl The invention discloses 1-amino-disiloxane, 1-di-n-butylamino-disiloxane, 1-di-sec-butylamino-disiloxane, 1-N-methylethylamino-disiloxane, 1-N-methylpropylamino-disiloxane, 1-N-methylbutylamino-disiloxane, 1-piperidinyl-disiloxane, 1-tert-butylamino-disiloxane, and 1-dimethylamino-1,1,5,5,5-pentamethyldisiloxane.

[0058] In some embodiments, the flow rate between about 0slm and about 30slm is used to introduce nitrogen (being understood as 0slm and refers to no nitrogen supply). In some embodiments, the flow rate between about 0slm and about 5slm is used to introduce hydrogen (being understood as 0slm and refers to no hydrogen supply).

[0059] The co-reactant is determined in part by the composition of the deposited film. Silicon oxide deposition uses an oxidizing plasma generated, for example, from oxygen (O2), nitrous oxide (N2O), or a combination thereof. Other oxygen-containing compounds, such as water (H2O), may be used.

[0060] Silicon nitride (SiN) can be deposited using N2 plasma, NH3 plasma, or other nitrogen-containing plasmas. In some embodiments, no oxidant is used during SiN deposition. Silicon carbide can be deposited using carbon-containing co-reactants (e.g., reacting silane with methane). Silicon oxynitride, silicon oxycarbide, silicon oxynitride and carbon oxynitride, etc. can be deposited using appropriate co-reactants.

[0061] The co-reactant may also be determined by the degree of conformality it induces during PEALD, as described above.

[0062] Plasma energy may be provided to activate the co-reactants into ions and free radicals and other activated species that react with the adsorbed layer of the adsorbed precursor and any precursor present in the gas phase. In various embodiments, the plasma is an in-situ plasma such that the plasma is formed directly on the substrate surface in the chamber. The in-situ plasma may be between about 0.333 W / cm 2 The power for four 300 mm wafers may range from about 400 W to about 6000 W.

[0063] Examples of chamber pressures may range from 1 to 40 Torr, or 2 to 20 Torr, or 2 to 10 Torr, such as 2 to 6 Torr.

[0064] An example range of plasma conversion (RF) time is 0.01 to 0.3 seconds, or 0.5 to 1.5 seconds, or 0.5 to 1 second. The RF plasma time may alternatively or also be characterized relative to the dielectric precursor batching time. In various embodiments, the dielectric precursor batching time may be at least 2, 3, 4, or 5 times longer than the plasma conversion time.

[0065] An example range of substrate temperature is from 50°C to 650°C.

[0066] The ranges described herein are inclusive of their endpoints.

[0067] Plasma can be generated by applying a radio frequency (RF) field to a gas using two capacitively coupled plates. The plasma is ignited by ionization of the gas between the plates by the RF field, thereby forming free electrons in the plasma discharge region. These electrons are accelerated by the RF field and can collide with gas phase reactant molecules. The collision of these electrons with the reactant molecules can form free radical species that participate in the deposition process. It should be understood that the RF field can be coupled via any suitable electrode.

[0068] After forming the air gap, various operations may be performed. In some embodiments, for example, a capping layer may be deposited on the dielectric material. In some embodiments, the dielectric film may be deposited by plasma enhanced chemical vapor deposition (PECVD). Figure 6 A structure is shown with air gaps 608 formed as described above, wherein a dielectric PECVD film 617 is deposited on dielectric material 603. Due to the PEALD deposition, an indentation 619 centered around the air gap 608 in dielectric material 603 is smoothed. Figure 6 Not shown in the figure, dielectric PECVD film 617 may include dimples centered around dimple 619, but their height may be reduced, for example, by at least 20% to 90% compared to the height in dielectric material 603. Deep dimples may result in uneven amounts of material being removed from the top of the structure during etching and CMP steps, which may result in excessive material being removed from the filled features, creating defects that may affect device performance. Depositing a capping layer such as dielectric PECVD film 617 ensures that the gap remains filled and, during subsequent planarization, the gap remains filled and, as shown in FIG. Figure 6 The resulting planarized dielectric film 621 is shown. In other embodiments, the capping layer can be deposited by thermal CVD. Deposition by CVD (PECVD or thermal CVD) allows for rapid deposition of thick films, which preferentially fills indentations, thereby forming a flatter film, reducing the frequency of defects in subsequent processing. In some operations, the CVD operation is performed in the same chamber as the suppression and ALD operations. This significantly reduces the number of transfer operations and processing tools. Exemplary thickness ranges for the capping layer are In some embodiments, thinner layers may be deposited, e.g.

[0069] For purposes herein, "near" a feature top, near a structure top, or near a gap top means an area in the gap that is within 25% or within 10% of the total depth measured vertically from the top of the feature that forms the gap sidewalls. "Near" a feature bottom means an area in the gap that is within 25% or within 10% of the total depth measured vertically from the feature bottom.

[0070] experiment

[0071] Silicon oxide was deposited into the gaps between features using a PEALD process. During the RF plasma, O2 was the oxidant and was supplied along with 5000 sccm He and 5000 sccm H2. The O2 flow rate was varied while all other deposition parameters were constant. <![CDATA[O2 flow rate]]> 100sccm 200sccm 500sccm 1000sccm Average air gap area <![CDATA[Approximately 370 nm 2 > <![CDATA[Approximately 270 nm 2 > <![CDATA[Approximately 180 nm 2 > <![CDATA[Approximately 150 nm 2 > As the H2:O2 ratio decreases from 50:1 to 10:1, the air gap area decreases. For the 10:1 and 5:1 ratios, all air gaps are below the features. A similar trend is observed using N2O as the oxidant. At the same flow rate, N2O is less conformal than O2, resulting in larger air gaps.

[0072] Silicon oxide was deposited into the gaps between features using a PEALD process. The RF power was varied while keeping all other parameters constant. During the RF plasma, the gas flows were 200 sccm O2, 5000 sccm He, and 5000 sccm H2. HFRF power per station 200W 375W 750W Average air gap area <![CDATA[Approximately 270 nm 2 > <![CDATA[Approximately 230 nm 2 > <![CDATA[Approximately 190 nm 2 >

[0073] As RF power increases, the air gap area decreases and conformality increases.The air gap can be formed at higher plasma powers, with exemplary powers of 200W-3000W for four stations and 300mm wafers. Device

[0074] Figure 7 A schematic diagram of an embodiment of an atomic layer deposition (ALD) processing station 700 having a processing chamber body 702 for maintaining a low pressure environment is depicted. Multiple ALD processing stations 700 can be included in a common low pressure processing tool environment. For example, Figure 7 An embodiment of a multi-station processing tool 700 is depicted. In some embodiments, one or more hardware parameters of the ALD processing station 700 (including the parameters discussed in detail below) can be programmatically adjusted by one or more system controllers 750.

[0075] The ALD processing station 700 is in fluid communication with a reactant delivery system 701a to deliver process gases to a distribution showerhead 706. The reactant delivery system 701a includes a mixing vessel 704 for mixing and / or conditioning process gases for delivery to the showerhead 706. In some embodiments, the process gases may be introduced into the mixing vessel before being introduced into the chamber body 702, for example if a carrier gas is provided. In some embodiments, the process gases may be delivered directly to the chamber body 702. One or more mixing vessel inlet valves 720 may control the introduction of process gases into the mixing vessel 704. These valves may be controlled depending on whether reactant gases, inhibitor gases, or carrier gases are turned on during various operations. In some embodiments, the inhibitor gas may be produced by using an inhibitor liquid and vaporizing it using a heated vaporizer.

[0076] For example, Figure 7 Embodiments include a vaporization point 703, which is used to vaporize liquid reactants to be supplied to a mixing container 704. In some embodiments, the vaporization point 703 can be a heated vaporizer. The saturated reactant vapor produced from such a vaporizer will condense in the downstream delivery pipeline. Incompatible gases exposed to condensed reactants will produce small particles. These small particles may block pipelines, hinder valve operation, contaminate substrates, etc. Some methods for dealing with these problems involve cleaning and / or emptying the delivery pipeline to remove residual reactants. However, cleaning the delivery pipeline will increase the processing station cycle time and reduce the processing station output. Therefore, in some embodiments, the delivery pipeline downstream of the vaporization point 703 can be heat traced. In some embodiments, the mixing container 704 can also be heat traced. In a non-limiting example, the pipeline downstream of the vaporization point 703 has an increased temperature curve, extending from about 100°C to about 150°C at the mixing container 704.

[0077] In some embodiments, a liquid precursor or a liquid reactant (e.g., a silicon-containing precursor) can be vaporized at a liquid injector. For example, a liquid injector can eject a pulse of a liquid reactant into a carrier gas stream upstream of a mixing vessel. In one embodiment, a liquid injector can vaporize a reactant by flashing a liquid from a higher pressure to a lower pressure. In another example, a liquid injector can atomize a liquid into dispersed droplets that are then vaporized in a heated delivery pipe. Smaller droplets can vaporize faster than larger droplets, thereby reducing the delay between liquid injection and completion of vaporization. Faster vaporization can reduce the length of the pipeline downstream of vaporization point 703. In one embodiment, a liquid injector can be loaded directly into a mixing vessel 704. In another embodiment, a liquid injector can be loaded directly into a spray head 706.

[0078] In some embodiments, a liquid flow controller (LFC) (not shown) can be set upstream of the vaporization point 703 to control the mass flow of the liquid for vaporization and delivery to the processing station 700. For example, the LFC can include a thermal mass flow meter (MFM) located downstream of the LFC. Then the plunger valve of the LFC can be adjusted in response to a feedback control signal provided by a proportional integral differential (PID) controller that communicates electrically with the MFM. However, it can take one second or longer to use feedback control to stabilize the liquid flow. This can extend the time of dosing liquid reactants. Therefore, in some embodiments, the LFC can be dynamically switched between feedback control mode and direct control mode. In some embodiments, this can be performed by disabling the sensing tube of the LFC and PID controller.

[0079] The showerhead 706 distributes gases to the substrate 712. For example, in various operations, the showerhead 706 may distribute a silicon-containing precursor gas to the substrate 712, or distribute a purge gas or a carrier gas to the chamber body 702, distribute a co-reactant to the substrate 712, and / or distribute a dilution gas to the substrate 712. Figure 7 In the illustrated embodiment, substrate 712 is positioned below showerhead 706 and is shown resting on pedestal 708. Showerhead 706 may have any suitable shape and may have any suitable number and arrangement of ports for distributing process gases to substrate 712.

[0080] In some embodiments, the microvolume is located below the showerhead 706. Practicing the disclosed embodiments in a microvolume rather than in the entire volume of the process station can reduce reactant exposure and sweep time, can reduce the time to change process conditions (e.g., pressure, temperature, etc.), can limit the exposure of the process station robot to process gases, etc. Exemplary microvolume sizes include, but are not limited to, volumes between 0.1 liters and 2 liters. This also affects productivity yields. In some embodiments, the disclosed embodiments are not performed in a microvolume.

[0081] In some embodiments, the pedestal 708 can be raised or lowered to expose the substrate 712 to the microvolume 707 and / or to change the volume of the microvolume 707. For example, during a substrate transfer phase, the pedestal 708 can be raised to position the substrate 712 within the microvolume 707. In some embodiments, the microvolume 707 can completely surround the substrate 712 and a portion of the pedestal 708 to form an area of ​​high flow impedance.

[0082] Optionally, the pedestal 708 can be lowered and / or raised during portions of the process to adjust process pressure, reactant concentrations, etc. within the microvolume 707. In one case where the process chamber body 702 is maintained at a base pressure during the process, lowering the pedestal 708 can allow the microvolume 707 to be evacuated. Exemplary ratios of microvolume to process chamber volume include, but are not limited to, volume ratios between 1:700 and 1:10. It should be appreciated that in some embodiments, the pedestal height can be programmatically adjusted by a suitable computer controller 750.

[0083] In another case, adjusting the height of the pedestal 708 can allow for changing the plasma density during plasma activation. At the end of a process phase, the pedestal 708 can be lowered during another substrate transfer phase to allow for removal of the substrate 712 from the pedestal 708.

[0084] Although the exemplary microvolume changes described herein involve a height-adjustable pedestal 708, it should be understood that in some embodiments, the position of the showerhead 706 can be adjusted relative to the pedestal 708 to change the volume of the microvolume 707. In addition, it should be understood that the vertical position of the pedestal 708 and / or showerhead 706 can be changed by any suitable mechanism within the scope of the present disclosure. In some embodiments, the pedestal 708 may include a rotation axis for rotating the orientation of the substrate 712. It should be understood that in some embodiments, one or more of these exemplary adjustments can be performed programmatically by one or more appropriate controllers 750.

[0085] The plasma used for the ALD process can be generated by applying a radio frequency (RF) field to the gas using two capacitively coupled plates. The plasma is ignited by the ionization of the gas between the plates by the RF field, thereby forming free electrons in the plasma discharge region. These electrons are accelerated by the RF field and can collide with gas phase reactant molecules. The collision of these electrons with the reactant molecules can form free radical species that participate in the deposition process. It should be understood that the RF field can be coupled via any suitable electrode. Non-limiting examples of electrodes include process gas distribution nozzles and substrate support bases. It should be understood that in addition to the capacitive coupling of the RF field to the gas, the plasma of the ALD process can be formed by one or more suitable methods. In one embodiment, the plasma is a remote plasma, so that the second reactant is ignited in a remote plasma generator upstream of the station and then transported to the station that accommodates the substrate.

[0086] The showerhead 706 and the base 708 are electrically connected to a radio frequency (RF) power supply 714 and a matching network 716 for powering the plasma. In some embodiments, the plasma energy can be controlled by controlling one or more of the processing station pressure, gas concentration and gas partial pressure or gas flow rate, RF source power, RF source frequency and plasma power pulse timing. For example, the RF power supply 714 and the matching network 716 can be operated at any suitable power to form a plasma with a desired ion energy. Examples of suitable power are included above. Similarly, the RF power supply 714 can provide RF power of any appropriate frequency. In some embodiments, the RF power source 714 can be configured to control a high-frequency RF power source and a low-frequency RF power source that are independent of each other. Exemplary low-frequency RF frequencies can include, but are not limited to, frequencies between 0kHz and 500kHz. Exemplary high-frequency RF frequencies can include, but are not limited to, frequencies between 1.8MHz and 2.45GHz, for example, or frequencies greater than about 13.56MHz, or greater than 27MHz, or greater than 40MHz, or greater than 60MHz. It should be understood that any suitable parameters can be adjusted discretely or continuously to provide plasma energy for surface reactions. In a non-limiting example, the plasma power can be intermittently pulsed to reduce ion bombardment with the substrate surface relative to a continuously powered plasma. In an alternative embodiment, a remote plasma generator can be used.

[0087] The ALD processing station 700 can also be used for CVD processes.

[0088] In some embodiments, the plasma can be monitored in situ by one or more plasma monitors. In one case, the plasma power can be monitored by one or more voltage and current sensors (e.g., VI probes). In another case, the plasma density and / or the concentration of the process gas can be measured by one or more optical emission spectroscopy sensors (OES). In some embodiments, one or more plasma parameters can be adjusted programmatically based on the measurement results from such an in-situ plasma monitor. For example, an OES sensor can be used in a feedback loop to provide programmatic control of the plasma power. It should be understood that in some embodiments, other monitors can be used to monitor plasma and other process characteristics. Such monitors may include, but are not limited to, infrared (IR) monitors, acoustic monitors, and pressure sensors.

[0089] In some embodiments, instructions for the controller 750 may be provided via input / output control (IOC) sequencing instructions. In one example, instructions for setting the conditions of a process stage may be included in a corresponding recipe stage of a process recipe. In some cases, the process recipe stages may be arranged in sequence so that all instructions for a process stage are executed simultaneously with the process stage. In some embodiments, instructions for setting one or more reactor parameters may be included in a recipe stage. For example, a first recipe stage may include instructions for setting the flow rate of an inert and / or reactive gas (e.g., a first precursor, such as disilane), instructions for setting a carrier gas (e.g., argon), and time delay instructions for the first recipe stage. A second (subsequent) recipe stage may include instructions for adjusting or stopping the flow rate of an inert and / or reactant gas, instructions for adjusting the flow rate of a carrier gas or a purge gas, and time delay instructions for the second recipe stage. A third recipe stage may include instructions for setting the flow rate of an inert gas, an inhibitor, and / or a reactive gas (which may be the same or different from the gas used in the first recipe stage), instructions for adjusting the flow rate of a carrier gas, and time delay instructions for a third recipe. The fourth recipe stage may include instructions for adjusting or stopping the flow rate of an inert and / or reactive gas (e.g., a second reactant such as nitrogen or a nitrogen- or oxygen-containing gas), instructions for adjusting the flow rate of a carrier gas or a purge gas, and time delay instructions for the fourth recipe stage. It should be understood that these recipe stages may be further subdivided and / or repeated in any suitable manner within the scope of the present disclosure.

[0090] In some embodiments, the pedestal 708 can be temperature controlled by a heater 710. Additionally, in some embodiments, pressure control of the processing station 700 can be provided by a butterfly valve 718. Figure 7 In the embodiment shown in FIG. 7 , butterfly valve 718 regulates the vacuum provided by a downstream vacuum pump (not shown). However, in some embodiments, the pressure control of the process station 700 can also be adjusted by changing the flow rate of one or more gases introduced into the process station 700.

[0091] As described above, one or more processing stations may be included in a multi-station processing tool. Figure 8A schematic view of an embodiment of a multi-station processing tool 800 is shown, having an inbound load lock 802 and an outbound load lock 804, one or both of which may include a remote plasma source. A robot 806 at atmospheric pressure is configured to move a substrate or wafer from a box loaded by a wafer boat 808 into the inbound load lock 802 via an atmospheric port. The substrate is placed on a pedestal 812 in the inbound load lock 802 by the robot 806, the atmospheric port is closed, and the load lock is evacuated. When the inbound load lock 802 includes a remote plasma source, the substrate can be exposed to remote plasma treatment in the load lock before being introduced into the processing chamber 814. In addition, the substrate can also be heated in the inbound load lock 802, for example to remove moisture and adsorbed gases. Next, the chamber transfer port 816 leading to the processing chamber 814 is opened, and another robot 810 places the substrate into the reactor on the pedestal of the first station shown in the reactor for processing. Although in Figure 8 The embodiment depicted in includes a load lock, but it should be understood that in some embodiments, the substrate can be directly introduced into the processing station. In various embodiments, when the substrate is placed on the pedestal 812 by the robot 806, the soaking gas is introduced into the station.

[0092] The depicted processing chamber 814 contains four processing stations, Figure 8 The stations are numbered 1 to 4 in the illustrated embodiment. Each station has a heated susceptor (shown as 818 for station 1) and a gas line inlet. It should be understood that in some embodiments, each processing station can have different or multiple uses. For example, in some embodiments, the processing station can switch between ALD and PEALD process modes. Additionally or alternatively, in some embodiments, the processing chamber 814 may include one or more pairs of matched ALD and plasma enhanced ALD processing stations. Although the depicted processing chamber 814 includes 4 stations, it is to be understood that the processing chamber described in accordance with the present disclosure can have any appropriate number of stations. For example, in some embodiments, the processing chamber can have 5 or more stations, while in other embodiments, the processing chamber can have 3 or fewer stations.

[0093] Figure 8 Also depicted is an embodiment of a system controller 850 for controlling process conditions and hardware states of the processing tool 800. The system controller 850 may include one or more memory devices 856, one or more mass data storage devices 854, and one or more processors 852. The processor 852 may include a CPU or computer, analog and / or digital input / output connections, a stepper motor controller board, etc. In some embodiments, the system controller 850 includes machine-readable instructions for performing operations such as those described herein.

[0094] In some embodiments, the system controller 850 controls all activities of the processing tool 800. The system controller 850 executes system control software 858 stored in the mass storage device 854, loaded into the memory device 856, and executed by the processor 852. Alternatively, the control logic can be hard-coded in the system controller 850. Application-specific integrated circuits, programmable logic devices (such as field programmable gate arrays, or FPGAs), etc. can be used for these purposes. In the following discussion, whether "software" or "code" is used, functionally equivalent hard-coded logic can be used instead. The system control software 858 can include instructions for controlling timing, mixing of gases, gas flow, chamber and / or station pressure, chamber and / or station temperature, substrate temperature, target power level, RF power level, substrate pedestal, chuck and / or pedestal position, and other parameters of a specific process performed by the processing tool 800. The system control software 858 can be configured in any appropriate manner. For example, various processing tool component subroutines or control objects can be written to control the operation of the processing tool components used to perform various processing tool processes. The system control software 858 may be coded in any suitable computer readable programming language.

[0095] In some embodiments, the system control software 858 may include input / output control (IOC) sequencing instructions for controlling the various parameters described above. Other computer software and / or programs associated with the system controller 850 and stored in the mass storage device 854 and / or the memory device 856 may be employed in some embodiments. Examples of programs or program segments for this purpose include substrate positioning programs, process gas control programs, pressure control programs, heater control programs, and plasma control programs.

[0096] The substrate positioning program may contain program code for processing tool components used to load a substrate into the pedestal 818 and control the spacing between the substrate and other parts of the processing tool 800.

[0097] The process gas control program may include code for controlling gas composition (e.g., silicon-containing precursors, co-reactants, dilution and purge gases as described herein) and flow rates, and optionally code for flowing gases into one or more process stations prior to deposition to stabilize the pressure in the process station. The pressure control program may include code for controlling the pressure within a process station by adjusting, for example, a throttle valve in an exhaust system of the process station, gas flow into the process station, and the like.

[0098] The heater control program may contain code for controlling the flow of current to a heating unit for heating the substrate. Alternatively, the heater control program may control the delivery of a heat transfer gas (such as helium) toward the substrate.

[0099] A plasma control program may include code for setting RF power levels applied to process electrodes within one or more processing stations according to embodiments herein.

[0100] The pressure control program may include code for maintaining the pressure within the reaction chamber according to embodiments herein.

[0101] In some embodiments, there may be a user interface associated with the system controller 850. The user interface may include a display screen, a graphical software display of apparatus and / or process conditions, and user input devices such as a pointing device, keyboard, touch screen, microphone, and the like.

[0102] In some embodiments, the parameters adjusted by the system controller 850 may relate to process conditions. Non-limiting examples include process gas composition and flow rate, temperature, pressure, plasma conditions (e.g., RF bias power level), etc. These parameters may be provided to the user in the form of a recipe, which may be entered using the user interface.

[0103] Signals for monitoring the process may be provided from various process tool sensors by analog and / or digital input connections of the system controller 850. Signals for controlling the process may be output through analog and digital output connections of the process tool 800. Non-limiting examples of process tool sensors that may be monitored include mass flow controllers, pressure sensors (e.g., manometers), thermocouples, etc. Appropriately programmed feedback and control algorithms may be used with the data from these sensors to maintain process conditions.

[0104] The system controller 850 may provide program instructions for performing the above-described deposition process. The program instructions may control various process parameters, such as DC power level, RF bias power level, pressure, temperature, etc. The instructions may control these parameters to operate the in-situ deposition of the film stack according to the various embodiments described herein.

[0105] The system controller 850 will typically include one or more memory devices and one or more processors configured to execute instructions so that the apparatus will perform the methods described in accordance with the disclosed embodiments. A machine-readable medium containing instructions for controlling process operations in accordance with the disclosed embodiments may be coupled to the system controller 850.

[0106] In some implementations, the system controller 850 is part of a system that can be part of the above-described embodiments. Such a system can include semiconductor processing equipment that includes one or more processing tools, one or more chambers, one or more platforms for processes, and / or specific process components (wafer pedestals, gas flow systems, etc.). These systems can be integrated with electronic devices for controlling their operations before, during, and after the process of semiconductor wafers or substrates. The electronic device can be referred to as a "controller" that can control various components or subcomponents of one or more systems. Depending on the process conditions and / or system type, the system controller 850 can be programmed to control any process disclosed herein, including the delivery of process gases and / or inhibitor gases, temperature settings (e.g., heating and / or cooling), pressure settings, vacuum settings, power settings, radio frequency (RF) generator settings, RF matching circuit settings, frequency settings, flow rate settings, fluid delivery settings, position and operation settings, wafer transfer in and out of tools connected or docked with specific systems and other transfer tools and / or load locks.

[0107] In general, the system controller 850 can be defined as an electronic device having various integrated circuits, logic, memory, and / or software to receive instructions, issue instructions, control operations, enable cleaning operations, enable endpoint measurements, etc. The integrated circuits can include chips in the form of firmware that store program instructions, digital signal processors (DSPs), chips defined as application specific integrated circuits (ASICs), and / or one or more microprocessors or microcontrollers that execute program instructions (e.g., software). The program instructions can be instructions sent to the system controller 650 in the form of various individual settings (or program files) that define operating parameters for performing a particular process on or for a semiconductor wafer or system. In some embodiments, the operating parameters can be part of a recipe defined by a process engineer to complete one or more process steps during the manufacture of one or more (kinds of) layers, materials, metals, oxides, silicon, silicon dioxide, surfaces, circuits, and / or dies of a wafer.

[0108] In some implementations, the system controller 850 may be part of or coupled to a computer that is integrated with the system, coupled to the system, otherwise networked to the system, or a combination thereof. For example, the system controller 850 may be in the "cloud" or may be all or part of a wafer fab host system that may allow remote access to wafer processes. The computer may enable remote access to the system to monitor the current progress of a manufacturing operation, examine the history of past manufacturing operations, examine trends or performance criteria for multiple manufacturing operations, to change parameters of a current process, set processing steps to follow the current process, or start a new process. In some examples, a remote computer (e.g., a server) may provide a processing recipe to the system via a network (which may include a local network or the Internet). The remote computer may include a user interface that enables input or programming of parameters and / or settings, which are then sent from the remote computer to the system. In some examples, the system controller 850 receives instructions in the form of data that specify parameters for each processing step to be performed during one or more operations. The parameters may be specific to the type of process to be performed and the type of tool that the system controller 850 is configured to interface with or control. Thus, as described above, the system controller 850 can be distributed, for example, by including one or more discrete controllers networked together and working toward a common purpose (e.g., the processes and controls described herein). An example of a distributed controller for such a purpose is one or more integrated circuits on a chamber that communicate with one or more integrated circuits remotely (e.g., at a platform level or as part of a remote computer), which combine to control the process on the chamber.

[0109] Exemplary systems may include, but are not limited to, plasma etching chambers or modules, deposition chambers or modules, spin rinse chambers or modules, metal plating chambers or modules, cleaning chambers or modules, chamfer edge etching chambers or modules, physical vapor deposition (PVD) chambers or modules, chemical vapor deposition (CVD) chambers or modules, ALD chambers or modules, atomic layer etching (ALE) chambers or modules, ion implantation chambers or modules, track chambers or modules, and any other semiconductor processing system that may be associated with or used in the manufacture and / or preparation of semiconductor wafers.

[0110] As described above, depending on one or more processing steps to be performed by the tool, the system controller 850 can communicate with one or more other tool circuits or modules, other tool components, cluster tools, other tool interfaces, adjacent tools, neighboring tools, tools located throughout the factory, a host computer, another controller, or tools used in the transport of materials for transporting wafer containers to and from tool locations and / or load ports in a semiconductor manufacturing facility.

[0111] The apparatus / processes described herein can be used in conjunction with photolithographic patterning tools or processes, e.g., for preparing or manufacturing semiconductor devices, displays, LEDs, photovoltaic panels, etc. Typically, though not necessarily, these tools / processes will be used or operated together in a common manufacturing facility. Photolithographic patterning of films typically involves some or all of the following operations, each of which enables multiple available tools: (1) coating a workpiece, i.e., substrate, with photoresist using a spin coating or spray coating tool; (2) curing the photoresist using a hot plate or oven or UV curing tool; (3) exposing the photoresist to visible light or ultraviolet light or x-rays using a tool such as a wafer stepper; (4) developing the resist to selectively remove the resist and thereby pattern it using a tool such as a wet bench; (5) transferring the resist pattern to an underlying film or workpiece using a dry or plasma assisted etching tool; and (6) removing the resist using a tool such as an RF or microwave plasma resist stripper. in conclusion

[0112] Although the above embodiments have been described in some detail for the purpose of clarity of understanding, it is apparent that certain variations and modifications may be implemented within the scope of the appended claims. It should be noted that there are many alternative ways of implementing the processes, systems and devices of the embodiments of the present invention. Therefore, the embodiments of the present invention should be considered illustrative rather than restrictive, and the embodiments are not limited to the details given herein.

Claims

1. A method comprising: providing a structure including features and an open gap between the features, the open gap including sidewalls and a bottom surface; as well as Perform multiple plasma enhanced atomic layer deposition (PEALD) cycles, each cycle consisting of: a) exposing the structure to a dose of a silicon-containing precursor to allow the silicon-containing precursor to adsorb on the sidewalls and bottom surface of the open gap; as well as b) exposing the adsorbed silicon-containing precursor to a plasma generated by a process gas including a co-reactant and one or more dilution gases to cause the co-reactant to react with the adsorbed silicon-containing precursor and form a dielectric material, wherein the dielectric material is preferentially formed near the top of the open gap, wherein the volume flow rate ratio of the one or more dilution gases to the co-reactant is at least 5:

1. 2 . The method of claim 1 , further comprising closing the open gaps with a deposited dielectric material to form closed air gaps between the features. The method of claim 2 , wherein a top of the enclosed air gap is lower than a top of the feature.

4. The method of claim 2, wherein a top of the enclosed air gap is at least 5 nanometers lower than a top of the feature.

5. The method of claim 1 further comprising purging a chamber housing the structure between steps (a) and (b).

6. The method of claim 1, wherein the volume flow rate ratio of the one or more diluent gases to the co-reactants is at least 10:

1.

7. The method of claim 1, wherein the volume flow rate ratio of the one or more diluent gases to the co-reactants is at least 20:

1.

8. The method of claim 1, wherein the volume flow rate ratio of the one or more dilution gases to the co-reactants is between 5:1 and 50:

1.

9. The method of claim 1, wherein the co-reactant is an oxygen-containing gas.

10. The method of claim 1, wherein the co-reactant is nitrous oxide (N2O) or oxygen (O2).

11. The method of claim 1, wherein the co-reactants are O2 and N2O.

12. The method of claim 1, wherein the co-reactant is nitrogen (N2).

13. The method of claim 1, wherein the duration of (a) in each cycle is at least twice the duration of (b).

14. The method of claim 2, wherein the open gap has a first area and the closed air gap occupies at least 80% of the first area.

15. The method of claim 14, wherein the enclosed air gap occupies at least 90% of the first area.

16. A method comprising: providing a structure including features and an open gap between the features, the open gap having a first area and including sidewalls and a bottom surface; as well as performing a plurality of plasma enhanced atomic layer deposition (PEALD) cycles to preferentially deposit a dielectric material on top of the open gaps to form closed air gaps between the features, each cycle comprising: a) exposing the structure to a dose of a silicon-containing precursor such that the silicon-containing precursor is adsorbed on the sidewalls and bottom surface of the open gap; and b) exposing the adsorbed silicon-containing precursor to a plasma generated from a process gas comprising a co-reactant and one or more diluent gases so that the co-reactant reacts with the adsorbed silicon-containing precursor and forms a dielectric material, The closed air gap is formed without etching or inhibiting operations, and the closed air gap occupies at least 80% of the first area.

17. The method of claim 16, wherein the enclosed air gap occupies at least 90% of the first area.

18. The method of claim 16, wherein the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 10:

1.

19. The method of claim 16, wherein the volume flow rate ratio of the one or more dilution gases to the co-reactants is at least 20:1.

Citation Information

Cited By

  • Atomic layer deposition process and structure for forming air gap

    CN121023459A