Contact formation process for CMOS devices

By performing pre-cleaning, selective deposition and removal of contact layers in semiconductor devices, the problem of structure damage caused by epitaxial layer formation is solved, and a high-efficiency and damage-free contact layer formation is achieved in CMOS devices. Improves manufacturing manufacturability and performance.

CN118891712APending Publication Date: 2024-11-01APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028968.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-03-20
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In semiconductor devices, forming epitaxial layer contacts with silicon-containing materials pose a risk of damaging the semiconductor structure, especially in CMOS devices, conventional hard masking and etching treatments can damage the spacer layer, gate cover layer or epitaxial growth layer.

Method used

Pre-cleaning treatment is performed using exposed surfaces forming multiple semiconductor regions on the substrate, followed by selective epitaxial deposition and patterning treatments in openings in the dielectric layer to form and remove the contact layer to ensure that existing without damaging In the case of structure, a contact layer is formed. The method includes pre-cleaning, selective deposition and selective removal treatments in the processing chamber, controlling the formation and removal of the contact layer using plasma-assisted dry etching technology and a remote plasma system.

Benefits of technology

A method and system for forming a contact layer in a semiconductor structure is realized, which avoids damage to the existing structure and improves the manufacturability and performance of CMOS devices, especially the formation of epitaxial layers on silicon or silicon germanium materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118891712A_ABST
    Figure CN118891712A_ABST
Patent Text Reader

Abstract

A method of forming a contact layer in a semiconductor structure includes performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate, where the exposed surfaces of the plurality of first and second semiconductor regions are each disposed within an opening formed in a dielectric layer, the dielectric layer is arranged above the substrate; performing a first selective epitaxial deposition process to form a first contact layer on the exposed surface of the first semiconductor region and a second contact layer on the exposed surface of the second semiconductor region; performing a patterning process to form a patterned stack, where the patterned stack includes a patterned layer including an opening formed over a first contact layer disposed within each opening in the dielectric layer and a portion of the patterned layer disposed over each second contact layer disposed within each opening in the dielectric layer; and performing a selective removal process to selectively remove the first contact layer from the plurality of first semiconductor regions, the dielectric layer, and the patterned layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments described herein relate generally to semiconductor device fabrication and, more particularly, to systems and methods for forming contacts within semiconductor structures. Background Art

[0002] Multi-gate metal oxide semiconductor field effect transistors (MOSFETs), such as complementary metal oxide semiconductor (CMOS) devices, pose challenges to manufacturability due to their three-dimensional (3D) design and small size. In advanced CMOS devices, an epitaxial layer of silicon-containing material (e.g., boron-doped p-type silicon germanium or phosphorus-doped n-type silicon) formed at the bottom of the trench contact is often used to reduce the contact resistivity to 10 -9 Ωꞏcm 2 range and achieve the performance required by advanced CMOS technology.

[0003] However, such epitaxial layer formation and patterning, for example, using a hard mask to protect the n-MOS region or the p-MOS region, may damage various portions of the CMOS device, such as spacers, gate capping layers, or epitaxial growth layers.

[0004] Thus, there is a need for methods and systems that can form contacts including an epitaxial layer of silicon-containing material at selected portions of a semiconductor device. Summary of the invention

[0005] An embodiment of the present disclosure provides a method for forming a contact layer in a semiconductor structure. The method includes: performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate, wherein the exposed surfaces of the plurality of first and second semiconductor regions are each disposed in an opening formed in a dielectric layer disposed above the substrate; performing a first selective epitaxial deposition process to form a first contact layer on the exposed surface of the first semiconductor region and a second contact layer on the exposed surface of the second semiconductor region; performing a patterning process to form a patterned stack, wherein the patterned stack includes a patterned layer, the patterned layer includes an opening formed above the first contact layer disposed in each opening disposed in the dielectric layer, and a portion of the patterned layer disposed above each second contact layer disposed in each opening disposed in the dielectric layer; and performing a selective removal process to selectively remove the first contact layer from the plurality of first semiconductor regions, the dielectric layer, and the patterned layer.

[0006] An embodiment of the present disclosure provides a method for forming a contact layer in a semiconductor structure. The method includes: performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate, wherein the exposed surfaces of the plurality of first and second semiconductor regions are each disposed within an opening formed in a dielectric layer disposed above the substrate; performing a first selective epitaxial deposition process to simultaneously form a first contact layer having a first thickness on the exposed surfaces of the first semiconductor regions, and forming a second contact layer having a second thickness on the exposed surfaces of the second semiconductor regions, wherein the second thickness is greater than the first thickness; and performing a selective removal process to selectively remove the first contact layer and the second contact layer from the plurality of first semiconductor regions and the dielectric layer until the first contact layer is substantially removed from the first semiconductor region and a portion of the second contact layer remains on the second semiconductor region.

[0007] An embodiment of the present disclosure provides a processing system, including a first processing chamber, a second processing chamber, a third processing chamber, and a system controller, wherein the system controller is configured to: perform a pre-cleaning process on exposed surfaces of multiple first semiconductor regions and multiple second semiconductor regions formed on a substrate in the first processing chamber; perform a first selective deposition process in the second processing chamber to epitaxially form a first contact layer on the exposed surfaces of the first semiconductor regions and epitaxially form a second contact layer on the exposed surfaces of the second semiconductor regions of the substrate; and perform a selective removal process in the third processing chamber to selectively remove the first contact layer from the first semiconductor regions. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] In order to be able to understand in detail the manner in which the above-mentioned features of the present disclosure are used, a more particular description of the present disclosure briefly summarized above may be obtained by reference to the implementation, some of which are shown in the accompanying drawings. It will be noted, however, that the accompanying drawings illustrate only typical embodiments of the present disclosure and are not to be considered limiting of its scope, as the present disclosure may admit to other equally effective embodiments.

[0009] 1 is a schematic top view of a multi-chamber processing system according to one or more embodiments of the present disclosure.

[0010]

[0026] Figure 2A is a cross-sectional view of a processing chamber according to one or more embodiments.

[0011] FIG. 2B is an enlarged view of a portion of the processing chamber of FIG. 2A .

[0012] 3 is a cross-sectional view of a processing chamber according to one or more embodiments.

[0013] 4 is a cross-sectional view of a processing chamber according to one or more embodiments.

[0014] 5 depicts a process flow diagram of a method of forming a contact layer in a semiconductor structure according to a first embodiment of the present disclosure.

[0015] 6A , 6B, 6C, 6D, 6E, 6F, and 6G are cross-sectional views of a portion of a semiconductor structure corresponding to respective states of the method of FIG. 5 .

[0016] 7 depicts a process flow diagram of a method of forming a contact layer in a semiconductor structure according to a second embodiment of the present disclosure.

[0017] 8A , 8B, 8C, 8D, and 8E are cross-sectional views of a portion of a semiconductor structure corresponding to respective states of the method of FIG. 7 .

[0018] To facilitate understanding, identical reference numerals have been used, where possible, to identify identical elements that are common to the figures. It is contemplated that elements and features of one embodiment may be beneficially incorporated in other embodiments without further recitation. DETAILED DESCRIPTION

[0019] Embodiments described herein provide methods and systems for forming contacts comprising an epitaxial layer of silicon-containing material (e.g., boron-doped p-type silicon germanium or phosphorus-doped n-type silicon) at selected portions of a structure used to form a CMOS device (e.g., on an exposed surface of a layer of silicon or silicon germanium). The methods and systems may be particularly useful for selectively forming an epitaxial layer comprising silicon germanium on an exposed surface of a silicon germanium material within an opening or feature (e.g., a contact trench) formed in a dielectric layer in a semiconductor structure having a region comprising silicon, a region comprising silicon germanium, and a dielectric layer formed thereover. Unlike conventional processes that require the formation of a hard mask and various etching and patterning processing steps (which often damage the semiconductor structures being manufactured (e.g., spacers, gate caps, etc.)) to form contacts, the processes described herein are configured to form contacts without damaging these previously formed semiconductor structures.

[0020] FIG. 1 is a schematic top view of a multi-chamber processing system 100 according to one or more embodiments of the present disclosure. The processing system 100 generally includes a factory interface 102, load lock chambers 104, 106, transfer chambers 108, 110 with corresponding transfer robots 112, 114, holding chambers 116, 118, and processing chambers 120, 122, 124, 126, 128, 130. As described in detail herein, substrates in the processing system 100 can be processed in each chamber and transferred between each chamber without exposing the substrate to an ambient environment outside the processing system 100 (e.g., such as an atmospheric ambient environment that may exist in a factory). For example, substrates can be processed in each chamber maintained at a low pressure (e.g., less than or equal to about 300 Torr) or a vacuum environment and transferred between each chamber without breaking the low pressure or vacuum environment between each process performed on the substrate in the processing chamber 100. Thus, the processing system 100 can provide an integrated solution for some processing of substrates.

[0021] Examples of treatment systems that may be suitably modified according to the teachings provided herein include Endura ® 、Producer ® or Centura ® An integrated processing system or other suitable processing system is commercially available from Applied Materials, Inc., located in Santa Clara, Calif. It is contemplated that other processing systems, including those from other manufacturers, may be adapted to benefit from the aspects described herein.

[0022] In the example shown in FIG1 , the factory interface 102 includes a docking station 132 and a factory interface robot 134 to facilitate the transfer of substrates. The docking station 132 is adapted to receive one or more front opening unified pods (FOUPs) 136. In some examples, each factory interface robot 134 generally includes a blade 138 disposed on one end of the corresponding factory interface robot 134, adapted to transfer substrates from the factory interface 102 to the load lock chambers 104, 106.

[0023] The load lock chambers 104, 106 have respective ports 140, 142 coupled to the factory interface 102 and respective ports 144, 146 coupled to the transfer chamber 108. The transfer chamber 108 further has respective ports 148, 150 coupled to the holding chambers 116, 118 and respective ports 152, 154 coupled to the processing chambers 120, 122. Similarly, the transfer chamber 110 has respective ports 156, 158 coupled to the holding chambers 116, 118 and respective ports 160, 162, 164, 166 coupled to the processing chambers 124, 126, 128, 130. The ports 144, 146, 148, 150, 152, 154, 156, 158, 160, 162, 164, 166 may be, for example, slit valve openings having slit valves for passing substrates therethrough by the transfer robots 112, 114 and for providing a seal between the respective chambers to prevent gas from passing therethrough. When any port is opened for transferring a substrate therethrough, the port is otherwise closed.

[0024] The load lock chambers 104, 106, the transfer chambers 108, 110, the holding chambers 116, 118, and the processing chambers 120, 122, 124, 126, 128, 130 may be fluidly coupled to a gas and pressure control system (not specifically shown). The gas and pressure control system may include one or more gas pumps (e.g., turbo pumps, cryopumps, roughing pumps), gas sources, various valves, and conduits fluidly coupled to the various chambers. In operation, the factory interface robot 134 transfers the substrate from the FOUP 136 through the port 140 or 142 to the load lock chamber 104 or 106. The gas and pressure control system then evacuates the load lock chamber 104 or 106. The gas and pressure control system further maintains the transfer chambers 108, 110 and the holding chambers 116, 118 to have an internal low pressure or vacuum environment (which may include an inert gas). Thus, evacuating the load lock chamber 104 or 106 facilitates transferring substrates between, for example, the atmospheric environment of the factory interface 102 and the low pressure or vacuum environment of the transfer chamber 108 .

[0025] With the substrate in the already evacuated load lock chamber 104 or 106, the transfer robot 112 transfers the substrate from the load lock chamber 104 or 106 into the transfer chamber 108 through the port 144 or 146. The transfer robot 112 can then transfer the substrate to and / or between any of the processing chambers 120, 122 through the respective ports 152, 154 for processing, and transfer the substrate to the holding chambers 116, 118 through the respective ports 148, 150 for holding to await further transfer. Similarly, the transfer robot 114 can access substrates in the holding chamber 116 or 118 through the port 156 or 158, and can transfer the substrate to any of the processing chambers 124, 126, 128, 130 and / or between any of these processing chambers for processing through the corresponding port 160, 162, 164, 166, and transfer the substrate to the holding chamber 116, 118 for holding to await further transfer through the corresponding port 156, 158. The transfer and holding of substrates within and between the various chambers can be in a low pressure or vacuum environment provided by a gas and pressure control system.

[0026] Processing chambers 120, 122, 124, 126, 128, 130 may be any suitable chamber for processing substrates. In some examples, processing chamber 120 may be capable of performing an etching process, processing chamber 122 may be capable of performing a cleaning process, processing chamber 124 may be capable of performing a selective removal process, and processing chambers 126, 128, 130 may be capable of performing a corresponding epitaxial growth process. Processing chamber 120 may be a Selectra state etch chamber available from Applied Materials, Inc., Santa Clara, California. Processing chamber 122 may be a SiCoNi pre-clean chamber available from Applied Materials, Inc., Santa Clara, California. Processing chambers 126, 128, or 130 may be a Centura Asia Santa Clara chamber available from Applied Materials, Inc., Santa Clara, California.

[0027] The system controller 168 is coupled to the processing system 100 for controlling the processing system 100 or components thereof. For example, the system controller 168 can control the operation of the processing system 100 using direct control of the chambers 104, 106, 108, 110, 116, 118, 120, 122, 124, 126, 128, 130 of the processing system 100 or by controlling controllers associated with the chambers 104, 106, 108, 110, 116, 118, 120, 122, 124, 126, 128, 130. In operation, the system controller 168 enables data collection and feedback from the respective chambers to coordinate the performance of the processing system 100.

[0028] The system controller 168 typically includes a central processing unit (CPU) 170, a memory 172, and support circuits 174. The CPU 170 may be one of any form of general purpose processor that may be used in an industrial environment. The memory 172 or non-transitory computer readable medium may be accessed by the CPU 170 and may be one or more of a memory such as a random access memory (RAM), a read-only memory (ROM), a floppy disk, a hard disk, or any other form of digital storage device (local or remote). The support circuits 174 are coupled to the CPU 170 and may include a cache, a clock circuit, an input / output subsystem, a power supply, and the like. The various methods disclosed herein may be implemented by the CPU 170 executing computer instruction codes (e.g., as software routines) stored in the memory 172 (or in the memory of a particular processing chamber), typically under the control of the CPU 170. When the computer instruction codes are executed by the CPU 170, the CPU 170 controls the chamber to perform processing according to the various methods.

[0029] Other processing systems may employ other configurations. For example, more or fewer processing chambers may be coupled to the transfer device. In the example shown, the transfer device includes transfer chambers 108, 110 and holding chambers 116, 118. In other examples, more or fewer transfer chambers (e.g., one transfer chamber) and / or more or fewer holding chambers (e.g., no holding chambers) may be implemented as a transfer device in a processing system.

[0030] Figure 2A is a cross-sectional view of a processing chamber 200 suitable for performing a pre-cleaning process as described in detail below according to one or more embodiments. The processing chamber 200 may be the processing chamber 122 shown in Figure 1. Figure 2B is an enlarged view of a portion of the processing chamber 200 of Figure 2A.

[0031] The processing chamber 200 can be particularly useful for performing thermal or plasma-based cleaning processes and / or plasma-assisted dry etching processes. The processing chamber 200 includes a chamber body 202, a lid assembly 204, and a support assembly 206. The lid assembly 204 is disposed at an upper end of the chamber body 202, and the support assembly 206 is at least partially disposed within the chamber body 202. A vacuum system can be used to remove gases from the processing chamber 200. The vacuum system includes a vacuum pump 208 coupled to a vacuum port 210 disposed in the chamber body 202. The processing chamber 200 also includes a controller 212 for controlling the process within the processing chamber 200.

[0032] The lid assembly 204 includes a stack of components adapted to provide precursor gas and / or plasma to a processing region 214 within the processing chamber 200. A first plate 216 is coupled to a second plate 218. A third plate 220 is coupled to the second plate 218. The lid assembly 204 may be connected to a power source (not shown) for supplying plasma to a conical cavity 222 formed in the lid assembly 204. The lid assembly 204 may also be connected to a remote plasma source 224 that generates plasma upstream of the lid stack. The remote plasma cavity (e.g., the processing region 214, the first plate 216, and the second plate 218 in FIGS. 2A-2B) is coupled to a gas source 226 (or, in the absence of a remote plasma source 224, the gas source 226 is directly coupled to the lid assembly 204). The gas source 226 may include a gas source adapted to provide helium, argon, or other inert gas. In some configurations, the gas provided by the gas source 226 may be ignited into a plasma that is provided to the lid assembly 204 using the remote plasma source 224. In an alternative embodiment, the gas source 226 can provide a process gas that can be activated by the remote plasma source 224 before being introduced to the surface of the substrate disposed within the processing chamber 200. Referring to FIG. 2B, the tapered chamber 222 has an opening 228 that allows the formed plasma to flow from the remote plasma source 224 to the volume 230 formed in the fourth plate 232 of the lid assembly 204.

[0033] In some configurations of the lid assembly 204, plasma is generated within the conical chamber 222 by applying energy delivered from a plasma source. In one example, energy may be provided by biasing the lid assembly 204 to capacitively couple RF, VHF, and / or UHF energy to the gas located in the conical chamber 222. In this configuration of the lid assembly 204, the remote plasma source 224 may not be used or may not be mounted within the lid assembly 204.

[0034] The central conduit 234 formed in the fourth plate 232 is adapted to provide plasma-generated species provided from the volume 230 to a mixing chamber 238 formed in a sixth plate 240 of the lid assembly 204 through the fifth plate 236. The central conduit 234 communicates with the mixing chamber 238 through an opening 242 in the fifth plate 236. The opening 242 may have a diameter that is less than, greater than, or the same as the diameter of the central conduit 234. In the embodiment of FIG. 2B , the opening 242 has the same diameter as the central conduit 234.

[0035] The fourth plate 232 also includes inlets 244 and 246 adapted to provide gas to the mixing chamber 238. The inlet 244 is coupled to a first gas source 248 and the inlet 246 is coupled to a second gas source 250. The first gas source 248 and the second gas source 250 may include a process gas and an inert gas used as a carrier gas, for example, an inert gas such as argon and / or helium. The first gas source 248 may include ammonia (NH3) and argon (Ar). The second gas source 250 may contain a fluorine-containing gas, a hydrogen-containing gas, or a combination thereof. In one example, the second gas source 250 may contain hydrogen fluoride (HF) and argon (Ar).

[0036] As shown in FIG. 2B , in some configurations, the inlet 244 is coupled to the mixing chamber 238 through the cylindrical passage 252 (shown in shaded form) and the hole 254 formed in the fifth plate 236. The inlet 246 is coupled to the mixing chamber 238 through the cylindrical passage 256 (shown in shaded form) and the hole 258 formed in the fifth plate 236. The size of the holes 254, 258 formed in the fifth plate 236 is generally adjusted so that they can achieve uniform flow of gas provided from their respective gas sources 248, 250 into the mixing chamber 238. In one configuration, the hole 258 has a diameter that is less than the opening width defined by the opposing sidewalls of the cylindrical passage 256 formed in the fourth plate 232. The holes 258 are generally distributed circumferentially around the centerline of the cylindrical passage 256 to provide uniform fluid flow into the mixing chamber 238. In one configuration, the holes 254 have a diameter that is smaller than the width of the opening defined by opposing sidewalls of the cylindrical passage 252 formed in the fourth plate 232. The holes 254 are generally distributed circumferentially about the centerline of the cylindrical passage 252 to provide uniform fluid flow into the mixing chamber 238.

[0037] The respective fluid flow paths provided by the inlets 244 and 246 transversely pass through the fourth plate 232, turn to the fifth plate 236 and pass through the fifth plate 236 to reach the mixing chamber 238. The lid assembly 204 also includes a seventh plate or first gas distributor 260, which may be a gas distribution plate, such as a showerhead, wherein the various gases mixed in the lid assembly 204 flow through the through-holes 262 formed therein. The through-holes 262 are in fluid communication with the mixing chamber 238 to provide a flow path from the mixing chamber 238 through the first gas distributor 260. Returning to FIG. 2A, a blocking plate 264 and a gas distribution plate (such as a second gas distributor 266, which may be a gas distribution plate, such as a showerhead) are disposed below the lid assembly 204.

[0038] Alternatively, a different cleaning process may be used to clean the substrate surface. For example, a remote plasma containing helium (He) and ammonia (NH3) may be introduced into the processing chamber 200 through the lid assembly 204, while ammonia (NH3) may be injected directly into the processing chamber 200 through a separate gas inlet 268 disposed at a side of the chamber body 202 and coupled to a gas source (not shown).

[0039] The support assembly 206 may include a substrate support 270 to support a substrate 272 thereon during processing. The substrate support 270 may be coupled to an actuator 274 via a shaft 276 that extends through a centrally located opening formed in the bottom of the chamber body 202. The actuator 274 may be flexibly sealed to the chamber body 202 via a bellows (not shown) that prevents vacuum leakage around the shaft 276. The actuator 274 allows the substrate support 270 to be moved vertically within the chamber body 202 between a processing position and a loading position. The loading position is slightly lower than the opening of a channel (not shown) formed in the sidewall of the chamber body 202.

[0040] The substrate support 270 has a flat, or substantially flat, substrate support surface for supporting a substrate 272 to be processed thereon. The substrate support 270 can be moved vertically within the chamber body 202 by an actuator 274, which is coupled to the substrate support 270 by a shaft 276. For some steps, the substrate support 270 can be raised to a position in close proximity to the lid assembly 204 to control the temperature of the substrate 272 being processed. Thus, the substrate 272 can be heated via radiation emitted from the second gas distributor 266 or another radiation source, or by convection or conduction from the second gas distributor 266 through an intermediate gas. In some processing steps, the substrate can be placed on lift pins 278 to perform additional thermal processing steps, such as performing an annealing step.

[0041] 3 is a cross-sectional view of a processing chamber 300 suitable for performing an epitaxial (Epi) deposition process as described in detail below, according to one or more embodiments. The processing chamber 300 may be the processing chamber 126, 128, or 130 shown in FIG.

[0042] The processing chamber 300 includes a housing structure 302 made of a process resistant material such as aluminum or stainless steel, for example 316L stainless steel. The housing structure 302 encloses various functional elements of the processing chamber 300, such as a quartz chamber 304, which includes an upper quartz chamber 306 and a lower quartz chamber 308, containing a processing volume 310. Reactive species are provided to the quartz chamber 304 through a gas distribution assembly 312, and process byproducts are removed from the processing volume 310 through an outlet port 314 that is generally in communication with a vacuum source (not shown).

[0043] The substrate support 316 is adapted to receive a substrate 318 that is transferred to the processing volume 310. The substrate support 316 is disposed along a longitudinal axis 320 of the processing chamber 300. The substrate support 316 may be made of a ceramic material or a graphite material coated with a silicon material (such as silicon carbide), or other processing resistant material. Reactive species from the precursor reactive material are applied to a surface 322 of the substrate 318, and byproducts may subsequently be removed from the surface 322 of the substrate 318. Heating of the substrate 318 and / or the processing volume 310 may be provided by a radiation source, such as an upper lamp module 324A and a lower lamp module 324B.

[0044] In one embodiment, the upper lamp module 324A and the lower lamp module 324B are infrared (IR) lamps. Non-thermal energy from the lamp modules 324A and 324B travels through the upper quartz window 326 of the upper quartz chamber 306 and through the lower quartz window 328 of the lower quartz chamber 308. Cooling gas for the upper quartz window 306 (if required) enters through the inlet 330 and exits through the outlet 332. Precursor reactant materials, as well as diluent, purge and exhaust gases for the processing chamber 300, enter through the gas distribution assembly 312 and exit through the outlet port 314. Although the upper quartz window 326 is illustrated as curved or convex, the upper quartz window 326 can be flat or concave because the pressure on both sides of the upper quartz window 326 is substantially the same (i.e., atmospheric pressure).

[0045] The low wavelength radiation in the processing volume 310 used to excite reactive species and assist in adsorption of reactants on the surface 322 of the substrate 318 and desorption of processing byproducts from the surface 322 of the substrate 318 typically varies from about 0.8 μm to about 1.2 μm, for example, between about 0.95 μm and about 1.05 μm, for example, providing various wavelength combinations depending on the composition of the film being epitaxially grown.

[0046] The component gases enter the processing volume 310 via the gas distribution assembly 312. As generally illustrated by the flow path 334, the gases flow from the gas distribution assembly 312 and exit through the outlet port 314. The combination of component gases used to clean / passivate the substrate surface, or to form a positive epitaxially grown silicon and / or germanium containing film, is typically mixed before entering the processing volume 310. The total pressure in the processing volume 310 can be adjusted by a valve (not shown) on the outlet port 314. At least a portion of the interior surface of the processing volume 310 is covered by a liner 336. In one embodiment, the liner 336 comprises an opaque quartz material. In this way, the chamber wall is insulated from the heat in the processing volume 310.

[0047] The temperature of the surfaces in the processing volume 310 may be controlled within a temperature range of about 200° C. to about 600° C., or greater, by the flow of cooling gas entering through the inlet 330 and exiting through the outlet 332 in combination with radiation from the upper lamp module 324A located above the upper quartz window 326. The temperature in the lower quartz chamber 308 may be controlled within a temperature range of about 200° C. to about 600° C., or greater, by adjusting the speed of a blower unit, not shown, and by radiation from the lower lamp module 324B disposed below the lower quartz chamber 308. The pressure in the processing volume 310 may be between about 0.1 Torr and about 600 Torr, such as between about 5 Torr and about 30 Torr.

[0048] The temperature at the surface 322 of the substrate 318 can be controlled by adjusting the power of the lower lamp module 324B in the lower quartz chamber 308, or by adjusting the power of both the upper lamp module 324A covering the upper quartz window 326 and the lower lamp module 324B in the lower quartz chamber 308. The power density in the processing volume 310 can be about 40 W / cm 2 to about 400 W / cm 2 between, such as about 80 W / cm 2 to about 120 W / cm 2 .

[0049] In one aspect, the gas distribution assembly 312 is disposed orthogonally to the longitudinal axis 320 of the processing chamber 300 or substrate 318, or in a radial direction 338 relative to the longitudinal axis 320 of the processing chamber 300 or substrate 318. In this orientation, the gas distribution assembly 312 is adapted to flow the processing gas in the radial direction 338 across or parallel to the surface 322 of the substrate 318. In one processing application, the processing gas is preheated at the point of introduction into the processing chamber 300 to initiate preheating of the gas, and / or to break specific bonds in the gas prior to introduction into the processing volume 310. In this manner, the surface reaction kinetics can be modified independently of the thermal temperature of the substrate 318.

[0050] In operation, precursors for forming blanket or selective epitaxial films of silicon (Si) and silicon germanium (SiGe) are provided to the gas distribution assembly 312 from one or more gas sources 340A and 340B. IR lamps 342 (only one is shown in FIG. 3 ) may be used to heat the precursors within the gas distribution assembly 312 and along the flow path 334. The gas sources 340A, 340B may be coupled to the gas distribution assembly 312 in a manner suitable for facilitating introduction into regions within the gas distribution assembly 312, such as radially outer regions and radially inner regions between the outer regions when viewed from a top plan view. The gas sources 340A, 340B may include valves (not shown) to control the rate of introduction into the regions.

[0051] Gas sources 340A, 340B may include silicon precursors, such as silanes, including silane (SiH4), disilane (Si2H6), dichlorosilane (SiH2Cl2), hexachlorodisilane (Si2Cl6), dibromosilane (SiH2Br2), higher order silanes, derivatives thereof, and combinations thereof. Gas sources 340A, 340B may also include germanium-containing precursors, such as germanium (GeH4), digermane (Ge2H6), germanium tetrachloride (GeCl4), dichlorogermane (GeH2Cl2), derivatives thereof, and combinations thereof. Precursors containing silicon and / or germanium may be used in combination with hydrogen chloride (HCl), chlorine (Cl2), hydrogen bromide (HBr), and combinations thereof. In one or both of gas sources 340A, 340B, gas sources 340A, 340B may include one or more of silicon- and germanium-containing precursors.

[0052] The precursor material in this excited state enters the processing volume 310 through openings or holes 344 (only one of which is shown in FIG. 3 ) in a perforated plate 346, which in one embodiment is a quartz material having holes 344 formed therethrough. The perforated plate 346 is transparent to IR energy and may be made of a transparent quartz material. In other embodiments, the perforated plate 346 may be any material that is transparent to IR energy and is resistant to process chemicals and other process chemicals. The excited precursor material flows through the holes 344 in the perforated plate 346 and through channels 348 (only one of which is shown in FIG. 3 ) toward the processing volume 310. A portion of the photons and non-thermal energy from the IR lamp 342 also passes through the holes 344, the perforated plate 346, and the channels 348, which benefit from the reflective materials and / or surfaces disposed on the inner surface of the gas distribution assembly 312, thereby illuminating the flow path 334 of the precursor material. In this way, the vibrational energy of the precursor material may be maintained along the flow path from the point of introduction into the processing volume 310 .

[0053] 4 is a cross-sectional view of a process chamber 400 suitable for performing a selective removal process (SRP) as described in detail below, according to one or more embodiments. The process chamber 400 may be the process chamber 124 shown in FIG.

[0054] The processing chamber 400 includes a chamber body 402, a lid assembly 404, and a support assembly 406. The lid assembly 404 is disposed at an upper end of the chamber body 402, and the support assembly 406 is at least partially disposed within the chamber body 402. A vacuum system can be used to remove gas from the processing chamber 400. The vacuum system includes a vacuum pump 408 coupled to a vacuum port 410 disposed in the chamber body 402.

[0055] The lid assembly 404 includes a remote plasma system (RPS) 412 that can process a fluorine-containing precursor that then travels through a gas inlet assembly 414. Two different gas supply channels can be seen within the gas inlet assembly 414. A first channel 416 carries gas through the RPS 412, while a second channel 418 bypasses the RPS 412. Either channel can be used for a fluorine-containing precursor. In some embodiments, the first channel 416 can be used for process gas and the second channel 418 can be used for treatment gas. The lid (also referred to as a "conductive top") 420 and the perforated diaphragm (also referred to as a "showerhead") 422 are shown with an insulating ring 424 therebetween that allows an AC potential to be applied to the lid 420 relative to the perforated diaphragm 422. The AC potential strikes the plasma in the chamber plasma region 426. The process gas may travel through the first passage 416 into the chamber plasma region 426 and may be excited by the plasma in the chamber plasma region 426 alone or in combination with the RPS 412. If the process gas (e.g., a fluorine-containing precursor) flows through the second passage 418, only the chamber plasma region 426 is used for excitation. The perforated partition 422 separates the chamber plasma region 426 from the substrate processing region 428 below the perforated partition 422. The perforated partition 422 allows the plasma present in the chamber plasma region 426 to avoid directly exciting the gases in the substrate processing region 428, while still allowing the excited species to travel from the chamber plasma region 426 into the substrate processing region 428.

[0056] The perforated baffle 422 is located between the chamber plasma region 426 and the substrate processing region 428 and allows plasma effluents (excited derivatives of precursors or other gases) generated within the RPS 412 and / or the chamber plasma region 426 to pass through vias 430 that traverse the thickness of the plate. The perforated baffle 422 also has one or more hollow volumes 432 that can be filled with a precursor (such as a fluorine-containing precursor) in vapor or gas form and pass through small holes 434 into the substrate processing region 428 but not directly into the chamber plasma region 426. In this embodiment, the perforated baffle 422 is thicker than the length of the minimum diameter 436 of the via 430. The length 438 of the minimum diameter 436 of the via 430 can be limited by forming a larger diameter portion of the via 430 that partially passes through the perforated baffle 422 to maintain a significant concentration of excited species that penetrate from the chamber plasma region 426 to the substrate processing region 428. In some embodiments, the length of the minimum diameter 436 of the via 430 can be of the same order of magnitude as or smaller than the minimum diameter 436 of the via 430 .

[0057] The perforated baffle 422 may be adapted to function as an ion suppressor. Alternatively, a separate processing chamber element (not shown) may be included that suppresses the concentration of ions traveling into the substrate processing region 428. The lid 420 and the perforated baffle 422 may function as a first electrode and a second electrode, respectively, such that the lid 420 and the perforated baffle 422 may receive different voltages. In these configurations, electrical power (e.g., RF power) may be applied to the lid 420, the perforated baffle 422, or both. For example, electrical power may be applied to the lid 420 while the perforated baffle 422 (functioning as an ion suppressor) is grounded. An RF generator may provide electrical power to the lid 420 and / or the perforated baffle 422. The voltage applied to the lid 420 may promote uniform distribution of plasma (i.e., reduced local plasma) within the chamber plasma region 426. To enable formation of plasma in the chamber plasma region 426, the insulating ring 424 may electrically insulate the lid 420 from the perforated baffle 422. The insulating ring 424 may be made of ceramic and may have a high breakdown voltage to avoid sparking. The portion of the processing chamber 400 near the capacitively coupled plasma components described above may further include a cooling unit (not shown) including one or more cooling fluid channels to cool the plasma-exposed surface using a circulating coolant (e.g., water).

[0058] In the illustrated embodiment, the perforated baffle 422 can distribute (via the vias 430) a process gas containing fluorine, hydrogen, or plasma effluents of the process gas after being excited by the plasma in the chamber plasma region 426. In some embodiments, the process gas introduced into the RPS 412 and / or the chamber plasma region 426 can contain fluorine (e.g., F2, NF3, or XeF2). The process gas can also include a diluent gas such as helium (He), argon (Ar), or nitrogen (N2). The plasma effluents can include ionized or neutral derivatives of the process gas and can also be referred to herein as radical fluorine and / or radical hydrogen, referring to the atomic composition of the introduced process gas.

[0059] The vias 430 inhibit the migration of ionic charged species out of the chamber plasma region 426 while allowing uncharged neutral or radical species to enter the substrate processing region 428 through the perforated partition 422. These uncharged species may include highly reactive species transported through the vias 430 along with a less reactive carrier gas. As mentioned above, the migration of ionic species through the vias 430 may be reduced, and in some examples, completely inhibited. Controlling the amount of ionic species passing through the perforated partition 422 provides increased control over the gas mixture in contact with the underlying patterned substrate, which in turn increases control over the deposition and / or etching characteristics of the gas mixture. For example, adjustments to the ion concentration of the gas mixture may alter the etch selectivity (e.g., the ratio of the etch rate of germanium silicon to the etch rate of silicon).

[0060] In some embodiments, the number of vias 430 may be between about 60 and about 2000. The vias 430 may have various shapes, but are most easily made circular. In some embodiments, the minimum diameter 436 of the vias 430 may be between about 0.5 mm and about 20 mm or between about 1 mm and about 6 mm. The choice of the cross-sectional shape of the vias is also flexible, and the vias may be made conical, cylindrical, or a combination of both shapes. In different embodiments, the number of apertures 434 for introducing unexcited precursors into the substrate processing region 428 may be between about 100 and about 5000 or between about 500 and about 2000. The diameter of the aperture 434 may be between about 0.1 mm and about 2 mm.

[0061] The vias 430 may control the passage of plasma activated gases (i.e., ions, radicals, and / or neutral species) through the perforated baffle 422. For example, the aspect ratio of the holes (i.e., the ratio of hole diameter to length) and / or the geometry of the holes may be controlled to reduce the flow of ionic charged species in the activated gas through the perforated baffle 422. The vias 430 in the perforated baffle 422 may include a tapered portion facing the chamber plasma region 426, and a cylindrical portion facing the substrate processing region 48. The proportions and dimensions of the cylindrical portion may be designed to control the flow of ionic species delivered to the substrate processing region 428. An adjustable electrical bias may also be applied to the perforated baffle 422 as an additional means of controlling the flow of ionic species through the perforated baffle 422.

[0062] Alternatively, the via 430 may have a smaller inner diameter (ID) toward the top surface of the perforated baffle 422 and a larger ID toward the bottom surface. In addition, the bottom edge of the via 430 may be chamfered to help evenly distribute the plasma effluents in the substrate processing region 428 when the plasma effluents leave the perforated baffle 422, and promote uniform distribution of the plasma effluents and precursor gases. The smaller ID can be placed at various locations along the via 430 and still allow the perforated baffle 422 to reduce the ion density within the substrate processing region 428. The reduction in ion density is caused by an increase in the number of collisions with the wall before entering the substrate processing region 428. Each collision increases the probability that the ion is neutralized by gaining or losing electrons from the wall. Generally speaking, the smaller ID of the via 430 may be between about 0.2 mm and about 20 mm. In other embodiments, the smaller ID may be between about 1 mm and 6 mm or between about 0.2 mm and about 5 mm. Additionally, the aspect ratio of via 430 (i.e., the ratio of the smaller ID to the hole length) may be approximately 1 to 20. The smaller ID of via 430 may be the smallest ID found along the length of via 430. The cross-sectional shape of via 430 may be generally cylindrical, conical, or any combination thereof.

[0063] The support assembly 406 may include a substrate support 440 to support a substrate 442 thereon during processing. The substrate support 440 may be coupled to an actuator 444 via a shaft 446 that extends through a centrally located opening formed in the bottom of the chamber body 402. The actuator 444 may be flexibly sealed to the chamber body 402 via a bellows (not shown) that prevents vacuum leaks around the shaft 446. The actuator 444 allows the substrate support 440 to be moved vertically within the chamber body 402 between a processing position and a loading position. The loading position is slightly lower than the opening of a channel (not shown) formed in the sidewall of the chamber body 402.

[0064] The substrate support 440 has a flat, or substantially flat, substrate support surface for supporting thereon a substrate 442 to be processed. The substrate support 440 may be moved vertically within the chamber body 402 by an actuator 444, which is coupled to the substrate support 440 by a shaft 446. In some processing steps, the substrate may be placed on lift pins 488 to perform additional thermal processing steps, such as performing an annealing step.

[0065] Processing Example

[0066] FIG5 depicts a process flow diagram of a method 500 for forming a contact layer in a semiconductor structure 600 according to a first embodiment of the present disclosure. FIG6A, FIG6B, FIG6C, FIG6D, FIG6E, FIG6F, and FIG6G correspond to cross-sectional views of a portion of the semiconductor structure 600 at various states of the method 500. It should be understood that FIG6A, FIG6B, FIG6C, FIG6D, FIG6E, FIG6F, and FIG6G only illustrate a partial schematic diagram of the semiconductor structure 600, and that the semiconductor structure 600 may contain any number of transistor sections and additional materials having aspects as shown in the figure. It should also be noted that although the method shown in FIG5 is described sequentially, other processing sequences including one or more operations that have been omitted and / or added, and / or have been rearranged in another desired order also fall within the scope of the embodiments of the disclosure provided herein.

[0067] 6A , 6B, 6C, 6D, 6E, 6F, and 6G, a semiconductor structure 600 may include a first transistor device 602 and a second transistor device 604 formed on a substrate.

[0068] As used herein, the term "substrate" refers to a layer of material that serves as a basis for subsequent processing operations and includes a surface to be cleaned. The substrate may be a silicon-based material or any suitable insulating or conductive material as desired. The substrate may include materials such as crystalline silicon (e.g., Si <100> or Si <111> ), silicon oxide, strained silicon, silicon germanium, doped or undoped polysilicon, doped or undoped silicon wafers and patterned or unpatterned wafers, silicon on insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, or sapphire.

[0069] As shown in FIG6A , a portion of a first transistor device 602 of a plurality of first transistor devices formed on a substrate includes a first semiconductor region 606 formed of a first material. A portion of a second transistor device 604 of a plurality of second transistor devices formed on a substrate includes a second semiconductor region 608 formed of a second material. The first and second materials include materials having different compositions such that the second material can be selectively etched relative to the first material (i.e., the etching rate of the second material is higher than the etching rate of the first material). The etching selectivity of the second material (i.e., the ratio of the etching rate of the second material to the etching rate of the first material) is between about 10:1 and 500:1. Example combinations of the first material and the second material include silicon (Si) / silicon germanium (SiGe), germanium (Ge) / silicon germanium (SiGe), or silicon (Si) / germanium tin (GeSn), respectively.

[0070] The first semiconductor region 606 may be doped with an n-type dopant, such as phosphorus (P) or antimony (Sb), at a concentration of about 10 20 cm -3 With 5×10 21 cm -3 The second semiconductor region 608 may be doped with a p-type dopant, such as boron (B) or gallium (Ga), at a concentration of about 10 20 cm -3 With 5×10 21 cm -3 between, depending on the desired conduction characteristics of the second transistor device 604.

[0071] The semiconductor structure 600 further includes a dielectric layer 610 having a first opening 612 formed over each of the first semiconductor regions 606 and a second opening 614 formed over each of the second semiconductor regions 608. The dielectric layer 610 may be formed of a dielectric material such as silicon dioxide (SiO2) or silicon nitride (Si3N4).

[0072] The first semiconductor region 606 and the second semiconductor region 608 may be formed using any suitable deposition technique, such as epitaxial (Epi) deposition, chemical vapor deposition (CVD), atomic layer deposition (ALD), or physical vapor deposition (PVD), and the openings 612 and 614 may be formed by a patterning technique, such as photolithography and etching processes.

[0073] The method 500 begins with a pre-clean process in block 510. The pre-clean process may be performed in a processing chamber, such as the processing chamber 122 shown in FIG. 1 or the processing chamber 200 shown in FIG.

[0074] The pre-cleaning process is configured to remove contaminants (such as a native oxide layer) or patterning residues (e.g., carbon fluoride) formed on the exposed surface of the first semiconductor region 606 in the first opening 612 and on the exposed surface of the second semiconductor region 608 in the second opening 614. The pre-cleaning process is used to prepare the exposed surface of the first semiconductor region 606 in the first opening 612 and the exposed surface of the second semiconductor region 608 in the second opening 614, on which epitaxial layers may be formed in a subsequent epitaxial deposition process. The pre-cleaning process may be used to further adjust the growth rate of the subsequently deposited epitaxial layer on the surface of the first semiconductor region 606 (e.g., silicon (Si)) and the surface of the second semiconductor region 608 (e.g., silicon germanium (SiGe)) in a subsequent epitaxial deposition process. Adjusting the growth rate of the subsequently deposited epitaxial layer may be performed by controlling the amount of residual material (such as the amount of remaining oxide material) disposed at the surface of the first semiconductor region 606 and the second semiconductor region 608, surface activation treatment, and / or altering the crystal structure of the material at the surface of the first semiconductor region 606 and the second semiconductor region 608 after performing the pre-cleaning treatment (e.g., promoting an amorphous or crystalline structure). In some embodiments, for example, the pre-cleaning treatment may have a certain etch rate selectivity between the surface of the oxidized SiGe:B-containing region and the surface of the oxidized Si:P-containing region, such that the pre-cleaning treatment will "clean" the SiGe:B surface (e.g., remove oxide formed thereon) and leave the Si:P surface with at least a portion of the oxide layer formed thereon.

[0075] The pre-cleaning process may include an anisotropic remote plasma assisted dry etching process, such as a reactive ion etching (RIE) process, using a plasma formed from a gas including argon (Ar), helium (He), or a combination thereof. The plasma effluent directionally strikes and removes the remaining dielectric layer within the first opening 612 and the second opening 614.

[0076] The pre-cleaning process may include an isotropic plasma etching process, such as a SiCoNi™ dry chemical etching process, using a plasma formed from a gas including ammonia (NH3), nitrogen trifluoride (NF3), hydrogen fluoride (HF), or a combination thereof, and a carrier gas such as nitrogen (N2), hydrogen (H2), or a combination thereof. The dry chemical etching process is selective to oxide layers, and therefore does not readily etch silicon, germanium, or nitride layers, regardless of whether the layers are amorphous, crystalline, or polycrystalline. The dry chemical etching process has a selectivity of at least about 3:1 for oxide relative to silicon or germanium, and is typically 5:1 or better, and sometimes 10:1. The dry chemical etching process is also highly selective to oxide relative to nitride. The dry chemical etching process has a selectivity of at least about 3:1, typically 5:1 or better, and sometimes 10:1 relative to nitride.

[0077] The pre-clean process may include an inductively coupled plasma (ICP) etch process that uses a plasma formed from gases including chlorine (Cl2) and hydrogen (H2), and a carrier gas including argon (Ar) and helium (He). The ICP etch process is used to form deep ridges with smooth sidewalls in silicon.

[0078] The pre-cleaning process may include a surface activation process based on an isotropic plasma etching process (such as SiCoNi™ dry chemical etching process) using a plasma formed by a gas including ammonia (NH3), nitrogen trifluoride (NF3), hydrogen fluoride (HF), or a combination thereof and a carrier gas such as nitrogen (N2), hydrogen (H2), or a combination thereof. In one example, the plasma cleaning process is a remote plasma-assisted dry cleaning process that involves exposing the substrate to HF and NH3 simultaneously, and optionally includes plasma byproducts of one or more gases. Inert gases such as argon and helium may also be used. Any of the three gases (inert / HF / NH3), or a combination thereof, may be exposed to energy, as described above, to form a plasma thereof, thereby being used to remove desired contaminants and passivate at least a portion of the substrate surface. Any residual compounds remaining on the substrate surface after exposing the substrate to the plasma can be subsequently removed by subsequently heating the substrate to a desired temperature.

[0079] At block 520, as shown in FIG6B, a first selective deposition process is performed to epitaxially form a first contact layer 616 on an exposed surface of the first semiconductor region 606 within the first opening 612, and to epitaxially form a second contact layer 618 on an exposed surface of the second semiconductor region 608 within the second opening 614. The first selective deposition process may be performed in a processing chamber, such as the processing chambers 126, 128, or 130 shown in FIG1, or the processing chamber 300 shown in FIG3.

[0080] The first contact layer 616 is subsequently removed, as discussed below. The second contact layer 618 is formed as an interface between the second semiconductor region 608 and a metal contact plug to be formed within the second opening 614 to minimize parasitic resistance. The first contact layer 616 and the second contact layer 618 are formed of a third material. An example of the third material includes silicon germanium (SiGe), wherein the ratio of germanium (Ge) varies between 20% and 100%. The first contact layer 616 and the second contact layer 618 may be doped with a p-type dopant, such as boron (B) or gallium (Ga), at a concentration of about 10 20 cm -3 With 5×10 21 cm -3 between, depending on the desired conductive properties of the second contact layer 618 .

[0081] In some embodiments, the first selective deposition process includes a first deposition process and a first etching process. The first deposition process is an epitaxial deposition process. The selectivity of the first selective deposition process may be derived from the difference between the nucleation of the third material on the exposed surface of the first semiconductor region 606 and the second semiconductor region 608 (e.g., silicon (Si) or silicon germanium (SiGe)) and the nucleation of the third material on the exposed surface of the dielectric layer 610 (e.g., silicon dioxide (SiO2) or silicon nitride (Si3N4)). Nucleation may occur at a faster rate on the exposed surfaces of the first semiconductor region 606 and the second semiconductor region 608 (e.g., silicon (Si) or silicon germanium (SiGe)) than on the exposed surface of the dielectric layer 610 (e.g., silicon dioxide (SiO2) or silicon nitride (Si3N4)), and thus when the semiconductor structure 600 is exposed to the deposition gas in the first deposition process, an epitaxial layer of the third material may be formed on the exposed surfaces of the first semiconductor region 606 and the second semiconductor region 608 (e.g., silicon (Si) or silicon germanium (SiGe)), and an amorphous layer of the third material may be formed on the exposed surface of the dielectric layer 610 (e.g., silicon dioxide (SiO2) or silicon nitride (Si3N4)). In the subsequent first etching process, the amorphous layer of the third material formed on the exposed surface of the dielectric layer 610 may be etched at a faster rate than the epitaxial layer of the third material formed on the exposed surfaces of the first semiconductor region 606 and the second semiconductor region 608 by an appropriate etching gas. Thus, the overall result of the combined first deposition process and first etching process may be epitaxial growth of the third material on exposed surfaces of the first semiconductor region 606 and the second semiconductor region 608 while minimizing growth, if any, of the third material on exposed surfaces of the dielectric layer 610 .

[0082] In some embodiments, the deposition gas includes a silicon-containing precursor, a germanium-containing precursor, and a dopant source. The silicon-containing precursor may include silane (SiH4), disilane (Si2H6), tetrasilane (Si4H 10 ), or a combination thereof. The germanium-containing precursor may include germane (GeH4), germanium tetrachloride (GeCl4), and digermane (Ge2H6). The dopant source may include, for example, boron or gallium, depending on the desired conductive properties of the second contact layer 618. The dopant source may include the precursor diborane (B2H6). The etching gas includes an etchant gas and a carrier gas. The etchant gas may include a halogen-containing gas, such as hydrogen chloride (HCl), chlorine (Cl2), or hydrogen fluoride (HF). The carrier gas may include nitrogen (N2), argon (Ar), helium (He), or hydrogen (H2).

[0083] The first deposition process and the first etching process may be performed at a low temperature of less than about 450° C. and at a pressure between 5 Torr and 600 Torr.

[0084] The cycle of the first deposition and second etching process may be repeated as needed to obtain the desired thickness of the first contact layer 616 and the second contact layer 618. The thickness of the first contact layer 616 and the second contact layer 618 may be between about 30 Å and about 100 Å.

[0085] At block 530, a patterning process is performed to form a patterned stack 620 over the second semiconductor region 608 so as to cover the second contact layer 618, as shown in Figure 6C. The patterning process may be performed using a conventional photolithography patterning process.

[0086] The patterned stack 620 may be deposited onto the exposed surface of the semiconductor structure 600 using a planarization filling process (e.g., spin coating), and subsequently patterned by suitable photolithography and etching processes. The patterned stack 620 may be formed of an organic dielectric layer (ODL), a silicon anti-reflective coating (SiARC), or a photoresist.

[0087] At block 540, a selective removal process (SRP) is performed to selectively remove the first contact layer 616 (e.g., silicon germanium (SiGe)) from the first semiconductor region 606 (e.g., silicon (Si)) and the dielectric layer 610 (e.g., silicon dioxide (SiO2) or silicon nitride (Si3N4)), as shown in FIG6D. The SRP may be performed in a processing chamber, such as the processing chamber 124 shown in FIG1, or the processing chamber 400 shown in FIG4.

[0088] SRP includes plasma etching using plasma effluents formed from a fluorine-containing precursor (e.g., nitrogen trifluoride (NF3)). Plasma effluents from a remote plasma source (e.g., remote plasma source 224 shown in FIG. 4) flow into a substrate processing region (e.g., substrate processing region 428 shown in FIG. 4). The plasma effluents react with the exposed surface of the semiconductor structure 600 and selectively remove the first contact layer 616 (e.g., silicon germanium (SiGe)) while very slowly removing the first semiconductor region 606 (e.g., silicon (Si)). In general, for all X>Y, the SRP described herein is used to compare the Si (1-Y) Ge Y Faster Si removal (1-X) Ge X (including germanium, i.e., X=1). In some embodiments, the etch selectivity of germanium to silicon is derived in part from the presence of an ion suppressor (e.g., perforated baffle 422 described in FIG. 4 ) positioned between a chamber plasma region (e.g., chamber plasma region 426 shown in FIG. 4 ) and a substrate processing region (e.g., substrate processing region 428 shown in FIG. 4 ).

[0089] The fluorine-containing precursor includes nitrogen trifluoride, carbon fluoride, atomic fluorine, diatomic fluorine, fluorine-halogen compounds (e.g., bromine trifluoride, chlorine trifluoride), sulfur hexafluoride, xenon difluoride, or a combination thereof. A diluent gas (e.g., argon (Ar), helium (He), nitrogen (N2), or a combination thereof) is also flowed into the chamber plasma region, where the diluent gas is simultaneously excited into a plasma with the fluorine-containing precursor. The diluent gas reduces the diffusion rate of the plasma effluent and thus increases the etching selectivity of germanium to silicon.

[0090] In some embodiments, a fluorine-containing precursor (e.g., nitrogen trifluoride (NF3)) is supplied at a flow rate between about 5 sccm (standard cubic centimeters per minute) and about 40 sccm, argon (Ar) is supplied at a flow rate between about 4 sccm and about 1500 sccm, helium (He) is supplied at a flow rate between about 100 sccm and about 5000 sccm, and nitrogen (N2) is supplied at a flow rate between about 100 sccm and about 5000 sccm. SRP can be performed at a temperature between about -20°C and about 60°C and at a pressure between 1 Torr and 50 Torr. The etch selectivity of silicon germanium (SiGe) (with a germanium (Ge) ratio of 30%) over phosphorus-doped silicon (Si:P) can be greater than 200:1, and over thermal oxide (SiO x ) has an etch selectivity of greater than 500:1, and has an etch selectivity of greater than 500:1 compared to silicon nitride (Si3N4).

[0091] At block 550, a conventional plasma ashing process is performed to remove the patterned stack 620, as shown in Figure 6E. The plasma ashing process may be performed in a processing chamber, such as the processing chamber 122 shown in Figure 1, or the processing chamber 200 shown in Figure 2.

[0092] The plasma ashing process may use plasma formed from a gas including oxygen (O 2 ). The ashing process may use a wet cleaning process using a solution such as a mixture of sulfuric acid (H 2 SO 4 ) and hydrogen peroxide (H 2 O 2 ) to remove residues of the patterned stack 620 on the semiconductor structure 600 .

[0093] At block 560, a second deposition process is performed, as shown in Figure 6F. The second deposition processes may each be performed in a processing chamber, such as processing chambers 126, 128, or 130 shown in Figure 1, or processing chamber 300 shown in Figure 3.

[0094] In the second deposition process, a metal layer 622 is formed on the exposed surface of the first semiconductor region 606 and the second contact layer 618. The metal layer 622 contacts the second contact layer 618 and provides an electrical connection between the contact plug to be formed in the second opening 614 and the second semiconductor region 608 while maintaining an electrical connection therethrough. The metal layer 622 may be formed of a metal material such as titanium (Ti), cobalt (Co), nickel (Ni), molybdenum (Mo), or tantalum (Ta), or a silicide thereof.

[0095] In some embodiments, the metal source may include a precursor including titanium (Ti), tantalum (Ta), cobalt (Co), nickel (Ni), or molybdenum (Mo), or a combination thereof. The second deposition processes may each be performed at a temperature between about 300° C. and about 800° C. and at a pressure between 1 Torr and 50 Torr.

[0096] In the second deposition process, a barrier metal layer 624 may also be formed on the exposed inner surfaces of the first opening 612 and the second opening 614, and on the exposed surface of the dielectric layer 610. The barrier metal layer 624 protects the metal layer 622 and allows nucleation and growth of contact plugs in the first opening 612 and the second opening 614, as discussed below. The barrier metal layer 624 may be formed of a barrier metal material that is titanium nitride (TiN) or tantalum nitride (TaN). In some embodiments, the metal layer 622 is a silicide layer formed from a portion of the barrier metal layer 624 by using a spike annealing process. In some other embodiments, the metal layer 622 is a silicide layer formed by a separate selective deposition process performed before forming the barrier metal layer 624.

[0097] The second deposition process performed in block 560 may include any suitable deposition process, such as atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), or the like, in a processing chamber (such as processing chambers 126, 128, or 130 shown in FIG. 1) at a temperature between about 100° C. and about 300° C.

[0098] In block 570, a metal filling process is performed to form a first contact plug 626 in the first opening 612 and a second contact plug 628 in the second opening 614, as shown in FIG6G. The first contact plug 626 and the second contact plug 628 may be formed of a contact plug metal material, such as tungsten (W), cobalt (Co), ruthenium (Ru), or molybdenum (Mo). The first contact plug 626 and the second contact plug 628 may include a metal having a desired work function. The metal filling process in block 570 may include a chemical vapor deposition (CVD) process using a tungsten-containing precursor (such as WF6) or a cobalt-containing precursor in a process chamber (such as the process chambers 126, 128, or 130 shown in FIG1).

[0099] After the metal fill process, the semiconductor structure 600 may be planarized, such as by using a chemical mechanical planarization (CMP) process.

[0100] Alternative Examples

[0101] FIG. 7 depicts a process flow diagram of a method 700 for forming a contact layer in a semiconductor structure 800 according to a second embodiment of the present disclosure. FIG. 8A , FIG. 8B , FIG. 8C , FIG. 8D , and FIG. 8E correspond to cross-sectional views of a portion of the semiconductor structure 800 at various states of the method 700 . It should be understood that FIG. 8A , FIG. 8B , FIG. 8C , FIG. 8D , and FIG. 8E only show a partial schematic diagram of the semiconductor structure 800 , and the semiconductor structure 800 may contain any number of transistor segments and additional materials having aspects as shown in the figure. It should also be noted that although the method shown in FIG. 7 is described sequentially, other processing sequences including one or more operations that have been omitted and / or added, and / or that have been rearranged in another desired order fall within the scope of the embodiments of the disclosure provided herein. In the following description, the same reference numerals are used for components that are substantially the same as those of the first embodiment, and descriptions of repeated components may be omitted.

[0102] The method 700 begins with a pre-cleaning process in block 710. The pre-cleaning process in block 710 is generally the same as the pre-cleaning process in block 510. The pre-cleaning process in block 710 may be adjusted so that the growth rate of the epitaxial layer of the third material (e.g., silicon germanium (SiGe)) on the exposed surface of the second semiconductor region 608 (e.g., silicon germanium (SiGe)) is higher than the growth rate of the epitaxial layer of the third material (e.g., silicon germanium (SiGe)) on the exposed surface of the first semiconductor region 606 (e.g., silicon (Si)). The knobs for controlling the pre-cleaning process may include gas chemistry, gas ratio, gas flow rate, substrate temperature, temperature gradient, chamber pressure, power and / or frequency of power supply, RF excitation frequency, duty cycle and / or frequency of RF power, etching time, or a combination thereof. As discussed above, the growth rate of the subsequently deposited epitaxial layer can be adjusted by controlling or adjusting the composition of the material disposed at the surface of the first semiconductor region 606 and the second semiconductor region 608, and / or changing the crystal structure of the material at the surface of the first semiconductor region 606 and the second semiconductor region 608 after performing a pre-cleaning process.

[0103] 8B , a first selective deposition process is performed to epitaxially form a first contact layer 816 on the exposed surface of the first semiconductor region 606 within the first opening 612, and to epitaxially form a second contact layer 818 on the exposed surface of the second semiconductor region 608 within the second opening 614. The first selective deposition process in block 720 may be generally the same as the first selective deposition process in block 520. In some embodiments, due to the manner in which the pre-cleaning process in block 710 is performed and thus the surface conditions of the first semiconductor region 606 and the second semiconductor region 608 during the first selective deposition process, the second contact layer 818 will grow to a greater thickness than the thickness of the first contact layer 816 during the same processing time period.

[0104] In some other embodiments of block 720, processing parameters for simultaneously forming the second contact layer 818 and the first contact layer 816 are adjusted and / or controlled such that the thickness of the second contact layer 818 formed on the second semiconductor region 608 is greater than the thickness of the first contact layer 816 formed on the first semiconductor region 606 during the same processing time period. It is believed that by controlling one or more deposition process parameters (e.g., temperature, process pressure, precursor gas composition, etc.), the growth rate of the second contact layer 818 containing silicon germanium (SiGe) on the second semiconductor region 608 containing silicon germanium (SiGe) can be significantly greater than the growth rate of the first contact layer 816 containing silicon germanium (SiGe) on the first semiconductor region 606 containing silicon.

[0105] In any of the examples of block 720, the first contact layer 816 can be formed to a thickness between about 5 Å and about 100 Å and the second contact layer 818 can be formed to a thickness between about 30 Å and about 100 Å, wherein the thickness of the first contact layer 816 is less than the thickness of the second contact layer 818.

[0106] In block 730, a selective removal process (SRP) is performed to selectively remove the first contact layer 816 (e.g., silicon germanium (SiGe)) to the first semiconductor region 606 (e.g., silicon (Si)) and the dielectric layer 610 (e.g., silicon dioxide (SiO2) or silicon nitride (Si3N4)), as shown in FIG8C. The SRP in block 730 is the same as the SRP in block 540. However, the second contact layer 818 is exposed (unlike the second contact layer 618 covered by the patterned stack 620 as shown in FIGS. 6C and 6D), and thus the second contact layer 818 is also selectively removed. In this process, a certain amount of the first contact layer 816 and the second contact layer 818 (such as all of the first contact layer 816) are removed, and thus a certain amount of the second contact layer 818 remains over the second semiconductor region 608 due to the increased thickness of the second contact layer 818 formed during block 720 compared to the first contact layer 816. The cycle of the first selective deposition process in block 720 and the SRP in block 730 may be repeated as needed to obtain a desired thickness of the second contact layer 818. The thickness of the second contact layer 618 may be between about 30 Å and about 100 Å.

[0107] In block 740, a second deposition process is performed to form the metal layer 622 and the barrier metal layer 624, as shown in Figure 8D. The second deposition process provided in block 740 may be the same as the second deposition process in block 560.

[0108] At block 750 , a metal filling process is performed to form a first contact plug 626 in the first opening 612 and a second contact plug 628 in the second opening 614 , as shown in FIG 6E . The metal filling process provided at block 750 may be the same as the metal filling process at block 670 .

[0109] Embodiments described herein provide methods and systems for forming a contact epitaxial layer in a trench at a selected portion of a transistor structure. The contact trench structure includes a metal contact plug formed in a trench between adjacent device modules, and a contact interposed between the contact plug in the device module and a silicon-based channel. The contact is formed by a selective deposition process, thereby reducing parasitic resistance. The metal contact plug is formed without gaps by a deposition-each-deposition process, thereby reducing contact resistance. The contact epitaxial layer can be p-type germanium silicon formed on an exposed surface of a p-type MOS device (e.g., germanium silicon), and no epitaxial layer will be formed on an n-type MOS (e.g., silicon) or on a dielectric layer formed above a p-type MOS device and an n-type MOS device. The method and system do not require the use of a photomask to pattern the epitaxial layer, and thus reduce damage to the manufactured semiconductor structure.

[0110] While the foregoing is directed to embodiments of the present disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope thereof, and the scope thereof is determined by the claims that follow.

Claims

1. A method for forming an electrical contact in a semiconductor structure, comprising the following steps: performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate, wherein the exposed surfaces of the plurality of first semiconductor regions and the plurality of second semiconductor regions are each disposed within an opening formed in a dielectric layer disposed above the substrate; performing a first selective epitaxial deposition process to form a first contact layer on the exposed surface of the first semiconductor region and a second contact layer on the exposed surface of the second semiconductor region; performing a patterning process to form a patterned stack, wherein the patterned stack includes a patterned layer, the patterned layer including an opening formed over the first contact layer within each opening disposed in the dielectric layer, and a portion of the patterned layer disposed over each second contact layer disposed within each opening in the dielectric layer; as well as A selective removal process is performed to selectively remove the first contact layer from the plurality of first semiconductor regions, the dielectric layer, and the patterned layer.

2. The method according to claim 1, wherein The first semiconductor region formed on the substrate includes silicon, The second semiconductor region formed on the substrate includes silicon germanium, and The first contact layer and the second contact layer include silicon germanium.

3. The method according to claim 1, wherein The patterned stack includes a material selected from an organic dielectric layer, a silicon anti-reflective coating, and a photoresist.

4. The method according to claim 1, wherein the selective removal process is performed under the following conditions: Temperature between -20℃ and 60℃, Pressures between 1 Torr and 50 Torr, A flow rate of the fluorine-containing precursor between about 5 sccm and 40 sccm, Argon (Ar) flow rate between 4 sccm and 1500 sccm, a helium (He) flow rate between 100 sccm and 5000 sccm, and A flow rate of nitrogen (N2) between 100 sccm and 5000 sccm.

5. The method according to claim 1, further comprising the following steps: After the selective removal process, an ashing process is performed to remove the patterned stack.

6. The method according to claim 5, further comprising the following steps: After the ashing process, a second deposition process is performed to form a metal layer on an exposed surface of the first semiconductor region and on an exposed surface of the second contact layer formed on the second semiconductor region.

7. The method according to claim 6, wherein The metal layer includes a material selected from titanium silicide (Ti), cobalt silicide (Co), nickel silicide (Ni), molybdenum silicide (Mo), and tantalum silicide (Ta).

8. A method for forming a contact layer in a semiconductor structure, the method comprising the following steps: performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate, wherein the exposed surfaces of the plurality of first semiconductor regions and the plurality of second semiconductor regions are each disposed within an opening formed in a dielectric layer disposed above the substrate; performing a first selective epitaxial deposition process to simultaneously form a first contact layer having a first thickness on the exposed surface of the first semiconductor region and a second contact layer having a second thickness on the exposed surface of the second semiconductor region, wherein the second thickness is greater than the first thickness; as well as A selective removal process is performed to selectively remove the first contact layer and the second contact layer from the plurality of first semiconductor regions and the dielectric layer until the first contact layer is substantially removed from the first semiconductor region and a portion of the second contact layer remains on the second semiconductor region.

9. The method according to claim 8, wherein The first semiconductor region formed on the substrate includes silicon, The second semiconductor region formed on the substrate includes silicon germanium, and The first contact layer and the second contact layer include silicon germanium.

10. The method according to claim 8, wherein the selective removal process is performed under the following conditions: Temperature between -20℃ and 60℃, Pressures between 1 Torr and 50 Torr, A flow rate of the fluorine-containing precursor between about 5 sccm and 40 sccm, Argon (Ar) flow rate between 4 sccm and 1500 sccm, a helium (He) flow rate between 100 sccm and 5000 sccm, and A flow rate of nitrogen (N2) between 100 sccm and 5000 sccm.

11. The method according to claim 8, further comprising the steps of: A second selective epitaxial deposition process is performed to form a metal layer on an exposed surface of the first semiconductor region and on an exposed surface of the second contact layer formed on the second semiconductor region.

12. The method according to claim 11, wherein The metal layer includes a material selected from titanium silicide (Ti), cobalt silicide (Co), nickel silicide (Ni), molybdenum silicide (Mo), and tantalum silicide (Ta).

13. A processing system comprising: a first processing chamber; a second processing chamber; a third processing chamber; and A system controller, the system controller being configured to: performing a pre-cleaning process on exposed surfaces of a plurality of first semiconductor regions and a plurality of second semiconductor regions formed on a substrate in the first process chamber; performing a first selective deposition process in the second processing chamber to epitaxially form a first contact layer on the exposed surface of the first semiconductor region and epitaxially form a second contact layer on the exposed surface of the second semiconductor region of the substrate; as well as A selective removal process is performed in the third process chamber to selectively remove the first contact layer from the first semiconductor region.

14. The processing system of claim 13, wherein the system controller is further configured to transfer the substrate among the first processing chamber, the second processing chamber, and the third processing chamber without breaking a vacuum environment.

15. The processing system of claim 13, wherein The first semiconductor region formed on the substrate includes silicon, The second semiconductor region formed on the substrate includes silicon germanium, and The first contact layer and the second contact layer include silicon germanium.

16. The processing system according to claim 13, wherein the selective removal process in the third processing chamber is performed under the following conditions: Temperature between -20℃ and 60℃, Pressures between 1 Torr and 50 Torr, A flow rate of the fluorine-containing precursor between about 5 sccm and 40 sccm, Argon (Ar) flow rate between 4 sccm and 1500 sccm, a helium (He) flow rate between 100 sccm and 5000 sccm, and A flow rate of nitrogen (N2) between 100 sccm and 5000 sccm.

17. The processing system of claim 13, further comprising: A fourth processing chamber, wherein the system controller is further configured to: A second deposition process is performed in the fourth process chamber to form a metal layer on an exposed surface of the first semiconductor region and on an exposed surface of the second contact layer formed on a second semiconductor region formed on the substrate, the metal layer comprising a material selected from titanium silicide (Ti), cobalt silicide (Co), nickel silicide (Ni), molybdenum silicide (Mo), and tantalum silicide (Ta).

18. The processing system of claim 17, further comprising: A fifth processing chamber, wherein the system controller is further configured to: A conformal deposition process is performed in the fifth processing chamber to form a barrier metal layer on the metal layer, the barrier metal layer comprising a material selected from titanium nitride (TiN) and tantalum nitride (TaN).

19. The processing system of claim 18, further comprising: a sixth processing chamber; Wherein the system controller is further configured to perform an ashing process in the sixth process chamber to remove the patterned stack before the second deposition process in the fourth process chamber and after the selective removal process in the third process chamber.