Negative electrode active material and method for producing negative electrode active material
By using Li silicate silicon compound particles covering the intermediate layer and carbon layer in the negative electrode active material of lithium-ion secondary batteries, the problem of surface fragmentation caused by expansion of silicon materials is solved, and the battery capacity and circulation characteristics are improved. And maintain stability during mass production and slurry .
Patent Information
- Application Number
- CN202380031496.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-02-15
- Publication Date
- 2024-11-01
Smart Images

Figure CN118891756A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a negative electrode active material and a method for producing the negative electrode active material. Background Art
[0002] In recent years, small electronic devices represented by mobile terminals have become widely popular, and there is a strong demand for further miniaturization, lightness and long life. In response to the above market demand, the development of a secondary battery that is particularly small and light and can obtain high energy density has been promoted. The application of this secondary battery is not limited to small electronic devices, and its application in large electronic devices represented by automobiles and power storage systems represented by houses is also under study.
[0003] Among them, lithium-ion secondary batteries are expected to be easy to reduce in size and increase in capacity, and can achieve higher energy density than lead batteries and nickel-cadmium batteries.
[0004] The lithium ion secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, and the negative electrode contains a negative electrode active material involved in charge and discharge reactions.
[0005] As the negative electrode active material, carbon-based active materials are widely used. However, according to recent market demand, the battery capacity is sought to be further improved. In order to increase the battery capacity, the use of silicon as a negative electrode active material is being studied. The reason is that the theoretical capacity of silicon (4199mAh / g) is more than 10 times that of graphite (372mAh / g), so a significant increase in battery capacity can be expected. For the development of silicon materials as negative electrode active material materials, not only silicon single substance has been studied, but also compounds represented by alloys and oxides have been studied. In addition, regarding the shape of the active material, for carbon-based active materials, there are studies ranging from standard coating types to integrated types directly deposited on the collector.
[0006] However, as the negative electrode active material, if silicon is used as the main material, the negative electrode active material will expand and shrink during charge and discharge, so it is easy to break mainly near the surface of the negative electrode active material. In addition, ionic substances will be generated inside the active material, and the negative electrode active material will become a substance that is easy to break. If the surface layer of the negative electrode active material breaks, a new surface will be generated, and the reaction area of the active material will increase. At this time, since the decomposition reaction of the electrolyte will occur on the new surface, and a film as a decomposition product of the electrolyte will be formed on the new surface, the electrolyte will be consumed. Therefore, it is easy to reduce the cycle characteristics.
[0007] Hitherto, various studies have been conducted on negative electrode materials and electrode structures for lithium-ion secondary batteries using silicon materials as main materials in order to improve the initial efficiency and cycle characteristics of the batteries.
[0008] Specifically, for the purpose of obtaining good cycle characteristics and high safety, a vapor phase method is used to simultaneously deposit silicon and amorphous silicon dioxide (for example, refer to patent document 1). In addition, in order to obtain high battery capacity and safety, a carbon material (conductive material) is provided on the surface layer of the silicon oxide particles (for example, refer to patent document 2). Further, in order to improve the cycle characteristics and obtain high input-output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer having a higher oxygen ratio near the collector is formed (for example, refer to patent document 3). In addition, in order to improve the cycle characteristics, oxygen is contained in the silicon active material, and is formed in a manner such that the average oxygen content is less than 40at% and the oxygen content near the collector becomes higher (for example, refer to patent document 4).
[0009] In addition, in order to improve the initial charge and discharge efficiency, a Si phase, SiO2, M y O metal oxide nanocomposite (for example, see Patent Document 5). In addition, in order to improve the cycle characteristics, SiO x (0.8≤x≤1.5, particle size range = 1μm~50μm) is mixed with a carbon material and calcined at a high temperature (for example, refer to patent document 6). In addition, in order to improve the cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1~1.2, and the active material is controlled within a range where the difference between the maximum and minimum values of the molar ratio of the active material near the interface of the collector is less than 0.4 (for example, refer to patent document 7). In addition, in order to improve the battery load characteristics, a metal oxide containing lithium is used (for example, refer to patent document 8). In addition, in order to improve the cycle characteristics, a hydrophobic layer of a silane compound or the like is formed on the surface of the silicon material (for example, refer to patent document 9). In addition, in order to improve the cycle characteristics, silicon oxide is used and a graphite film is formed on its surface to impart conductivity (for example, refer to patent document 10). In patent document 10, regarding the shift value obtained from the RAMAN spectrum associated with the graphite film, at 1330cm -1 and 1580cm -1 Broad peaks appear at the 1330 / I 1580 1.5<I 1330 / I 1580 <3. In addition, in order to improve the high battery capacity and cycle characteristics, particles having a silicon microcrystalline phase dispersed in silicon dioxide are used (for example, refer to Patent Document 11). In addition, in order to improve the overcharge and overdischarge characteristics, silicon oxides in which the atomic ratio of silicon to oxygen is controlled to 1:y (0<y<2) are used (for example, refer to Patent Document 12).
[0010] As a lithium-ion secondary battery using silicon oxide, Hitachi Maxell has started shipping square secondary batteries for smartphones using nano-silicon composites since June 2010 (see, for example, Non-Patent Document 1). 0+ ~Si 4+ Composite materials have various oxidation states (see non-patent document 2). In addition, Kapaklis proposed a disproportionate structure in which silicon oxide is separated into Si and SiO2 by applying a heat load to silicon oxide (see non-patent document 3). Miyachi et al. are focusing on Si and SiO2 that contribute to charging and discharging in silicon oxide with a disproportionate structure (see non-patent document 4), and Yamada et al. proposed the following reaction formula between silicon oxide and Li (see non-patent document 5).
[0011] 2SiO(Si+SiO2)+6.85Li + +6.85e - →1.4Li 3.75 Si+0.4Li4SiO4+0.2SiO2
[0012] The above reaction formula shows that Si and SiO 2 constituting silicon oxide react with Li to separate into Li silicide and Li silicate, and a portion of unreacted SiO 2 .
[0013] The Li silicate generated here is considered to be irreversible and will not release Li once formed, so it is a stable substance. The capacity per unit mass calculated from this reaction formula is close to the experimental value and is considered to be the reaction mechanism of silicon oxide. Kim et al. used 7 Li-MAS-NMR or 29 Si-MAS-NMR identified Li silicate, an irreversible component generated by charge and discharge of silicon oxide, as Li 4 SiO 4 (see Non-Patent Document 6).
[0014] This irreversible capacity is the biggest drawback of silicon oxide, and improvements are being sought. In response, Kim et al. used a Li pre-doping method to preform Li silicate, which greatly improved the initial efficiency of the battery and produced a negative electrode that can withstand actual use (see Non-Patent Document 7).
[0015] In addition, a method of treating powder instead of doping the electrode with Li has been proposed, and this method achieves improvement in irreversible capacity (see Patent Document 13).
[0016] In order to improve the water resistance of the obtained Li-doped material, aluminum isopropoxide was used as the material and AlO was applied to the upper layer of the C layer. xCoating (see Patent Document 14).
[0017] Prior art literature
[0018] Patent Literature
[0019] Patent Document 1: Japanese Patent Application Publication No. 2001-185127
[0020] Patent Document 2: Japanese Patent Application Publication No. 2002-042806
[0021] Patent Document 3: Japanese Patent Application Publication No. 2006-164954
[0022] Patent Document 4: Japanese Patent Application Publication No. 2006-114454
[0023] Patent Document 5: Japanese Patent Application Publication No. 2009-070825
[0024] Patent Document 6: Japanese Patent Application Publication No. 2008-282819
[0025] Patent Document 7: Japanese Patent Application Publication No. 2008-251369
[0026] Patent Document 8: Japanese Patent Application Publication No. 2008-177346
[0027] Patent Document 9: Japanese Patent Application Publication No. 2007-234255
[0028] Patent Document 10: Japanese Patent Application Publication No. 2009-212074
[0029] Patent Document 11: Japanese Patent Application Publication No. 2009-205950
[0030] Patent Document 12: Japanese Patent Application Laid-Open No. 06-325765
[0031] Patent Document 13: Japanese Patent Application Publication No. 2015-156355
[0032] Patent Document 14: Japanese Patent Application Publication No. 2017-10645
[0033] Non-patent literature
[0034] Non-patent document 1: Battery Manufacturers Association official paper "でんち" dated May 1, 2012, page 10
[0035] Non-patent document 2: A. Hohl, T. Wieder, PA van Aken, TE Weirich, G.Denninger, M. Vidal, S. Oswald, C. Deneke, J. Mayer, and H. Fuess: J. Non-Cryst. Solids, 320, (2003), 255.
[0036] Non-patent document 3: V. Kapaklis, J. Non-Crystalline Solids, 354 (2008) 612
[0037] Non-patent document 4: Mariko Miyachi, Hironori Yamamoto, and Hidemasa Kawai, J. Electrochem. Soc. 2007 volume 154, issue 4, A376-A380
[0038] Non-patent document 5: M. Yamada, M. Inaba, A. Ueda, K. Matsumoto, T. Iwasaki, T. Ohzuku, J. Electrochem. Soc., 159, A1630 (2012)
[0039] Non-patent document 6: Taeahn Kim, Sangjin Park, and Seung M. Oh, J. Electrochem. Soc. volume 154, (2007), A1112-A1117.
[0040] Non-patent literature 7: Hye Jin Kim, Sunghun Choi, Seung Jong Lee, Myung Won Seo, Jae Goo Lee, Erhan Deniz, Yong Ju Lee, Eun Kyung Kim, and Jang Wook Choi,. Nano Lett. 2016, 16, 282-288. Summary of the invention
[0041] 1. Technical issues to be resolved
[0042] As mentioned above, in recent years, small electronic devices represented by mobile terminals are being promoted to be high-performance and multifunctional, and lithium-ion secondary batteries as their main power sources are required to increase battery capacity. As one of the means to solve this problem, it is expected to develop a lithium-ion secondary battery including a negative electrode using a silicon material as the main material. In addition, it is expected that the lithium-ion secondary battery using silicon materials has initial charge and discharge characteristics and cycle characteristics that are approximately equivalent to those of lithium-ion secondary batteries using carbon-based active materials. In response to this, silicon oxide modified by the embedding of Li and partial deintercalation of the embedded Li (doped with Li) is used as a negative electrode active material, thereby improving the cycle characteristics and initial charge and discharge characteristics. However, for a negative electrode material embedded with Li, when used in a slurry in an electrode polarization process, a portion of the Li component will dissolve into the slurry, so that various problems such as reducing the viscosity of the binder (thickener) will occur.
[0043] As a solution to the above problems, the use of AlO x The outermost layer of SiO / C doped with Li was coated with a layer (Patent Document 14), but as a result, shear force was applied during stirring during slurrying, and the film peeled off, reducing the effect by half. In particular, when a small machine of several liters was used for slurrying, the shear force was small and there was no problem, but it was found that if it was transferred to a mass production machine larger than the scale of this small machine, the slurry stability could not be maintained for 2 days.
[0044] The present invention is completed in view of the above-mentioned problems, and its purpose is to provide a negative electrode active material and a manufacturing method capable of manufacturing such a negative electrode active material, which can improve the initial efficiency and increase the battery capacity, can achieve sufficient battery cycle characteristics and improve the stability during mass production of slurry.
[0045] (II) Technical solution
[0046] In order to solve the above technical problems, the present invention provides a negative electrode active material, which is a negative electrode active material comprising negative electrode active material particles, characterized in that:
[0047] The negative electrode active material particles have:
[0048] Silicon compound particles comprising Li silicate;
[0049] an intermediate layer covering the surface of the silicon compound particle and comprising a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle; and
[0050] The outermost carbon layer has covered the intermediate layer.
[0051] The negative electrode active material of the present invention includes negative electrode active material particles, the negative electrode active material particles include silicon compound particles, and the silicon compound particles include Li silicate, and therefore the battery capacity can be increased.
[0052] In addition, in the negative electrode active material of the present invention, the silicon compound particles include Li silicate, and the surface of the silicon compound particles is coated by an intermediate layer, and the intermediate layer includes a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles, and the intermediate layer has been coated with the outermost carbon layer providing conductivity, so that the stability during mass production of slurry can be improved, and excellent Li diffusibility and conductivity in the bulk can be obtained. By improving Li diffusibility, the initial efficiency, battery cycle characteristics and input characteristics can be improved.
[0053] As a result, the negative electrode active material of the present invention can improve initial efficiency and increase battery capacity, realize sufficient battery cycle characteristics, and improve stability during mass production of slurry.
[0054] It is preferred that at least a portion of the silicon compound particles contain at least one selected from the group consisting of Li2SiO3, Li4SiO4 and Li6Si2O7 as the Li silicate.
[0055] Such silicon compound particles can reduce the irreversible capacity generated during charging because the SiO2 component part of the silicon compound particles is pre-modified into lithium silicate. The SiO2 component part is unstable when inserting and extracting lithium during charging and discharging of the battery.
[0056] It is preferred that the intermediate layer contains the Li compound, and the Li compound is a composite compound containing Li, C, and O.
[0057] The composite compound containing Li, C and O has excellent Li permeability. Therefore, by making the intermediate layer contain such a Li compound, the Li diffusivity can be further improved. By further improving the Li diffusivity, the initial efficiency, battery cycle characteristics and input characteristics can be further improved.
[0058] At this time, for example, in the C1s waveform obtained from the XPS spectrum, at least a portion of the composite compound including Li, C, and O has an OC═O structure.
[0059] The composite compound including Li, C, and O can have, for example, an OC═O structure in at least a portion.
[0060] It is preferred that the intermediate layer contains the metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide contains at least one element selected from the group consisting of aluminum, magnesium, titanium, zirconium, calcium, and niobium.
[0061] If the intermediate layer covering the surface of the silicon compound particles contains such a cation, excellent adhesion and excellent water resistance can be more reliably exhibited.
[0062] In this case, it is preferred that the thickness of the metal oxide and / or metal hydroxide in the intermediate layer is 0.1 nm or more and 10 nm or less.
[0063] When the thickness of the metal oxide and / or metal hydroxide in the intermediate layer is within this range, it is easy to control the film thickness and sufficient Li permeability can be exhibited.
[0064] It is particularly preferred that the intermediate layer contains the Li compound and the metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide covers the Li compound.
[0065] Metal oxides and / or metal hydroxides can show better water resistance. In addition, the water resistance of Li compounds different from Li silicates is not too high, but Li permeability is excellent. Therefore, if negative electrode active material particles are included, the negative electrode active material particles include an intermediate layer, the intermediate layer includes a Li compound different from Li silicates, and a metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide is coated with a Li compound different from Li silicates, the stability during mass production slurry can be further improved, and better Li diffusibility in the body can be shown.
[0066] Before charging and discharging the negative electrode active material particles, the negative electrode active material particles preferably have a peak originating from the Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα rays, and the grain size corresponding to the crystal plane is 5.0 nm or less, and the ratio A / B of the intensity A of the peak originating from the Si (111) crystal plane to the intensity B of the peak originating from the Li2SiO3 (111) crystal plane satisfies the following formula (1):
[0067] 0.4≤A / B≤1.0 …(1).
[0068] When the negative electrode active material includes such negative electrode active material particles, the irreversible capacity can be reduced and a high battery capacity can be achieved.
[0069] It is preferred that the negative electrode active material particles have a median particle size of 4.5 μm or more and 15 μm or less.
[0070] When the median diameter of the negative electrode active material particles is within this range, it is possible to prevent the reaction with the electrolyte from being promoted and prevent the electronic connection from being lost due to the expansion of the active material during charge and discharge.
[0071] In addition, the present invention provides a method for producing a negative electrode active material, which is a method for producing a negative electrode active material containing negative electrode active material particles, characterized by comprising:
[0072] Made of general formula SiO x The process of silicon oxide particles represented by , wherein 0.5≤x≤1.6;
[0073] A step of inserting Li into the silicon oxide particles to prepare silicon compound particles containing Li silicate;
[0074] A step of forming an intermediate layer on the surface of the silicon compound particle, wherein the intermediate layer comprises a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle;
[0075] forming a carbon layer covering the outermost layer of the intermediate layer to obtain negative electrode active material particles; and
[0076] A process of manufacturing a negative electrode active material using the negative electrode active material particles.
[0077] Since the negative electrode active material produced by such a production method includes negative electrode active material particles, the negative electrode active material particles include silicon compound particles, and the silicon compound particles include Li silicate, the battery capacity can be increased.
[0078] In addition, in the negative electrode active material manufactured by such a manufacturing method, the silicon compound particles contain Li silicate, and the surface of the silicon compound particles is coated by an intermediate layer, and the intermediate layer contains a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles, and the intermediate layer is coated with the outermost carbon layer providing conductivity, so that the stability during mass production of slurry can be improved, and excellent Li diffusibility and conductivity in the body can be obtained. By improving Li diffusibility, the initial efficiency, battery cycle characteristics and input characteristics can be improved.
[0079] As a result, the negative electrode active material produced by the method for producing a negative electrode active material of the present invention can improve initial efficiency and increase battery capacity, realize sufficient battery cycle characteristics, and improve stability during mass production of slurry.
[0080] Preferably, in the step of preparing silicon compound particles containing Li silicate, silicon compound particles whose surfaces contain the Li compound are prepared.
[0081] In the step of forming the intermediate layer, a portion of the Li compound present on the surface of the silicon compound particles is removed, and a portion of the surface of the silicon compound particles and the surface of the Li compound are coated with a metal oxide and / or a metal hydroxide, thereby forming the intermediate layer comprising the metal oxide and / or the metal hydroxide and the Li compound.
[0082] The method for producing a negative electrode active material of this preferred embodiment can produce a negative electrode active material in which the interlayer contains both a Li compound different from Li silicate and a metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide covers the Li compound.
[0083] Metal oxides and / or metal hydroxides can show better water resistance. In addition, Li compounds different from Li silicates have low water resistance but excellent Li permeability. Therefore, by the manufacturing method of the preferred embodiment, a negative electrode active material can be manufactured, which further improves the stability during mass production of slurry and shows better Li diffusivity in the main body.
[0084] At this time, for example, in the step of forming the intermediate layer, the metal oxide and / or the metal hydroxide can be formed by hydrolysis and dehydration condensation of the metal alkoxide.
[0085] The metal oxide and / or the metal hydroxide can be formed by, for example, hydrolysis and dehydration condensation of a metal alkoxide.
[0086] (III) Beneficial effects
[0087] As described above, the negative electrode active material of the present invention can improve initial efficiency and increase battery capacity, realize sufficient battery cycle characteristics, and improve stability during mass production of slurry.
[0088] Furthermore, according to the method for producing a negative electrode active material of the present invention, it is possible to produce a negative electrode active material that can improve initial efficiency and increase battery capacity, can achieve sufficient battery cycle characteristics, and exhibits high stability during mass production of slurry. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] Figure 1 It is a schematic partial cross-sectional view of negative electrode active material particles included in one example of the negative electrode active material of the present invention.
[0090] Figure 2It is a schematic partial cross-sectional view of negative electrode active material particles included in another example of the negative electrode active material of the present invention.
[0091] Figure 3 A schematic partial cross-sectional view of negative electrode active material particles included in another example of the negative electrode active material of the present invention.
[0092] Figure 4 It is a schematic cross-sectional view showing an example of the structure of a negative electrode including the negative electrode active material of the present invention.
[0093] Figure 5 It is an exploded view showing a structural example (laminated film type) of a lithium ion secondary battery including a negative electrode containing the negative electrode active material of the present invention.
[0094] Figure 6 Schematic diagram of a partial cross-section of negative electrode active material particles included in the negative electrode active material of Comparative Example 4.
[0095] Figure 7 This is a part of the XPS spectrum of the negative electrode active material particles included in the negative electrode active material of Example 16 after six etchings.
[0096] Figure 8 This is a part of the XPS spectrum of the outermost layer of the negative electrode active material particles of the negative electrode active material of Example 1 and the XPS spectrum after etching three times. DETAILED DESCRIPTION
[0097] As described above, as a method of increasing the battery capacity of a lithium-ion secondary battery, a study is being conducted on using a negative electrode using silicon oxide as a main material as a negative electrode of a lithium-ion secondary battery. It is expected that a lithium-ion secondary battery using the silicon oxide will show initial charge and discharge characteristics approximately equivalent to those of a lithium-ion secondary battery using a carbon-based active material. In addition, it is expected that SiO doped with Li, which can improve the initial charge and discharge characteristics, will have cycle characteristics approximately equivalent to those of a carbon-based active material. However, a negative electrode active material having a satisfactory pot life of the slurry when mass-producing the slurry has not yet been proposed.
[0098] Therefore, the inventors of the present application have repeatedly conducted serious research to obtain a negative electrode active material that has excellent handling properties when used as a negative electrode active material for a secondary battery, can obtain high cycle characteristics, and improve initial charge and discharge characteristics, resulting in an increase in battery capacity. As a result, the following facts were discovered, thereby completing the present invention: by coating the surface of the silicon compound particles containing Li silicate with an intermediate layer containing a Li compound different from Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles, and coating the intermediate layer with a carbon layer that provides conductivity as the outermost layer, the stability during mass production of slurry can be improved, and excellent Li diffusion and conductivity in the body can be obtained.
[0099] That is, the present invention is a negative electrode active material, which is a negative electrode active material containing negative electrode active material particles, characterized in that:
[0100] The negative electrode active material particles have:
[0101] Silicon compound particles comprising Li silicate;
[0102] an intermediate layer covering the surface of the silicon compound particle and comprising a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle; and
[0103] The outermost carbon layer has covered the intermediate layer.
[0104] In addition, the present invention also provides a method for producing a negative electrode active material, which is a method for producing a negative electrode active material containing negative electrode active material particles, characterized by comprising:
[0105] Made of general formula SiO x The process of silicon oxide particles represented by , wherein 0.5≤x≤1.6;
[0106] A step of inserting Li into the silicon oxide particles to prepare silicon compound particles containing Li silicate;
[0107] A step of forming an intermediate layer on the surface of the silicon compound particle, wherein the intermediate layer comprises a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle;
[0108] forming a carbon layer covering the outermost layer of the intermediate layer to obtain negative electrode active material particles; and
[0109] A process of manufacturing a negative electrode active material using the negative electrode active material particles.
[0110] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0111] <Negative electrode active material>
[0112] The negative electrode active material (hereinafter also referred to as silicon-based negative electrode active material) of the present invention includes negative electrode active material particles (hereinafter also referred to as silicon-based negative electrode active material particles) containing silicon compound particles, and thus can improve battery capacity.
[0113] In addition, by forming Li silicate on at least a portion of the silicon compound particles, the slurry can be stabilized before coating, and by using a stable slurry, a good electrode can be obtained and the battery characteristics can be improved. However, it is known that such a slurry has insufficient long-term storage properties, and the formed Li silicate will slowly dissolve in the slurry over time.
[0114] When forming Li silicate, for example, by applying a heat load, the crystal phase of Li silicate can be coarsened, thereby reducing the dissolution of Li components in the slurry, but at the same time, the crystallinity of Si will be improved. The generation of such high-crystallinity Si will become the main cause of a significant reduction in battery characteristics.
[0115] Furthermore, when the Li silicate phase is coarsened, the diffusibility of Li is greatly reduced, thereby deteriorating the battery characteristics.
[0116] On the other hand, if the crystal phase of Li silicate is infinitely reduced to suppress the crystallization of Si and the coarsening of the Li silicate phase, a Li silicate phase that gradually dissolves into water is generated.
[0117] As a result, the battery characteristics are satisfactory. However, if the electrode polarization process, especially the slurry preparation, is left for a long time, the binder will deteriorate and the battery characteristics will deteriorate. Therefore, it is necessary to apply the slurry as soon as possible after preparation.
[0118] Therefore, the inventors of the present application have developed a material, which is obtained by coating the surface of silicon compound particles containing Li silicate with an intermediate layer containing a Li compound different from Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles, and coating the intermediate layer with a carbon layer as the outermost layer that provides conductivity, thereby improving the stability during mass production of slurry and obtaining excellent Li diffusion properties in the body.
[0119] In the negative electrode active material of the present invention, the silicon compound particles contain Li silicate, and the surface of the silicon compound particles is coated with an intermediate layer, and the intermediate layer contains a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles, and the intermediate layer is coated with the outermost carbon layer.
[0120] Metal oxides and / or metal hydroxides can show excellent water resistance. Therefore, the intermediate layer includes metal oxides and / or metal hydroxides in a manner adjacent to at least a portion of the surface of the silicon compound particles, which can improve the water resistance of the negative electrode active material without hindering the permeability of Li, and improve the stability during mass production of slurry. In addition, by making the metal oxide and the metal hydroxide coexist, it is possible to further show excellent stability and excellent Li permeability.
[0121] The Li compound different from the Li silicate in the negative electrode active material of the present invention is, for example, a composite compound containing Li, C and O. Such a composite compound may be, for example, a material having a carboxylic acid structure (OC=O) in part, which is synthesized by condensation of a decomposition product of a solvent used in the manufacture of the negative electrode active material during a heat treatment process.
[0122] Although such a Li compound has low water resistance, it is contained in the intermediate layer in a manner adjacent to a portion of the surface of the silicon compound particles, thereby improving the stability of the negative electrode active material during mass production of slurry. In addition, since such a Li compound has excellent Li permeability, the intermediate layer containing such a Li compound can show excellent Li permeability.
[0123] Furthermore, the outermost carbon layer covering the intermediate layer can provide electrical conductivity.
[0124] As a result, the negative electrode active material of the present invention can improve the stability during mass production of slurry and obtain excellent Li diffusibility and conductivity in the body. By improving Li diffusibility, the initial efficiency, battery cycle characteristics and input characteristics can be improved.
[0125] Therefore, according to the negative electrode active material of the present invention, the initial efficiency can be improved to increase the battery capacity, sufficient battery cycle characteristics can be achieved, and the stability during mass production of slurry can be improved.
[0126] Hereinafter, the negative electrode active material of the present invention will be described in more detail.
[0127] The negative electrode active material of the present invention can be used as a negative electrode active material for, for example, a non-aqueous electrolyte secondary battery, particularly a lithium ion secondary battery.
[0128] Figure 1 Schematic diagram of a partial cross section of negative electrode active material particles included in one example of the negative electrode active material of the present invention is shown in FIG.
[0129] Figure 1 The negative electrode active material particles 1 shown include silicon compound particles 2. The silicon compound particles 2 can be called silicon oxide materials, and the silicon oxide materials include silicon compounds containing oxygen. The ratio of silicon to oxygen constituting the silicon oxide is preferably between SiO x : in the range of 0.8≤x≤1.2. If x is greater than 0.8, the oxygen ratio is higher than that of silicon alone, so the cycle characteristics are good. If x is less than 1.2, the resistance of the silicon oxide particles will not be excessively increased, so it is preferred. Among them, SiO x In the composition, the closer x is to 1, the more preferred. The reason is that high cycle characteristics can be obtained. In addition, the composition of the silicon compound in the present invention is not necessarily 100% pure, and may also contain trace impurity elements.
[0130] in addition, Figure 1 SiO x The embodiment in which the particle 2 contains the Si phase 3 is taken as an example.
[0131] In addition, in the negative electrode active material of the present invention, the silicon compound particles 2 contain Li silicate. Specifically, it is preferred that the silicon compound particles 2 contain at least one selected from the group consisting of Li2SiO3, Li4SiO4 and Li6Si2O7 in at least a portion. More specifically, it is more preferred that the silicon compound particles 2 contain Li2SiO3. Since such a material partially modifies the SiO2 component in the silicon oxide into another lithium silicate in advance, the irreversible capacity generated during charging can be reduced. The SiO2 component is unstable when lithium is inserted and released during the charging and discharging of the battery. In addition, by coarsening the Li silicate within the range where the crystal growth of Si has been suppressed, the irreversible capacity generated by charging and discharging can be reduced. Therefore, it is expected that the Li2SiO3 in the Li silicate generated in the body has crystallinity.
[0132] However, if the particles are too coarse, they will not contribute to charge and discharge, so there is an optimal range.
[0133] When formed into slurry, Li4SiO4 and Li6Si2O7 have high solubility in water and are therefore more unstable than Li2SiO3. However, by utilizing the intermediate layer described below, the stability of mass-produced slurry is improved, allowing them to be fully used.
[0134] At this time, Li4SiO4 has the best Li diffusion performance, and it is desirable to use it together with Li2SiO3 which has substantially high structural stability.
[0135] Furthermore, Li silicates such as Li2SiO3, Li4SiO4 and Li6Si2O7 contained in the main body of the silicon oxide particles can be quantified by NMR (Nuclear Magnetic Resonance). NMR measurement can be performed, for example, under the following conditions.
[0136] 29 Si-MAS-NMR (Magic angle spinning nuclear magnetic resonance)
[0137] · Equipment: 700NMR spectrometer manufactured by Bruker,
[0138] Probe: 4mm HR-MAS rotor 50μL,
[0139] Sample speed: 10kHz,
[0140] ·Measurement environment temperature: 25℃.
[0141] The degree of coarsening of Li silicate and the degree of crystallization of Si can be confirmed by XRD (X-ray Diffraction). As an X-ray diffraction device, D8 ADVANCE manufactured by Bruker can be used. For example, the X-ray source uses Cu Kα rays and a Ni filter, and the measurement is performed from 10 to 40° with an output of 40 kV / 40 mA, a slit width of 0.3°, a step length of 0.008°, and a counting time of 0.15 seconds per step.
[0142] The negative electrode active material particle 1 further includes: an intermediate layer 4 covering the surface of the silicon compound particle 2 ; and an outermost carbon layer 7 covering the surface of the intermediate layer 4 .
[0143] The intermediate layer 4 included in the negative electrode active material 1 of the present invention includes a Li compound 5 other than Li silicate adjacent to a portion of the surface of the silicon compound particle 2 and / or a metal oxide and / or metal hydroxide 6 adjacent to at least a portion of the surface of the silicon compound particle 2 .
[0144] Figure 1 In the example shown, the intermediate layer 4 contains both a Li compound 5 other than Li silicate and a metal oxide and / or metal hydroxide 6 .
[0145] Or, if Figure 2 In the example shown, the intermediate layer 4 may contain only Li compounds 5 other than Li silicates.
[0146] Or, if Figure 3In the example shown, the intermediate layer 4 can thus contain only metal oxides and / or metal hydroxides 6 .
[0147] The metal oxide and / or metal hydroxide 6 can exhibit excellent water resistance. Therefore, by including the metal oxide and / or metal hydroxide 6 in the intermediate layer 4 in a manner adjacent to at least a portion of the surface of the silicon compound particles 2, the water resistance of the negative electrode active material can be improved without hindering the penetration of Li, thereby improving the stability during mass production of slurry. For example, if an aluminum oxide layer is present in the intermediate layer, Li-AlO x This substance allows Li to pass smoothly, so although the aluminum oxide layer may not exist, if the aluminum oxide layer exists, a better effect related to the permeability of Li can be obtained.
[0148] For example, metal oxides can be generated by hydrolysis and dehydration condensation of metal alkoxides. When a metal oxide layer is formed using metal alkoxides, heat treatment at 100° C. or higher is performed, but the metal alkoxide is likely to remain in a part of the body as a hydroxide layer.
[0149] Such a metal oxide layer can exhibit excellent stability and excellent Li permeability.
[0150] The Li compound 5 used in the present invention, which is different from the Li silicate, is, for example, a composite compound containing Li, C, and O. Such a composite compound may be, for example, a material that is synthesized by condensation of a decomposition product of a solvent used in the manufacture of the negative electrode active material during a heat treatment process and has a carboxylic acid structure (OC=O) in a part.
[0151] In the C1s waveform obtained by XPS (X-ray photoelectron spectroscopy) spectrum, at least a part of Li, C, and O having a carboxylic acid structure has an OC═O structure.
[0152] Although the water resistance of the Li compound 5 different from the Li silicate is not very high, it is contained in the intermediate layer 4 in a manner adjacent to a part of the surface of the silicon compound particle 2, thereby improving the stability of the negative electrode active material during mass production of slurry. In addition, since such a Li compound 5 is excellent in Li permeability, the intermediate layer 4 containing such a Li compound can show excellent Li permeability.
[0153] Furthermore, the carbon layer 7 covering the outermost layer of the intermediate layer 4 can provide electrical conductivity.
[0154] By including the negative electrode active material particles 1 having such a structure, the negative electrode active material of the present invention can improve the stability during mass production of slurry and obtain excellent Li diffusibility and conductivity in the body. By improving Li diffusibility, the initial efficiency, battery cycle characteristics and input characteristics can be improved.
[0155] The negative electrode active material of the present invention is Figure 2 In the case where the intermediate layer 4 comprises only the Li compound 5, or even in the case where Figure 3 In the case where the intermediate layer 4 only comprises the metal oxide and / or metal hydroxide 6, the stability during mass production of the slurry can still be improved. Figure 1 As shown, when the intermediate layer 4 includes a Li compound 5 and a metal oxide and / or a metal hydroxide 6, and the metal oxide and / or the metal hydroxide 6 has coated the Li compound 5, the negative electrode active material of the present invention can enjoy the effects of both the Li compound 5 and the metal oxide and / or the metal hydroxide 6, thereby being able to further improve the stability during mass production of slurry and show better Li diffusion properties within the body.
[0156] Figure 1 In the example shown, the Li compound 5 is adjacent to a portion of the surface of the silicon compound particle 2. In addition, the metal oxide and / or metal hydroxide 6 is adjacent to a portion of the surface of the silicon compound particle 2, specifically, the portion not adjacent to the Li compound 5, and covers the Li compound 5.
[0157] On the other hand, for example, as described in Patent Document 14, when the surface of the silicon compound particles is coated with a carbon layer and the surface of the carbon layer is coated with a metal oxide in the outermost layer, there is no problem in using a small machine for slurrying, but the stability during mass production of slurrying will be reduced due to the reasons described above.
[0158] The presence of the Li compound 5 and the metal oxide and / or metal hydroxide 6 in the negative electrode active material particles 1 can be confirmed by X-ray photoelectron spectroscopy (XPS).
[0159] It is preferred that the metal oxide and / or metal hydroxide 6 contain at least one element selected from the group consisting of aluminum, magnesium, titanium, zirconium, calcium, and niobium.
[0160] If the intermediate layer 4 covering the surface of the silicon compound particle 2 contains such a cation, excellent adhesion and excellent water resistance can be more reliably exhibited.
[0161] Furthermore, it is preferred that the thickness of the metal oxide and / or metal hydroxide 6 in the intermediate layer 4 is 0.1 nm or more and 10 nm or less.
[0162] When the thickness of the metal oxide and / or metal hydroxide 6 in the intermediate layer 4 is within this range, it is easy to control the film thickness and sufficient Li permeability can be exhibited.
[0163] The thickness of the metal oxide and / or metal hydroxide 6 can be measured by the following steps. First, the metal element is quantified by inductively coupled plasma (ICP) analysis, and the volume is calculated based on the known specific gravity (density). In addition, the particle size of the median particle size D50 can be known from the particle size distribution of the powder, and the surface area is calculated by replacing it with a sphere. It is assumed that the metal oxide has uniformly coated the area, thereby being able to calculate the thickness of the metal oxide and / or metal hydroxide 6.
[0164] The negative electrode active material particles 1 included in the negative electrode active material of the present invention preferably have a peak due to the Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα rays before charging and discharging the negative electrode active material particles 1, the grain size corresponding to the crystal plane is 5.0 nm or less, and the ratio A / B of the intensity A of the peak due to the Si (111) crystal plane to the intensity B of the peak due to the Li2SiO3 (111) crystal plane satisfies the following formula (1):
[0165] 0.4≤A / B≤1.0 …(1).
[0166] If the negative electrode active material includes such negative electrode active material particles 1, the irreversible capacity can be reduced and a high battery capacity can be achieved. The smaller the grain size corresponding to the Si (111) crystal plane, the more preferred. Since it is desired to be substantially amorphous, the lower limit of the grain size corresponding to the Si (111) crystal plane is 0 nm (amorphous).
[0167] The negative electrode active material particles 1 preferably have a median particle size of 4.5 μm or more and 15 μm or less.
[0168] If the median particle size of the negative electrode active material particles 1 is within this range, the reaction with the electrolyte can be prevented from being promoted, and the electronic connection can be prevented from being lost due to the expansion of the active material during charge and discharge. The median particle size of the negative electrode active material particles 1 can be measured using a laser diffraction particle size distribution measuring device.
[0169] <Method for producing negative electrode active material>
[0170] The method for producing a negative electrode active material of the present invention is a method for producing a negative electrode active material containing negative electrode active material particles, and the method comprises:
[0171] Made of general formula SiO x The process of silicon oxide particles represented by , wherein 0.5≤x≤1.6;
[0172] A step of inserting Li into the silicon oxide particles to prepare silicon compound particles containing Li silicate;
[0173] A step of forming an intermediate layer on the surface of the silicon compound particle, wherein the intermediate layer comprises a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle;
[0174] forming a carbon layer covering the outermost layer of the intermediate layer to obtain negative electrode active material particles; and
[0175] A process of manufacturing a negative electrode active material using the negative electrode active material particles.
[0176] The negative electrode active material of the present invention described above can be produced by the above-described production method. However, the negative electrode active material of the present invention can also be produced by a production method other than the production method described here.
[0177] Hereinafter, a specific example of the method for producing the negative electrode active material of the present invention will be described.
[0178] [Process for producing silicon oxide particles]
[0179] First, silicon oxide particles (silicon oxide particles) are prepared, and the silicon oxide particles contain a silicon compound containing oxygen. x The case where silicon oxide represented by (0.5≤x≤1.6) is used as the silicon compound containing oxygen.
[0180] First, a raw material that generates silicon oxide gas is heated in the temperature range of 900°C to 1600°C under reduced pressure in the presence of an inert gas, thereby generating silicon oxide gas. At this time, the raw material can be a mixture of metal silicon powder and silicon dioxide powder. Considering the presence of surface oxygen of the metal silicon powder and trace oxygen in the reaction furnace, the mixing molar ratio is expected to be in the range of 0.9 < metal silicon powder / silicon dioxide powder < 1.2.
[0181] The generated silicon oxide gas solidifies and deposits on the adsorption plate. Then, the silicon oxide deposit is taken out while the temperature in the reactor is lowered to below 100°C, and crushed and powdered using a ball mill, jet mill, etc. Silicon oxide particles can be produced in the above manner. In addition, the Si grains in the silicon oxide particles can be controlled by changing the vaporization temperature of the raw material that generates the silicon oxide gas or by heat treatment after the silicon oxide particles are generated.
[0182] [Step of Producing Silicon Compound Particles Containing Li Silicate]
[0183] Then, Li is embedded in the silicon oxide particles prepared in the above manner. Thus, silicon compound particles containing Li silicate are prepared. That is, Li silicate is generated inside the silicon oxide particles. The embedding of Li is preferably performed by an electrochemical method or a redox method.
[0184] In the reformation (intercalation of Li) by the redox method, for example, first, silicon oxide particles are immersed in a solution A in which lithium is dissolved in an ether solvent, so that lithium can be intercalated, thereby obtaining silicon compound particles containing Li silicate. The solution A may further contain a polycyclic aromatic compound or a linear polyphenylene compound.
[0185] After the lithium is embedded, the silicon compound particles are immersed in a solution B containing a polycyclic aromatic compound and its derivatives, thereby enabling the active lithium to be deintercalated from the silicon compound particles. The solvent of the solution B can use, for example, an ether solvent, a ketone solvent, an ester solvent, an alcohol solvent, an amine solvent or a mixed solvent thereof. Alternatively, after being immersed in solution A, the obtained silicon compound particles can be heat-treated under an inert gas. Heat treatment can stabilize the Li compound. Then, washing can be performed by washing with alcohol, alkaline water, weak acid or pure water, etc., which dissolves lithium carbonate.
[0186] As the ether solvent used in solution A, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, or a mixed solvent thereof can be used. Among them, tetrahydrofuran, dioxane, and 1,2-dimethoxyethane are particularly preferably used. These solvents are preferably dehydrated, preferably deoxygenated.
[0187] In addition, as the polycyclic aromatic compounds contained in solution A, one or more of naphthalene, anthracene, phenanthrene, tetracene, pentacene, pyrene, picene, triphenylene, coronene, chrysene and their derivatives can be used, and as the straight-chain polyphenylene compound, one or more of biphenyl, terphenyl and their derivatives can be used.
[0188] As the polycyclic aromatic compound contained in the solution B, one or more of naphthalene, anthracene, phenanthrene, tetracene, pentacene, pyrene, chrysene, triphenylene, coronene, chrysene and derivatives thereof can be used.
[0189] As the ether solvent of the solution B, diethyl ether, tert-butyl methyl ether, tetrahydrofuran, dioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and the like can be used.
[0190] As the ketone solvent, acetone, acetophenone, etc. can be used.
[0191] As the ester solvent, methyl formate, methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, and the like can be used.
[0192] As the alcohol solvent, methanol, ethanol, propanol, isopropanol, etc. can be used.
[0193] As the amine solvent, methylamine, ethylamine, ethylenediamine, and the like can be used.
[0194] The surface layer of the silicon compound particles obtained in this step may be coated with the decomposed product of the solution used in the process of inserting Li.
[0195] [Step of forming an intermediate layer on the surface of silicon compound particles]
[0196] Then, an intermediate layer is formed on the surface of the silicon compound particles. The intermediate layer can be configured as follows: Figure 1 As shown, it contains both a Li compound 5 different from the Li silicate adjacent to a portion of the surface of the silicon compound particle 2, and a metal oxide and / or metal hydroxide 6 adjacent to at least a portion of the surface of the silicon compound particle 2; or Figure 2 As shown, it contains only Li compound 5; or as Figure 3 As shown, only metal oxides and / or metal hydroxides 6 are contained.
[0197] The following are respectively explained Figure 1~Figure 3 An example of a method for forming the intermediate layer 4 is shown.
[0198] ( Figure 1 Circumstances)
[0199] When formed Figure 1 In the case of forming the intermediate layer 4 shown in the figure, first, in the previous step of forming the silicon compound particles 2 containing Li silicate, the silicon compound particles 2 containing the Li compound on the surface are formed.
[0200] Then, a portion of the Li compound present on the surface of the silicon compound particles 2 is removed. For example, the silicon compound particles 2 are fully washed with the solution B selected from the examples listed above to form particles in which the carbon component (C component in the Li compound other than Li silicate) on the surface is 0.5 mass % or less relative to the entire particle. Figure 1 As shown, a Li compound 5 different from Li silicate is obtained adjacent to a part of the surface of the silicon compound particle 2 .
[0201] Then, a part of the surface of the silicon compound particles 2 and the surface of the Li compound 5 are coated with the metal oxide and / or metal hydroxide 6 .
[0202] The metal oxide and / or metal hydroxide 6 is preferably formed by hydrolysis and dehydration condensation of the metal alkoxide. In addition, by performing a heat treatment at 100° C. or higher during the process of forming a metal oxide layer using the metal alkoxide, the metal alkoxide is likely to remain in a part of the body as a hydroxide layer.
[0203] For example, aluminum isopropoxide, magnesium methoxide, calcium isopropoxide, calcium methoxide, aluminum tert-butoxide, aluminum sec-butoxide, aluminum isopropoxide, aluminum n-butoxide, zirconium n-butoxide, titanium tert-butoxide, titanium isopropoxide, titanium n-butoxide, niobium isopropoxide, or niobium n-butoxide is preferably used as a metal alkoxide to form a metal oxide and / or metal hydroxide 6. If the surface of the silicon compound particles 2 is coated with the intermediate layer 4 containing the metal oxide and / or metal hydroxide 6 formed using the above substances as starting materials, excellent water resistance can be more reliably exhibited.
[0204] More specifically, the metal oxide and / or metal hydroxide 6 can be formed by, for example, the following steps.
[0205] The silicon compound particles 2 washed sufficiently in the above manner are added to a solution in which the solution B selected from the above-mentioned examples and a metal alkoxide are dispersed, and stirred sufficiently. As an example, the following method is proposed.
[0206] The mixture was stirred using a 200 mL beaker and a hot plate at 100° C. and 500 rpm for 3 hours.
[0207] As raw materials, 50 g of Li-SiO, 0.25 g (0.5% relative to the silicon compound particles) of Al(Oi-Pr) 3 , and 100 mL of diethylene glycol dimethyl ether were used.
[0208] The powder obtained after stirring is filtered and dried in the range of 100°C to 400°C to obtain Figure 1 The intermediate layer 4 shown contains a Li compound 5 and a metal oxide and / or a metal hydroxide 6 .
[0209] ( Figure 2 Example)
[0210] When formed Figure 2 In the case of forming the intermediate layer 4 shown in the figure, first, in the previous step of forming the silicon compound particles 2 containing Li silicate, the silicon compound particles 2 containing the Li compound on the surface are formed.
[0211] Then, similarly to the above-described steps, a portion of the Li compound present on the surface of the silicon compound particles 2 is removed. Thus, an intermediate layer 4 is obtained. Figure 2As shown, only the Li compound 5 other than the Li silicate is contained adjacent to a part of the surface of the silicon compound particle 2 .
[0212] ( Figure 3 Example)
[0213] Figure 3 The intermediate layer 4 shown can be formed, for example, by the following steps.
[0214] When the silicon compound particles 2 including Li silicate are produced in the previous step of producing the silicon compound particles 2 including Li silicate, the Li compound other than Li silicate existing on the surface of the silicon compound particles 2 is completely removed.
[0215] Then, in the same steps as those described above, metal oxide and / or metal hydroxide 6 is formed on the surface of the silicon compound particles 2. Thus, an intermediate layer 4 is obtained. Figure 3 In the illustrated embodiment, only the metal oxides and / or metal hydroxides 6 which are adjacent to the surface of the silicon compound particles 2 are contained.
[0216] [Step of forming a carbon layer covering the outermost layer of the intermediate layer to obtain negative electrode active material particles]
[0217] Then, a carbon layer as the outermost layer is formed on the surface of the intermediate layer.
[0218] The method for producing the carbon layer is not particularly limited, and an example thereof may be a pyrolytic CVD (chemical vapor deposition) method. An example of a method for producing the carbon layer by the pyrolytic CVD method will be described below.
[0219] First, silicon compound particles whose surfaces are coated with an intermediate layer are placed in a furnace. Then, hydrocarbon gas is introduced into the furnace, and the temperature in the furnace is raised. The decomposition temperature is not particularly limited, but is preferably below 650°C, more preferably below 600°C. By setting the decomposition temperature below 650°C, it is possible to suppress unexpected disproportionation of silicon compound particles. After the temperature in the furnace is raised to a predetermined temperature, a carbon layer is generated on the surface of the intermediate layer. In addition, the hydrocarbon gas that is the raw material of the carbon material is not particularly limited, but is preferably below C n H m In the composition, n≤3 is desirable. When n≤3, the production cost can be reduced and the physical properties of the decomposition product can be improved.
[0220] Although the Li silicate produced by Li insertion (modification) by the redox method is Li4SiO4, it can be converted into other Li silicates such as Li2SiO3 by CVD treatment. The degree of crystallization of Li silicate and Si will change due to the temperature at that time. In addition, the reaction temperature during Li insertion is also related to the degree of crystallization of Li silicate and Si.
[0221] Through this process, it is possible to obtain Figure 1~Figure 3 Negative electrode active material particles 1 having the structure shown.
[0222] [Process of manufacturing negative electrode active material using negative electrode active material particles]
[0223] A negative electrode active material can be produced using the negative electrode active material particles prepared as described above. Thus, an example of the negative electrode active material of the present invention can be produced.
[0224] <Negative electrode>
[0225] The negative electrode active material of the present invention can be used in a negative electrode for, for example, a non-aqueous electrolyte secondary battery, particularly a lithium ion secondary battery.
[0226] Next, the structure of a negative electrode including the negative electrode active material of the present invention is described with examples. Figure 4 A schematic cross-sectional view showing an example of a negative electrode including the negative electrode active material of the present invention. Figure 4 As shown, the negative electrode 10 has a structure in which a negative electrode active material layer 12 is provided on a negative electrode current collector 11. The negative electrode active material layer 12 may be Figure 4 As shown, the negative electrode current collector 11 may be provided on both sides, or may be provided on only one side. Furthermore, the negative electrode of the present invention may not have the negative electrode current collector 11.
[0227] Hereinafter, each component will be described.
[0228] [Negative electrode current collector]
[0229] The negative electrode current collector 11 is an excellent conductive material and is composed of a material having excellent mechanical strength. Examples of conductive materials that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). The conductive material is preferably a material that does not form an intermetallic compound with lithium (Li).
[0230] It is preferred that the negative electrode current collector 11 contains carbon (C) and sulfur (S) in addition to the main elements. This is because the physical strength of the negative electrode current collector 11 will increase. In particular, in the case of an active material layer that expands during charging, if the current collector contains the above elements, it has the effect of suppressing deformation of the electrode containing the current collector. The content of the above-mentioned elements is not particularly limited, and it is preferably less than 100 mass ppm respectively. This is because a higher effect of suppressing deformation can be obtained.
[0231] The surface of the negative electrode current collector 11 may or may not be roughened. A roughened negative electrode current collector is, for example, a metal foil that has been subjected to electrolytic treatment, embossing treatment, or chemical etching. An unroughened negative electrode current collector is, for example, a rolled metal foil.
[0232] [Negative Electrode Active Material Layer]
[0233] The negative electrode active material layer 12 includes the negative electrode active material of the present invention that can absorb and release lithium ions, and may further include other materials such as a negative electrode binder (binder) and a conductive aid from the perspective of battery design. The negative electrode active material includes the negative electrode active material of the present invention.
[0234] In addition, the negative electrode active material layer 12 may include a mixed negative electrode active material, which includes the negative electrode active material (silicon-based negative electrode active material) of the present invention and a carbon-based active material. As a result, the resistance of the negative electrode active material layer is reduced, and the expansion stress generated by charging can be relaxed. As a carbon-based active material, for example, pyrolytic carbon, coke, glassy carbon fiber, organic polymer compound calcined body, carbon black, etc. can be used.
[0235] In addition, as the negative electrode binder contained in the negative electrode active material layer 12, for example, any one or more of a polymer material, a synthetic rubber, etc. can be used. The polymer material is, for example, polyvinylidene fluoride, polyimide, polyamide-imide, aramid, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, carboxymethyl cellulose, etc. The synthetic rubber is, for example, styrene butadiene rubber, fluorine rubber, ethylene propylene diene, etc.
[0236] As the negative electrode conductive additive, for example, one or more carbon materials such as carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers can be used.
[0237] The negative electrode active material layer 12 is formed by, for example, a coating method in which a silicon-based negative electrode active material is mixed with the above-mentioned binder and, if necessary, a conductive aid and a carbon-based active material, and then dispersed in an organic solvent or water and then coated.
[0238] Specifically, for example, as described below. First, the negative electrode active material of the present invention prepared in the manner described above is mixed with other materials such as a negative electrode binder and a conductive aid to prepare a negative electrode mixture, and then an organic solvent or water is added to prepare a slurry. Then, the slurry is applied to the surface of the negative electrode collector and dried to form a negative electrode active material layer. At this time, hot pressing or the like can be performed as needed. A negative electrode containing the negative electrode active material of the present invention can be prepared in the above manner.
[0239] Furthermore, the negative electrode active material of the present invention is particularly suitable for forming a slurry using water, but can also be applied to forming a slurry using an organic solvent.
[0240] <Lithium-ion secondary battery>
[0241] The negative electrode including the negative electrode active material of the present invention can be used as a negative electrode of a non-aqueous electrolyte secondary battery, for example, a lithium ion secondary battery.
[0242] Next, as a specific example of a non-aqueous electrolyte secondary battery that can use the negative electrode active material of the present invention, a laminated film type lithium ion secondary battery will be described.
[0243] [Structure of laminated film type secondary battery]
[0244] Figure 5 The laminated film type lithium ion secondary battery 30 shown is mainly formed by housing a wound electrode body 31 inside a sheet-like outer casing 35. The wound electrode body 31 has a separator between the positive electrode and the negative electrode and is wound. In addition, there is also a case where a laminate with a separator between the positive electrode and the negative electrode is housed without winding. In any electrode body, a positive electrode lead 32 is installed on the positive electrode and a negative electrode lead 33 is installed on the negative electrode. The outermost periphery of the electrode body 31 is protected by a protective tape.
[0245] The positive lead 32 and the negative lead 33 are led out in one direction from inside the outer casing 35 to the outside. The positive lead 32 is made of a conductive material such as aluminum, and the negative lead 33 is made of a conductive material such as nickel or copper.
[0246] The outer packaging member 35 is, for example, a laminated film in which a welding layer, a metal layer, and a surface protective layer are sequentially laminated, and in this laminated film, the outer peripheral edges of the welding layers of two films are welded to each other or adhered with an adhesive or the like so that the welding layer faces the electrode body 31. The welding portion is, for example, a film of polyethylene, polypropylene, etc., and the metal portion is, for example, aluminum foil, etc. The protective layer is, for example, nylon, etc.
[0247] Adhesive films 34 are inserted between the outer casing 35 and the positive electrode lead 32 and between the outer casing 35 and the negative electrode lead 33 to prevent the infiltration of external air. The material of the adhesive films 34 is, for example, polyethylene, polypropylene, or polyolefin resin.
[0248] Hereinafter, each component will be described separately.
[0249] [positive electrode]
[0250] The positive electrode is for example Figure 4 The negative electrode 10 is the same as that of the positive electrode 10, and has a positive electrode active material layer on both sides or one side of the positive electrode collector.
[0251] The positive electrode current collector is formed of a conductive material such as aluminum.
[0252] The positive electrode active material layer contains any one or two or more positive electrode materials (positive electrode active materials) capable of absorbing and releasing lithium ions, and may contain other materials such as a positive electrode binder, a positive electrode conductive aid, and a dispersant according to the design.
[0253] The positive electrode material is preferably a lithium-containing compound. Examples of the lithium-containing compound include: a composite oxide composed of lithium and a transition metal element, or a phosphate compound containing lithium and a transition metal element. Among these positive electrode materials, a compound containing at least one of nickel, iron, manganese, and cobalt is preferred. As its chemical formula, for example, Li x M1O2 or Li y M2PO4 represents. In the formula, M1 and M2 represent at least one transition metal element. The values of x and y vary depending on the charge and discharge state of the battery, but are generally represented by 0.05≤x≤1.10 and 0.05≤y≤1.10.
[0254] Examples of composite oxides containing lithium and transition metal elements include lithium cobalt composite oxides (Li x CoO2), lithium nickel composite oxide (Li x NiO2), lithium nickel cobalt composite oxide, etc. Examples of lithium nickel cobalt composite oxides include lithium nickel cobalt aluminum composite oxide (NCA) and lithium nickel cobalt manganese composite oxide (NCM).
[0255] Examples of the phosphate compound containing lithium and a transition metal element include lithium iron phosphate compound (LiFePO4) and lithium iron manganese phosphate compound (LiFe 1-u Mn u PO4 (0<u<1)), etc. When these positive electrode materials are used, a high battery capacity can be obtained, and excellent cycle characteristics can also be obtained.
[0256] As the positive electrode binder, for example, any one or more of a polymer material, a synthetic rubber, etc. can be used. The polymer material is, for example, polyvinylidene fluoride, polyimide, polyamide-imide, aramid, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, carboxymethyl cellulose, etc. The synthetic rubber is, for example, styrene butadiene rubber, fluorine rubber, ethylene propylene diene, etc.
[0257] As the positive electrode conductive additive, for example, one or more carbon materials such as carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers can be used.
[0258] [negative electrode]
[0259] As the negative electrode of the secondary battery, a negative electrode containing the negative electrode active material of the present invention is used. Preferably, the negative electrode charge capacity of the negative electrode constituting the secondary battery is larger than the electric capacity (as the charge capacity of the battery) obtained by the positive electrode active material agent. Thus, the precipitation of lithium metal on the negative electrode can be suppressed.
[0260] In this example, the positive electrode active material layer is disposed on a portion of both sides of the positive electrode current collector, and similarly, the negative electrode active material layer of the present invention is also disposed on a portion of both sides of the negative electrode current collector. In this case, for example, the negative electrode active material layer disposed on the negative electrode current collector is preferably provided with an area where there is no positive electrode active material layer relative thereto. This is for the purpose of stable battery design.
[0261] The region where the negative electrode active material layer and the positive electrode active material layer are not opposite to each other is hardly affected by charge and discharge. Therefore, the state of the negative electrode active material layer is maintained at the state immediately after formation, thereby being able to accurately investigate the composition of the negative electrode active material with good reproducibility regardless of charge and discharge.
[0262] [Diaphragm]
[0263] The separator isolates lithium metal or the positive electrode from the negative electrode to prevent the current short circuit caused by the contact between the two electrodes and allows lithium ions to pass. The separator is formed of a porous film composed of, for example, a synthetic resin or ceramic, and may also have a laminated structure formed by laminating two or more porous films. As synthetic resins, for example, polytetrafluoroethylene, polypropylene, polyethylene, etc. can be listed.
[0264] [Electrolyte]
[0265] At least a portion of each of the positive electrode active material layer and the negative electrode active material layer, or the separator, is impregnated with a liquid nonaqueous electrolyte (electrolyte solution). The electrolyte solution is an electrolyte salt dissolved in a solvent, and may contain other materials such as additives.
[0266] The solvent can use, for example, a non-aqueous solvent. As the non-aqueous solvent, for example, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane or tetrahydrofuran can be listed. Among them, it is desirable to use at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. The reason is that better properties can be obtained. In addition, at this time, by combining high-viscosity solvents such as ethylene carbonate and propylene carbonate with low-viscosity solvents such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, more excellent properties can be obtained. The reason is that the dissociation and ion mobility of the electrolyte salt will increase.
[0267] When using an alloy-based negative electrode, it is particularly desirable to include at least one of a halogenated chain carbonate or a halogenated cyclic carbonate as a solvent. Thus, during charge and discharge, particularly during charging, a stable coating will be formed on the surface of the negative electrode active material. Here, a halogenated chain carbonate refers to a chain carbonate having a halogen as a constituent element (at least one hydrogen has been replaced by a halogen). In addition, a halogenated cyclic carbonate refers to a cyclic carbonate having a halogen as a constituent element (that is, at least one hydrogen has been replaced by a halogen).
[0268] The type of halogen is not particularly limited, but fluorine is preferred. The reason is that it forms a film of better quality than other halogens. In addition, the more halogens there are, the more ideal it is. The reason is that the resulting film will be more stable and the decomposition reaction of the electrolyte will be reduced.
[0269] Examples of the halogenated chain carbonate include fluoromethyl methyl carbonate, difluoromethyl methyl carbonate, etc. Examples of the halogenated cyclic carbonate include 4-fluoro-1,3-dioxolane-2-one, 4,5-difluoro-1,3-dioxolane-2-one, etc.
[0270] As the solvent additive, it is preferred to include unsaturated carbon bonded cyclic carbonate. The reason is that a stable coating will be formed on the negative electrode surface during charge and discharge, which can inhibit the decomposition reaction of the electrolyte. As the unsaturated carbon bonded cyclic carbonate, for example, vinylene carbonate or vinyl ethylene carbonate can be listed.
[0271] Furthermore, as the solvent additive, it is preferable to contain sultone (cyclic sulfonate) because the chemical stability of the battery is improved. Examples of sultone include propane sultone and propene sultone.
[0272] Furthermore, it is preferred that the solvent contains an acid anhydride. This is because the chemical stability of the electrolyte solution is improved. Examples of the acid anhydride include propanedisulfonic anhydride.
[0273] The electrolyte salt may include, for example, one or more light metal salts such as lithium salts. Examples of lithium salts include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).
[0274] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent because high ion conductivity can be obtained.
[0275] [Method for producing laminated film type secondary battery]
[0276] The laminated film type secondary battery described above can be produced, for example, by the following steps.
[0277] Initially, the positive electrode is made using the above-mentioned positive electrode material. First, the positive electrode active material is mixed with the required positive electrode binder, positive electrode conductive aid, etc. to form a positive electrode mixture, and then dispersed in an organic solvent to form a positive electrode mixture slurry. Then, the mixture slurry is applied to the positive electrode collector using a coating device such as a die coater with a knife roll or a die head, and hot air is dried to obtain a positive electrode active material layer. Finally, the positive electrode active material layer is compression molded using a roller press or the like. At this time, it can be heated and can also be repeatedly compressed multiple times.
[0278] Then, the negative electrode 10 is produced by forming a negative electrode active material layer on the negative electrode current collector in the same operation procedure as that for producing the negative electrode 10 described above.
[0279] When manufacturing the positive electrode and the negative electrode, each active material layer is formed on both sides of the positive electrode and the negative electrode current collector. At this time, in any electrode, the length of the active material coating on both sides can be deviated (refer to Figure 4 ).
[0280] Then, prepare the electrolyte. Then, by ultrasonic welding or the like, the positive lead 32 is installed on the positive electrode collector, and the negative lead 33 is installed on the negative electrode collector. Then, the positive electrode and the negative electrode are stacked across the separator, and then the electrode body 31 is wound to make the wound electrode body, and the protective tape is bonded to its outermost part. Then, the wound electrode body 31 is formed in a flat shape. Then, the wound electrode body 31 is sandwiched between the folded film-like outer packaging members 35, and then the insulating parts of the outer packaging members are bonded to each other by a thermal welding method, and the wound electrode body 31 is sealed in a state open in only one direction. Then, the sealing film 34 is inserted between the positive lead 32 and the outer packaging member 35 and the negative lead 33 and the outer packaging member 35. Then, a predetermined amount of the above-prepared electrolyte is added from the open portion, and vacuum impregnation is performed. After impregnation, the open portion is bonded by a vacuum thermal welding method. The laminated film type secondary battery 30 can be manufactured in the above manner.
[0281] In the non-aqueous electrolyte secondary batteries such as the laminated film type secondary battery 30 prepared above, the negative electrode utilization rate during charge and discharge is preferably 93% or more and 99% or less. If the negative electrode utilization rate is set to a range of more than 93%, the initial charge and discharge efficiency will not decrease, and the battery capacity can be greatly improved. In addition, if the negative electrode utilization rate is set to a range of less than 99%, Li will not precipitate, and safety can be ensured.
[0282] Example
[0283] Hereinafter, the present invention will be specifically described using Examples and Comparative Examples, but the present invention is not limited thereto.
[0284] (Examples 1 to 3)
[0285] First, the negative electrode active material is prepared in the following manner. A raw material obtained by mixing metal silicon and silicon dioxide is introduced into a reactor. In the reactor, the raw material is vaporized in an atmosphere with a vacuum degree of 10 Pa and deposited on an adsorption plate. After sufficient cooling, the deposit is taken out and crushed using a ball mill. The SiO2 content of the silicon oxide particles obtained in this way is 1.347 W / m2. x The value of x is 1.0.
[0286] Then, the particle size of the silicon oxide particles is adjusted by classification. Then, lithium is inserted into the silicon oxide particles by a redox method using an ether solvent in which the water content has been reduced to 50 ppm, thereby modifying the silicon oxide particles. Thus, silicon compound particles containing Li silicate are obtained.
[0287] The obtained silicon compound particles were analyzed by X-ray photoelectron spectroscopy (XPS), and the results showed that the surfaces of the silicon compound particles were coated with a Li compound different from Li silicate.
[0288] The obtained silicon compound particles were then washed with diethyl ether to form particles having a surface carbon component (C component constituting a Li compound other than Li silicate) of 0.2 mass %. Thus, a portion of the Li compound present on the surface of the silicon compound particles was removed, and a portion remained.
[0289] Then, the thoroughly washed particles are added to a solution in which diethyl ether and aluminum sec-butoxide are dispersed, and the mixture is stirred at 100° C. and 500 rpm for 3 hours. The powder is filtered and dried at a temperature in the range of 100° C. to 400° C. to form an aluminum oxide layer. Thus, an intermediate layer is obtained, which covers the surface of the silicon compound particles and contains a Li compound different from Li silicate and aluminum oxide.
[0290] Then, pyrolytic CVD is performed in the range of 450° C. to 650° C., thereby further coating the intermediate layer covering the surface of the silicon compound particles with a carbon layer and changing the type of Li silicate contained in the silicon compound particles.
[0291] In the above manner, each negative electrode active material of Examples 1 to 3 including negative electrode active material particles was obtained.
[0292] XPS (using XPS / PHI Quantera II) was used to observe each negative electrode active material. The results showed that each negative electrode active material of Examples 1 to 3 contained Figure 1 The negative electrode active material particles 1 having the structure described above are shown in FIG. Observation using XPS will be described in detail in the following paragraphs.
[0293] In addition, Li silicate contained in the negative electrode active material particles of each negative electrode active material was analyzed using NMR. The analysis conditions were set to the conditions shown above. The analysis results are shown in Table 1 below.
[0294] In addition, the median particle size of the negative electrode active material particles contained in each negative electrode active material, and the ratio of the intensity A of the peak caused by the Si (111) crystal plane to the intensity B of the peak caused by the Li2SiO3 (111) crystal plane (peak intensity ratio A / B) are shown in the following Table 1. In addition, the intensity ratio A / B is confirmed by XRD. In addition, it is confirmed by XRD that the Si contained in each negative electrode active material is amorphous.
[0295] Then, the negative electrode active material prepared in the above manner (an active material comprising silicon compound particles coated with an intermediate layer and a carbon layer in sequence), graphite, conductive aid 1 (carbon nanotube, CNT), conductive aid 2 (carbon particles with a median particle size of about 50 nm), sodium polyacrylate, and carboxymethyl cellulose (hereinafter referred to as CMC) were mixed at a dry mass ratio of 9.3:83.7:1:1:4:1, and diluted with pure water to prepare a negative electrode mixture slurry. The materials were mixed using a mass production machine and a high shear force was applied to obtain a slurry.
[0296] At this time, the stability of the slurry during mass production was observed based on the usable time, and whether it was stable after 48 hours was confirmed. This can be determined by whether hydrogen gas is generated from the slurry. The results are shown in Table 3 below.
[0297] In addition, as the negative electrode collector, an electrolytic copper foil with a thickness of 15 μm was used. The electrolytic copper foil contained carbon and sulfur at a concentration of 70 mass ppm respectively. Finally, the negative electrode mixture slurry was applied to the negative electrode collector and dried at 100°C in a vacuum atmosphere for 1 hour. After drying, the deposition amount of the negative electrode active material layer per unit area of a single side of the negative electrode (also called area density) was 7.0 mg / cm 2 .
[0298] [Assembly of button batteries for testing]
[0299] Then, ethylene carbonate (EC) and dimethyl carbonate (DMC) as solvents are mixed, and electrolyte salt (lithium hexafluorophosphate: LiPF6) is dissolved to prepare an electrolyte solution. At this time, the composition of the solvent is set to EC:DMC=30:70 by volume, and the content of the electrolyte salt is set to 1 mol / kg relative to the solvent. Vinylene carbonate (VC) and fluoroethylene carbonate (FEC) are added as additives in an amount of 1.0% by mass and 2.0% by mass, respectively.
[0300] Then, the coin cell was assembled in the following manner: First, a Li foil having a thickness of 1 mm was punched out to a diameter of 16 mm and then attached to the aluminum coating layer.
[0301] Then, the negative electrode obtained previously was punched into a diameter of 15 mm, and was placed opposite to the Li foil attached to the aluminum coating layer via a separator, and an electrolyte was injected to produce a 2032 coin cell.
[0302] [Determination of initial efficiency]
[0303] The initial efficiency was measured under the following conditions. First, for the button cell produced for the initial efficiency test, the charging rate was set to 0.03C and charged in CCCV (constant current constant voltage) mode (initial charge). CV was set to 0V and the cutoff current was set to 0.04mA. Then, the discharge rate was also set to 0.03C, the discharge cutoff voltage was set to 1.2V, and CC discharge (initial discharge) was performed.
[0304] When investigating the initial charge and discharge characteristics, the initial efficiency (hereinafter sometimes referred to as initial efficiency) is calculated. The initial efficiency is calculated according to the formula represented by initial efficiency (%) = (initial discharge capacity / initial charge capacity) × 100. The results are shown in Table 3 below as initial efficiency.
[0305] [Manufacturing and evaluation of lithium-ion secondary batteries]
[0306] Based on the obtained initial data, the counter positive electrode was designed so that the utilization rate of the negative electrode was 95%. The utilization rate was calculated based on the capacity of the positive and negative electrodes obtained by the counter electrode Li according to the following formula.
[0307] Utilization rate = (positive electrode capacity - negative electrode loss) / (negative electrode capacity - negative electrode loss) × 100
[0308] Based on this design, lithium ion secondary batteries were manufactured in Examples 1 to 3. Battery evaluation was performed on the lithium ion secondary batteries of Examples and Comparative Examples.
[0309] The cycle characteristics were investigated in the following manner. Initially, in order to stabilize the battery, two cycles of charge and discharge were performed at 0.2C in an atmosphere of 25°C, and the discharge capacity of the second cycle was measured. The battery cycle characteristics were calculated based on the discharge capacity of the third cycle, and the battery test was stopped when the number of cycles was 100. Charge and discharge were performed at 0.7C for charge and 0.5C for discharge. The charging voltage was set to 4.3V, the discharge cutoff voltage was set to 2.5V, and the charging cutoff rate was set to 0.07C. The results are shown in Table 3 below.
[0310] (Comparative Examples 1 to 3)
[0311] In Comparative Examples 1 to 3, after Li doping (embedding), a strong shear force was applied and the particles were washed three times in diethyl ether (filtering-washing was performed three times), thereby removing all Li compounds different from Li silicate present on the surface of the silicon compound particles and not forming an aluminum oxide layer. In addition, each negative electrode active material of Comparative Examples 1 to 3 was obtained in the same manner as in Examples 1 to 3.
[0312] The negative electrode active materials of Comparative Examples 1 to 3 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that the stability of mass-produced slurries was significantly reduced. The mass-produced slurries require a durability of at least 2 days (48 hours), which was not satisfactory.
[0313] (Comparative Example 4)
[0314] In Comparative Example 4, SiO particles coated with a carbon layer on the surface by CVD at 600°C were subjected to Li doping treatment to obtain carbon-coated silicon compound particles. Then, aluminum isopropoxide was dispersed in isopropanol (IPA), and the carbon-coated silicon compound particles were added thereto, and stirred and dried to form a metal oxide (aluminum oxide) layer on the carbon layer. Thus, the negative electrode active material of Comparative Example 4 was obtained.
[0315] Figure 6 Schematic diagram of negative electrode active material particles included in the negative electrode active material of Comparative Example 4 is shown in FIG.
[0316] The negative electrode active material particles 8 included in the negative electrode active material of Comparative Example 4 include silicon compound particles 2, and the silicon compound particles 2 include Si phase 3. The silicon compound particles 2 include Li silicate by lithium doping (intercalation). The surface of the silicon compound particles 2 is coated with a carbon layer 7. The surface of the carbon layer 7 is coated with a layer 6 of aluminum oxide as the outermost layer.
[0317] Between the silicon compound particles 2 and the carbon layer 7 , there is no Li compound other than Li silicate, and no metal oxide and / or metal hydroxide.
[0318] The negative electrode active material of Comparative Example 4 was tested in the same manner as in Example 1. The results are shown in Table 3, and stability during 48 hours of mass production slurrying could not be obtained. In addition, when the negative electrode active material of Comparative Example 4 was slurried using a small machine, stability during 48 hours of slurrying could be achieved.
[0319] (Examples 1 to 3)
[0320] From the results shown in Table 3, it was confirmed that Examples 1 to 3 could achieve durability of 48 hours or more when slurried in mass production.
[0321] Furthermore, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 1 to 3 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 4, and can achieve sufficient battery cycle characteristics.
[0322] (Examples 4 to 15)
[0323] In Examples 4 to 15, each negative electrode active material was prepared in the same manner as in Example 1 except that the starting material (metal alkoxide type) for forming the metal oxide was changed as shown in Table 1 below.
[0324] The negative electrode active materials of Examples 4 to 15 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that, like Examples 1 to 3, the negative electrode active materials of Examples 4 to 15 could achieve durability of 48 hours or more in mass production slurry.
[0325] Furthermore, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 4 to 15 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 4, and can achieve sufficient battery cycle characteristics.
[0326] (Examples 16 to 18)
[0327] In Examples 16 to 18, each negative electrode active material was prepared in the same manner as in Example 1 except that the aluminum oxide layer was not formed.
[0328] The negative electrode active materials of Examples 16 to 18 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that, like Examples 1 to 3, the negative electrode active materials of Examples 16 to 18 could achieve durability of 48 hours or more in mass production slurry.
[0329] Furthermore, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 16 to 18 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 4, and can achieve sufficient battery cycle characteristics.
[0330] (Examples 19 to 24)
[0331] In Examples 19 to 24, each negative electrode active material was prepared in the same manner as in Example 1, except that the amount of aluminum sec-butoxide added to form the aluminum oxide layer was changed to vary the thickness of the aluminum oxide layer.
[0332] The negative electrode active materials of Examples 19 to 24 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that, like Examples 1 to 3, the negative electrode active materials of Examples 19 to 24 could achieve durability of 48 hours or more in mass production slurry.
[0333] In addition, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 19 to 24 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 3, and can achieve sufficient battery cycle characteristics. Further, the negative electrode active materials of Examples 19 to 23 can show a higher capacity retention rate than the negative electrode active material of Comparative Example 4, and can further achieve sufficient battery cycle characteristics.
[0334] The above results show that even when the aluminum oxide layer is 0.1 nm, sufficient characteristics are exhibited. However, if the aluminum oxide layer is thicker, the cycle characteristics tend to decrease due to increased resistance, and it can be said that there is an optimal range.
[0335] (Examples 25 to 29)
[0336] In Examples 25 to 29, after forming the outermost carbon layer, the negative electrode active material particles were subjected to an additional heat treatment to change the crystallinity of Si and Li silicates. Each negative electrode active material was prepared in the same manner as in Example 1 except that the temperature was adjusted within the range of 600 to 700°C.
[0337] The negative electrode active materials of Examples 25 to 29 before charge and discharge were analyzed by X-ray diffraction (XRD) using Cu—Kα rays.
[0338] Based on the XRD chart obtained by XRD analysis, the ratio A / B of the intensity A of the peak (appearing near 2θ=28.4°) caused by the Si(111) crystal plane to the intensity B of the peak (appearing in the range of 2θ=17°~24°) caused by the Li2SiO3(111) crystal plane was calculated. In addition, based on the peak caused by the Si(111) crystal plane, the grain size corresponding to the Si(111) crystal plane was calculated based on the Scherrer equation.
[0339] The results obtained by XRD analysis are shown in the following Table 2. In addition, each negative electrode active material of Examples other than Examples 25 to 29 and Comparative Examples was also analyzed by XRD, and the results are also shown in the following Tables 1 and 2.
[0340] The negative electrode active materials of Examples 25 to 29 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that, like Example 1, the negative electrode active materials of Examples 25 to 29 could achieve durability of 48 hours or more when slurried in mass production.
[0341] In addition, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 25 to 29 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 3, and can achieve sufficient battery cycle characteristics. Further, the negative electrode active materials of Examples 26 to 29 can show a higher capacity retention rate than the negative electrode active material of Comparative Example 4, and can further achieve sufficient battery cycle characteristics.
[0342] Furthermore, from the results of Examples 25 to 29, it can be seen that Examples 26 to 29, in which the grain size corresponding to the Si (111) crystal plane is 5.0 nm or less, show better cycle characteristics than Example 25, in which the grain size corresponding to the Si (111) crystal plane is 9.2 nm or less.
[0343] (Comparative Example 5)
[0344] In Comparative Example 5, a negative electrode active material was prepared in the same manner as in Example 1 except that the outermost carbon layer was not formed.
[0345] The negative electrode active material of Comparative Example 5 was tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that the negative electrode active material of Comparative Example 5 could achieve durability of 48 hours or more in mass production slurry, as in Examples 1 to 3.
[0346] However, as shown in the results in Table 3, the negative electrode active material of Comparative Example 5 showed a lower capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 3. As shown in this result, if the outermost carbon layer is not formed, the conductivity is reduced and sufficient battery characteristics cannot be obtained.
[0347] (Examples 30 to 36)
[0348] In Examples 30 to 36, each negative electrode active material was prepared in the same manner as in Example 1, except that the particle size of the silicon oxide particles was adjusted by classification, thereby changing the median particle size of the negative electrode active material as shown in the following Table 2. The particle sizes of the negative electrode active material particles contained in the negative electrode active materials of other Examples and Comparative Examples are also shown in Tables 1 and 2.
[0349] The negative electrode active materials of Examples 30 to 36 were tested in the same manner as in Example 1. The results are shown in Table 3, and it was confirmed that, like Example 1, the negative electrode active materials of Examples 30 to 36 could achieve durability of 48 hours or more when slurried in mass production.
[0350] In addition, from the results shown in Table 3, it can be seen that the negative electrode active materials of Examples 30 to 36 can show a higher capacity retention rate than the negative electrode active materials of Comparative Examples 1 to 3, and can achieve sufficient battery cycle characteristics. Further, the negative electrode active materials of Examples 31 to 36 can show a higher capacity retention rate than the negative electrode active material of Comparative Example 4, and can further achieve sufficient battery cycle characteristics.
[0351] Furthermore, from the results of Examples 30 to 36, it can be seen that Examples 31 to 35 in which the median particle size of the negative electrode active material particles is greater than 4.5 nm and less than 15 nm show better cycle characteristics than Examples 30 and 36 in which the median particle size of the negative electrode active material particles is 4 nm or 17 nm.
[0352] (Comparative Example 6)
[0353] In Comparative Example 6, silicon oxide particles were obtained by the same procedure as in Example 1, and the particle size of the obtained silicon oxide particles was adjusted by classification. The silicon oxide particles thus obtained were used as the negative electrode active material of Comparative Example 6.
[0354] The negative electrode active material of Comparative Example 6 was tested in the same manner as in Example 1. The results are shown in Table 3, and the initial efficiency was 65%. In contrast, the negative electrode active materials of Examples 1 to 36 of the present invention were able to achieve an initial efficiency of 85% or more.
[0355] The conditions of each example and each comparative example are shown in the following Table 1 and Table 2. In addition, the evaluation results of each example and each comparative example are shown in the following Table 3.
[0356] [Table 1]
[0357]
[0358] [Table 2]
[0359]
[0360] [Table 3]
[0361]
[0362] In addition, although not shown in Table 3, the negative electrode active materials of Examples 1 to 36 can achieve higher capacities than conventional carbon-based negative electrode active materials.
[0363] [Observation of negative electrode active material particles by XPS]
[0364] Using XPS / PHI Quantera II (manufactured by ULVAC-PHI Co., Ltd.), the structure of each negative electrode active material particle was observed by measuring at each depth while dry etching the surface.
[0365] The etching conditions were set to 30 minutes, an acceleration voltage of 2 kV, and an etching range of 2 mm×2 mm.
[0366] Figure 7 Graph 3 shows a part of an XPS spectrum of the negative electrode active material particles included in the negative electrode active material of Example 16 after etching six times.
[0367] Figure 7 The spectrum shown shows multiple peaks of C1s, the peak near 284 eV corresponds to the CC structure, and the peak near 290 eV (indicated by an arrow) corresponds to the OC=O structure. In addition, according to the XPS observation results, Figure 7 The peak corresponding to Li was confirmed in the binding energy region different from the binding energy region shown, thereby confirming the presence of Li. That is, the intermediate layer of the negative electrode active material particles of the negative electrode active material of Example 16 contains a Li compound having an OC=O structure. According to the XPS observation of the negative electrode active material particles contained in each negative electrode active material of Examples 1 to 15 and 17 to 36, the presence of the same Li compound was also confirmed. The presence or absence of "Li, C, O compound" is shown in Tables 1 and 2 above.
[0368] also, Figure 8 2 and 3 show a part of the XPS spectrum of the outermost layer of the negative electrode active material particles contained in the negative electrode active material of Example 1 (solid line) and a part of the XPS spectrum (dashed line) after etching three times.
[0369] Figure 8 The dotted spectrum shown has a peak near 74.4 eV (indicated by an arrow) that is not present in the solid spectrum. This peak corresponds to AlO xIn addition, in the XPS observation result of the surface layer, the presence of C was confirmed. From the above results, it can be seen that the negative electrode active material particles contained in the negative electrode active material of Example 1 include a carbon layer on the outermost surface and an aluminum oxide layer thereunder.
[0370] It was confirmed that the negative electrode active material particles contained in each of the negative electrode active materials of Examples 2 to 15 and 19 to 36 also contained a carbon layer as the outermost layer and a metal oxide layer thereunder.
[0371] In addition, although not shown in Tables 1 and 2 above, in the intermediate layer of the negative electrode active material particles contained in the negative electrode active materials of Examples 1 to 33, the presence of metal hydroxides in addition to metal oxides was also confirmed. It is believed that the reason is that although the alkoxide is converted into a metal oxide by applying heat thereto, a portion of the alkoxide remains inside in the form of a hydroxide. Therefore, in the column of the metal oxide in Tables 1 and 2 above, the amount of oxygen atoms relative to the metal element is marked with x.
[0372] This specification contains the following protocols.
[0373] (1) A negative electrode active material, which is a negative electrode active material comprising negative electrode active material particles, characterized in that the negative electrode active material particles have: silicon compound particles comprising Li silicate; an intermediate layer which covers the surface of the silicon compound particles and comprises a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles; and an outermost carbon layer which has covered the intermediate layer.
[0374] (2) The negative electrode active material according to (1), characterized in that at least a portion of the silicon compound particles contains at least one selected from the group consisting of Li2SiO3, Li4SiO4 and Li6Si2O7 as the Li silicate.
[0375] (3) The negative electrode active material according to (1) or (2), wherein the intermediate layer contains the Li compound, and the Li compound is a composite compound containing Li, C, and O.
[0376] (4) The negative electrode active material according to (3), characterized in that, in the C1s waveform obtained from the XPS spectrum, at least a portion of the composite compound containing Li, C, and O has an OC═O structure.
[0377] (5) The negative electrode active material according to any one of (1) to (4), characterized in that the intermediate layer contains the metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide contains at least one element selected from the group consisting of aluminum, magnesium, titanium, zirconium, calcium and niobium.
[0378] (6) The negative electrode active material according to (5), characterized in that the thickness of the metal oxide and / or metal hydroxide in the intermediate layer is 0.1 nm or more and 10 nm or less.
[0379] (7) The negative electrode active material according to any one of (1) to (6), characterized in that the intermediate layer contains the Li compound and the metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide covers the Li compound.
[0380] (8) The negative electrode active material according to any one of (1) to (7), characterized in that before the negative electrode active material particles are charged and discharged, the negative electrode active material particles have a peak originating from the Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα rays, the grain size corresponding to the crystal plane is 5.0 nm or less, and the ratio A / B of the intensity A of the peak originating from the Si (111) crystal plane to the intensity B of the peak originating from the Li2SiO3 (111) crystal plane satisfies the following formula (1):
[0381] 0.4≤A / B≤1.0 …(1).
[0382] (9) The negative electrode active material according to any one of (1) to (8), wherein the negative electrode active material particles have a median particle size of 4.5 μm or more and 15 μm or less.
[0383] (10) A method for producing a negative electrode active material, which is a method for producing a negative electrode active material containing negative electrode active material particles, characterized in that it comprises: preparing a negative electrode active material having a general formula of SiO x The process of producing silicon oxide particles represented by the present invention, wherein 0.5≤x≤1.6; the process of embedding Li into the silicon oxide particles to produce silicon compound particles containing Li silicate; the process of forming an intermediate layer on the surface of the silicon compound particles, wherein the intermediate layer contains a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particles, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particles; the process of forming an outermost carbon layer covering the intermediate layer to obtain negative electrode active material particles; and the process of using the negative electrode active material particles to produce a negative electrode active material.
[0384] (11) A method for producing a negative electrode active material according to (10), characterized in that, in the step of producing silicon compound particles containing Li silicate, silicon compound particles whose surfaces contain the Li compound are produced, and in the step of forming an intermediate layer, a portion of the Li compound present on the surface of the silicon compound particles is removed, and a portion of the surface of the silicon compound particles and the surface of the Li compound are coated with a metal oxide and / or a metal hydroxide, thereby forming the intermediate layer containing the metal oxide and / or the metal hydroxide and the Li compound.
[0385] (12) The method for producing a negative electrode active material according to (11), characterized in that, in the step of forming the intermediate layer, the metal oxide and / or the metal hydroxide is formed by hydrolysis and dehydration condensation of a metal alkoxide.
[0386] In addition, the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are examples, and any technical solutions having substantially the same structure and exerting the same technical effects as the technical concept described in the claims of the present invention are included in the technical scope of the present invention.
Claims
1. A negative electrode active material, comprising negative electrode active material particles, characterized in that: The negative electrode active material particles have: Silicon compound particles comprising Li silicate; an intermediate layer covering the surface of the silicon compound particle and comprising a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle; and The outermost carbon layer has covered the intermediate layer.
2. The negative electrode active material according to claim 1, characterized in that At least a portion of the silicon compound particles includes at least one selected from the group consisting of Li2SiO3, Li4SiO4 and Li6Si2O7 as the Li silicate.
3. The negative electrode active material according to claim 1 or 2, characterized in that: The intermediate layer includes the Li compound, and the Li compound is a composite compound including Li, C, and O.
4. The negative electrode active material according to claim 3, characterized in that In the C1s waveform obtained from the XPS spectrum, at least a portion of the composite compound including Li, C, and O has an OC═O structure.
5. The negative electrode active material according to any one of claims 1 to 4, characterized in that The intermediate layer includes the metal oxide and / or the metal hydroxide, and the metal oxide and / or the metal hydroxide includes at least one element selected from the group consisting of aluminum, magnesium, titanium, zirconium, calcium, and niobium.
6. The negative electrode active material according to claim 5, characterized in that The thickness of the metal oxide and / or metal hydroxide in the intermediate layer is greater than or equal to 0.1 nm and less than or equal to 10 nm.
7. The negative electrode active material according to any one of claims 1 to 6, characterized in that The intermediate layer includes the Li compound and the metal oxide and / or metal hydroxide, and the metal oxide and / or metal hydroxide covers the Li compound.
8. The negative electrode active material according to any one of claims 1 to 7, characterized in that Before the negative electrode active material particles are charged and discharged, the negative electrode active material particles have a peak originating from the Si (111) crystal plane obtained by X-ray diffraction using Cu-Kα rays, the grain size corresponding to the crystal plane is 5.0 nm or less, and the ratio A / B of the intensity A of the peak originating from the Si (111) crystal plane to the intensity B of the peak originating from the Li2SiO3 (111) crystal plane satisfies the following formula (1): 0.4≤A / B≤1.0 …(1).
9. The negative electrode active material according to any one of claims 1 to 8, characterized in that The negative electrode active material particles have a median particle size of 4.5 μm or more and 15 μm or less.
10. A method for producing a negative electrode active material, which is a method for producing a negative electrode active material containing negative electrode active material particles, characterized in that: include: Made of general formula SiO x The process of silicon oxide particles represented by , wherein 0.5≤x≤1.6; A step of inserting Li into the silicon oxide particles to prepare silicon compound particles containing Li silicate; A step of forming an intermediate layer on the surface of the silicon compound particle, wherein the intermediate layer comprises a Li compound different from the Li silicate adjacent to a portion of the surface of the silicon compound particle, and / or a metal oxide and / or a metal hydroxide adjacent to at least a portion of the surface of the silicon compound particle; forming a carbon layer covering the outermost layer of the intermediate layer to obtain negative electrode active material particles; and A process of manufacturing a negative electrode active material using the negative electrode active material particles.
11. The method for producing a negative electrode active material according to claim 10, characterized in that: In the step of preparing silicon compound particles containing Li silicate, silicon compound particles whose surfaces contain the Li compound are prepared. In the step of forming the intermediate layer, a portion of the Li compound present on the surface of the silicon compound particles is removed, and a portion of the surface of the silicon compound particles and the surface of the Li compound are coated with a metal oxide and / or a metal hydroxide, thereby forming the intermediate layer comprising the metal oxide and / or the metal hydroxide and the Li compound.
12. The method for producing a negative electrode active material according to claim 11, characterized in that: In the step of forming the intermediate layer, the metal oxide and / or the metal hydroxide is formed by hydrolysis and dehydration condensation of the metal alkoxide.