Substrate for printed wiring board, printed wiring board, and multilayer printed wiring board
By employing an alternating layered structure of polyimide and fluoropolymer layers in the printed wiring board, combined with an electrolytic or rolled copper foil conductive layer, the problem of balancing high-frequency characteristics and flexibility is solved, achieving low transmission loss and good flexibility.
Patent Information
- Application Number
- CN202380025809.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-01
AI Technical Summary
Existing technologies struggle to balance the high-frequency characteristics and flexibility of printed wiring boards.
The insulating layer consists of multiple alternating layers of polyimide and fluoropolymer, with the fluoropolymer layer as the outermost layer. The total thickness of the polyimide layers does not exceed 0.95 times the thickness of the insulating layer. Electrolytic or rolled copper foil is used as the conductive layer.
It achieves excellent high-frequency characteristics and flexibility, low transmission loss, and can avoid warping under small bending radii, ensuring the patterning quality of the conductive layer.
Smart Images

Figure CN118891960A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a substrate for a printed wiring board, a printed wiring board, and a multilayer printed wiring board. This application claims priority based on Japanese patent application No. 2022-053269 filed on March 29, 2022. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art
[0002] International Publication No. 2010 / 084867 (Patent Document 1) describes a multilayer fluororesin film. The multilayer fluororesin film described in Patent Document 1 is used, for example, for a printed wiring board. The multilayer fluororesin film described in Patent Document 1 has three polyimide films and two fluororesin films. In the multilayer fluororesin film described in Patent Document 1, the polyimide film and the fluororesin film are alternately stacked in such a manner that the polyimide film becomes the outermost layer. Copper foil is disposed on the outermost polyimide film.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2010 / 084867 Summary of the invention
[0006] The printed wiring board substrate disclosed in the present invention comprises an insulating layer, a first copper foil and a second copper foil. The insulating layer comprises a first main surface and a second main surface which is a surface opposite to the first main surface. The insulating layer comprises a plurality of polyimide layers and a plurality of fluororesin layers. The total number of the plurality of polyimide layers and the number of the plurality of fluororesin layers is 5 or more. Each of the plurality of polyimide layers and each of the plurality of fluororesin layers are alternately stacked along the thickness direction of the insulating layer. One of the plurality of fluororesin layers becomes the outermost layer on the first main surface side, namely the first outermost layer. Another of the plurality of fluororesin layers becomes the outermost layer on the second main surface side, namely the second outermost layer. The thickness of the first outermost layer and the thickness of the second outermost layer are greater than 1.0 μm and less than 50 μm. The value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer is less than 0.95. The first copper foil and the second copper foil are respectively arranged on the first main surface and the second main surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 It is a cross-sectional view of the printed wiring board substrate 100 .
[0008] Figure 2 is a cross-sectional view of the printed wiring board 200 .
[0009] Figure 3 is a cross-sectional view of a multilayer printed wiring board 300 . DETAILED DESCRIPTION
[0010] [Technical Problems to be Solved by the Present Disclosure]
[0011] However, in the multilayer fluororesin film described in Patent Document 1, it is difficult to achieve both good high-frequency characteristics and good bendability.
[0012] The present disclosure is made in view of the above-mentioned problems of the prior art. More specifically, the present disclosure provides a printed wiring board substrate, a printed wiring board, and a multilayer printed wiring board that can achieve both good high-frequency characteristics and good bendability.
[0013] [Effects of the present disclosure]
[0014] According to the printed wiring board substrate of the present disclosure, it is possible to achieve both good high frequency characteristics and good bendability.
[0015] [Description of Embodiments of the Present Disclosure]
[0016] First, embodiments of the present disclosure will be listed and described.
[0017] (1) The printed wiring board substrate according to the embodiment comprises an insulating layer, a first copper foil and a second copper foil. The insulating layer comprises a first main surface and a second main surface which is a surface opposite to the first main surface. The insulating layer comprises a plurality of polyimide layers and a plurality of fluororesin layers. The total number of the plurality of polyimide layers and the number of the plurality of fluororesin layers is 5 or more. Each of the plurality of polyimide layers and each of the plurality of fluororesin layers are alternately stacked along the thickness direction of the insulating layer. One of the plurality of fluororesin layers becomes the outermost layer on the first main surface side, namely the first outermost layer. Another of the plurality of fluororesin layers becomes the outermost layer on the second main surface side, namely the second outermost layer. The thickness of the first outermost layer and the thickness of the second outermost layer are greater than 1.0 μm and less than 50 μm. The value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer is less than 0.95. The first copper foil and the second copper foil are respectively arranged on the first main surface and the second main surface.
[0018] According to the printed wiring board substrate of (1) above, both good high frequency characteristics and good bendability can be achieved.
[0019] (2) In the printed wiring board substrate of (1) above, the plurality of fluororesin layers may be formed of at least one selected from the group consisting of tetrafluoroethylene-hexafluoropropylene copolymers, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymers, and polytetrafluoroethylene.
[0020] (3) In the printed wiring board substrate of (1) or (2) above, the plurality of polyimide layers may be formed of a polyimide having a relative dielectric constant of 2 or more and 4 or less.
[0021] According to the printed wiring board substrate of (3) above, it is possible to further ensure good high frequency characteristics.
[0022] (4) In the printed wiring board substrates of (1) to (3) above, the first copper foil and the second copper foil may be formed of electrolytic copper foil.
[0023] (5) In the printed wiring board substrates of (1) to (3) above, the first copper foil and the second copper foil may be rolled copper foils.
[0024] According to the printed wiring board substrate of (5) above, it is possible to ensure further good bendability.
[0025] (6) In the printed wiring board substrate of (1) to (5) above, the thermal expansion coefficient of the insulating layer may be 16.0 ppm / K or more and 100 ppm / K or less.
[0026] (7) In the printed wiring board substrates of (1) to (6) above, the thickness of the insulating layer may be 170 μm or less.
[0027] According to the printed wiring board substrate of (7) above, it is possible to ensure further good bendability.
[0028] (8) The printed wiring board involved in the embodiment comprises an insulating layer, a first wiring and a second wiring. The insulating layer has a first main surface and a second main surface which is a surface opposite to the first main surface. The insulating layer has a plurality of polyimide layers and a plurality of fluororesin layers. The total number of the plurality of polyimide layers and the number of the plurality of fluororesin layers is 5 or more. Each of the plurality of polyimide layers and each of the plurality of fluororesin layers are alternately stacked along the thickness direction of the insulating layer. One of the plurality of fluororesin layers becomes the outermost layer on the first main surface side, namely the first outermost layer. Another of the plurality of fluororesin layers becomes the outermost layer on the second main surface side, namely the second outermost layer. The thickness of the first outermost layer and the thickness of the second outermost layer are greater than 1.0 μm and less than 50 μm. The value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer is less than 0.95. The first wiring and the second wiring are respectively arranged on the first main surface and the second main surface.
[0029] According to the printed wiring board of (8) above, it is possible to achieve both good high frequency characteristics and good bendability.
[0030] (9) In the printed wiring board of (8) above, a transmission loss per 100 mm of the first wiring at 50 GHz and a transmission loss per 100 mm of the second wiring at 50 GHz may be 7 dB or less.
[0031] According to the printed wiring board of (9) above, it is possible to further ensure good high frequency characteristics.
[0032] (10) A multilayer printed wiring board according to an embodiment includes a plurality of printed wiring boards. Each of the plurality of printed wiring boards is the printed wiring board according to (8) or (9) above.
[0033] According to the multilayer printed wiring board of (10) above, it is possible to achieve both good high frequency characteristics and good bendability.
[0034] [Details of the embodiments of the present disclosure]
[0035] The details of the embodiments of the present disclosure will be described with reference to the drawings. In the following drawings, the same or corresponding parts are denoted by the same reference numerals, and repeated description will not be repeated.
[0036] (Printed wiring board substrate according to the embodiment)
[0037] A printed wiring board substrate according to an embodiment will be described. Hereinafter, the printed wiring board substrate according to an embodiment is referred to as a printed wiring board substrate 100 .
[0038] <Structure of printed wiring board substrate 100>
[0039] Hereinafter, the structure of the printed wiring board substrate 100 will be described.
[0040] Figure 1 1 is a cross-sectional view of a printed wiring board substrate 100. Figure 1 As shown, the printed wiring board substrate 100 includes an insulating layer 10 , a first copper foil 20 , and a second copper foil 30 .
[0041] The insulating layer 10 has a first main surface 10a and a second main surface 10b. The first main surface 10a and the second main surface 10b are end surfaces of the insulating layer 10 in the thickness direction. The thickness of the insulating layer 10 is defined as thickness T1. Thickness T1 is, for example, 170 μm or less.
[0042] The thermal expansion coefficient of the insulating layer 10 is preferably 16.0 ppm / K or more and 100 ppm / K or less. The thermal expansion coefficient of the insulating layer 10 is measured by thermomechanical analysis (TMA). The thermal expansion coefficient of the insulating layer 10 is measured in the in-layer direction of the insulating layer 10. The in-layer direction of the insulating layer 10 refers to a direction orthogonal to the thickness direction of the insulating layer 10.
[0043] The insulating layer 10 has a plurality of polyimide layers 11 and a plurality of fluororesin layers 12. The total number of the plurality of polyimide layers 11 and the number of the plurality of fluororesin layers 12 is 5 or more.
[0044] A plurality of polyimide layers 11 and a plurality of fluororesin layers 12 are alternately stacked in the thickness direction of the insulating layer 10. The first outermost layer (the layer closest to the first main surface 10a) of the insulating layer 10 and the second outermost layer (the layer closest to the second main surface 10b) of the insulating layer 10 are fluororesin layers 12. The fluororesin layer 12 to be the first outermost layer is set as fluororesin layer 12a. The fluororesin layer 12 to be the second outermost layer is set as fluororesin layer 12b.
[0045] The thickness of the polyimide layer 11 is set to thickness T2. The value obtained by dividing the total thickness T2 of the plurality of polyimide layers 11 by the thickness T1 is 0.95 or less. The value obtained by dividing the total thickness T2 of the plurality of polyimide layers 11 by the thickness T1 is preferably 0.25 or less. The value obtained by dividing the total thickness T2 of the plurality of polyimide layers 11 by the thickness T1 may also be 0.20 or less. The thickness T2 is, for example, 12 μm or more and 25 μm or less.
[0046] The thickness of the fluororesin layer 12 is set to thickness T3. The thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b is 1.0 μm or more and 50 μm or less. The thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b is preferably 3.0 μm or more and 25 μm or less. The thickness T3 of the fluororesin layer 12 other than the fluororesin layer 12a and the fluororesin layer 12b may be different from the thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b. The thickness T3 of the fluororesin layer 12 other than the fluororesin layer 12a and the fluororesin layer 12b is, for example, greater than the thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b. The thickness T3 of the fluororesin layer 12 other than the fluororesin layer 12a and the fluororesin layer 12b is preferably 100 μm or more and 140 μm or less.
[0047] The polyimide layer 11 is preferably formed of a polyimide having a relative dielectric constant of 2 to 4. The relative dielectric constant of the polyimide layer 11 is measured by a cavity resonator method specified in JIS C 2565. The polyimide layer 11 is formed of, for example, Kapton (registered trademark) EN-C.
[0048] The fluororesin layer 12 is formed of, for example, at least one selected from the group consisting of a tetrafluoroethylene-hexafluoropropylene copolymer, a tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and polytetrafluoroethylene.
[0049] The first copper foil 20 and the second copper foil 30 are disposed on the first main surface 10a and the second main surface 10b, respectively. The first copper foil 20 and the second copper foil 30 are formed of, for example, electrolytic copper foils. The first copper foil 20 and the second copper foil 30 may be formed of rolled copper foils.
[0050] The printed wiring board substrate 100 is manufactured by laminating a plurality of polyimide sheets, a plurality of fluororesin sheets, and two copper foils, and then performing vacuum heat pressing. However, the manufacturing method of the printed wiring board substrate 100 is not limited to this.
[0051] <Effects of the printed wiring board substrate 100>
[0052] Hereinafter, the effects of the printed wiring board substrate 100 will be described.
[0053] In a printed wiring board substrate having an insulating layer including a plurality of stacked polyimide layers and a plurality of fluororesin layers, the greater the value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer, the better the bending characteristics are. However, the greater the value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer, the more the high-frequency characteristics tend to deteriorate.
[0054] In the printed wiring board substrate 100 , since the value obtained by dividing the total thickness of the plurality of polyimide layers 11 by the thickness T1 is 0.95 or less, the bending characteristics are improved.
[0055] In addition, in the printed wiring board substrate 100, the first outermost layer in contact with the first copper foil 20 and the second outermost layer in contact with the second copper foil 30 are respectively the fluororesin layer 12a and the fluororesin layer 12b having excellent high-frequency characteristics, and the thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b is 1.0 μm or more and 50 μm or less, so even if the value obtained by dividing the total thickness of the plurality of polyimide layers 11 by the thickness T1 is 0.95 or less, excellent high-frequency characteristics are exhibited. In this way, according to the printed wiring board substrate 100, both good high-frequency characteristics and good bendability can be achieved.
[0056] The first copper foil 20 and the second copper foil 30 are patterned to form wiring, thereby forming a printed wiring board from the printed wiring board substrate 100. When the total number of the plurality of polyimide layers 11 and the number of the plurality of fluororesin layers 12 is less than 5, warping may occur when the first copper foil 20 and the second copper foil 30 are patterned. In the printed wiring board substrate 100, since the total number of the plurality of polyimide layers 11 and the number of the plurality of fluororesin layers 12 is 5 or more, warping can be suppressed when the first copper foil 20 and the second copper foil 30 are patterned.
[0057] When the first copper foil 20 and the second copper foil 30 are formed of rolled copper foil, good bendability can be ensured because the rolled copper foil has good elongation. When the polyimide layer 11 is formed of polyimide having a relative dielectric constant of 2 or more and 4 or less, high-frequency characteristics can be further improved. When the thermal expansion coefficient of the insulating layer 10 is 16 ppm / K or more and 100 ppm / K or less, substrate warping can be suppressed.
[0058] When the thickness T1 is 170 μm or less, good bendability can be ensured. More specifically, in this case, the bending radius of the insulating layer 10 can be set to 0.5 mm or less.
[0059] (Printed wiring board according to embodiment)
[0060] A printed wiring board according to the embodiment will be described. Hereinafter, the printed wiring board according to the embodiment is referred to as printed wiring board 200 .
[0061] <Structure of Printed Wiring Board 200>
[0062] Hereinafter, the structure of the printed wiring board 200 will be described.
[0063] Figure 2 2 is a cross-sectional view of the printed wiring board 200. Figure 2 As shown, the printed wiring board 200 includes an insulating layer 10, first wirings 21, and second wirings 31. The first wirings 21 are arranged on the first main surface 10a, and the second wirings 31 are arranged on the second main surface 10b.
[0064] The printed wiring board 200 is formed using the printed wiring board substrate 100. More specifically, the printed wiring board 200 is formed by patterning the first copper foil 20 to form the first wiring 21 and patterning the second copper foil 30 to form the second wiring 31.
[0065] It should be noted that the patterning of the first copper foil 20 (second copper foil 30) is performed, for example, by pasting a dry film resist on the first copper foil 20 (second copper foil 30), exposing and developing the pasted dry film resist to form a mask, and etching the first copper foil 20 (second copper foil 30) exposed from the opening of the mask.
[0066] In printed wiring board 200, transmission loss per 100 mm of first wiring 21 at 50 GHz and transmission loss per 100 mm of second wiring 31 at 50 GHz are preferably 7 dB or less. Transmission loss of first wiring 21 and transmission loss of second wiring 31 are measured by a network analyzer.
[0067] In the printed wiring board 200, a through hole 10c may be formed in the insulating layer 10. The through hole 10c penetrates the insulating layer 10 in the thickness direction. The through hole 10c is formed to overlap with the pad portion 21a of the first wiring 21 and the pad portion 31a of the second wiring 31 in a plan view.
[0068] The conductor layer 40 is arranged on the inner wall surface of the through hole 10c, the side surface and the upper surface of the pad portion 21a located around the through hole 10c, and the side surface and the upper surface of the pad portion 31a located around the through hole 10c. Thus, the first wiring 21 and the second wiring 31 are electrically connected. It should be noted that the conductor layer 40 can also be filled in the through hole 10c. The conductor layer 40 is formed of copper, for example.
[0069] (Multilayer printed wiring board according to embodiment)
[0070] A multilayer printed wiring board according to the embodiment will be described. Hereinafter, the multilayer printed wiring board according to the embodiment will be referred to as a multilayer printed wiring board 300 .
[0071] <Structure of Multilayer Printed Wiring Board 300>
[0072] Figure 3 3 is a cross-sectional view of a multilayer printed wiring board 300. Figure 3 As shown, the multilayer printed wiring board 300 has a plurality of printed wiring boards 200 . Figure 3 Although two printed wiring boards are shown in FIG. 2 , the number of the plurality of printed wiring boards 200 is not limited thereto.
[0073] The multilayer printed wiring board 300 further includes a bonding layer 50. One of the two adjacent printed wiring boards 200 is set as a printed wiring board 201, and the other of the two adjacent printed wiring boards 200 is set as a printed wiring board 202. The bonding layer 50 is arranged between the first main surface 10a of the printed wiring board 201 and the second main surface 10b of the printed wiring board 202 in a manner covering the first wiring 21 of the printed wiring board 201 and the second wiring 31 of the printed wiring board 202. The bonding layer 50 is formed of, for example, an epoxy-based bonding agent.
[0074] (Example of Printed Wiring Board)
[0075] In order to evaluate the relationship between the thickness T1, thickness T2, the outermost fluororesin layer 12 (fluororesin layer 12a, fluororesin layer 12b) and the thickness T3 of the fluororesin layer 12 other than the outermost layer in the printed wiring board and the transmission loss of the wiring (first wiring 21, second wiring 31), samples A1 to A9 were prepared. In samples A1 to A9, the total number of the plurality of polyimide layers 11 and the total number of the plurality of fluororesin layers 12 was set to 5.
[0076] The thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b is 1 μm or more and 50 μm or less as condition A. The value obtained by dividing the total thickness T2 of the plurality of polyimide layers 11 by the thickness T1 is 0.95 or less as condition B. As shown in Table 1, samples A1 to A9 satisfy condition A and condition B. That is, samples A1 to A9 correspond to the printed wiring board 200.
[0077]
[0078] In addition, as comparative examples, samples A10 and A11 were prepared. The insulating layer of sample A10 was formed only of two polyimide layers 11 (i.e., the thickness T3 of the outermost fluororesin layer 12 and the thickness T3 of the fluororesin layer 12 other than the outermost layer was set to 0). Although not shown in Table 1, the insulating layer of sample A11 was formed only of a layer of a liquid crystal polymer. In sample A11, the thickness of the insulating layer was set to 100 μm.
[0079] The transmission loss of samples A1 to A11 was measured using a microstrip line formed by wiring formed on a printed wiring board and matched to an impedance of 50Ω. In samples A1 to A9, the transmission loss per 100 mm of the wiring at 50 GHz was smaller than that of sample A11. More specifically, in samples A1 to A9, the transmission loss per 100 mm of the wiring at 50 GHz was less than 7 dB. In sample A10, the transmission loss per 100 mm of the wiring at 50 GHz was greater than that of sample A11. It can be seen from this that good high-frequency characteristics can be obtained according to the printed wiring board 200.
[0080] Sample A10 can be bent with a bending radius of 0.5 mm or more. As the thickness T1 decreases, the high-frequency characteristics decrease (the transmission loss of the wiring increases). On the other hand, as the thickness T1 decreases, the bendability improves.
[0081] In addition, even for the samples (samples A1 to A5) whose thickness T1 is 170 μm or less among samples A1 to A9, that is, the samples that can be bent with a bending radius of 0.5 mm or more among samples A1 to A9, the transmission loss per 100 mm of the wiring at 50 GHz is smaller than that of sample A11. It can be seen that according to the printed wiring board 200, both good high-frequency characteristics and good bendability can be achieved.
[0082] In order to evaluate the bendability of samples A4 and A8, a mandrel test specified in JIS K5600-5 was performed. The mandrel test was performed 10 times with a mandrel diameter of 2 mm. The mandrel test was performed in such a way that the microstrip line became a bend. After the mandrel test was performed 10 times with a mandrel diameter of 2 mm, a probe was brought into contact with the pad of the microstrip line arranged at the end of the printed wiring board to determine whether the microstrip line was broken.
[0083]
[0084] As shown in Table 4, in Samples A4 and A8, after the mandrel test was performed 10 times with a mandrel diameter of 2 mm, no breakage of the microstrip line occurred. This shows that the printed wiring board 200 can ensure the bendability.
[0085] (Embodiment of Multilayer Printed Wiring Board)
[0086] In order to evaluate the relationship between the thickness T1, thickness T2 of each printed wiring board included in the multilayer printed wiring board, the outermost fluororesin layer 12 (fluororesin layer 12a, fluororesin layer 12b), and the thickness T3 of the fluororesin layer 12 other than the outermost layer, and the transmission loss of the wiring (first wiring 21, second wiring 31), samples B1 to B25 were prepared. Samples B1 to B25 are composed of two printed wiring boards stacked. In samples B1 to B25, the total number of the plurality of polyimide layers 11 and the number of the plurality of fluororesin layers 12 is set to 5.
[0087] The thickness T3 of the fluororesin layer 12a and the fluororesin layer 12b is 1 μm or more and 50 μm or less as condition A. The value obtained by dividing the total thickness T2 of the plurality of polyimide layers 11 by the thickness T1 is 0.95 or less as condition B. As shown in Table 3, samples B1 to B25 satisfy condition A and condition B. That is, samples B1 to B25 correspond to the multilayer printed wiring board 300.
[0088]
[0089] In addition, as comparative examples, sample B26 and sample B27 were prepared. The insulating layer of sample B26 was formed only of two polyimide layers 11 (i.e., the thickness T3 of the outermost fluororesin layer 12 and the thickness T3 of the fluororesin layer 12 other than the outermost layer were set to 0). Although not shown in Table 3, the insulating layer of sample B27 was formed only of a layer of a liquid crystal polymer. In sample B27, the thickness of the insulating layer was set to 100 μm.
[0090] The transmission loss of samples B1 to B27 was measured using a strip line composed of wiring formed on a multilayer printed wiring board and matched to 50Ω impedance. In samples B1 to B25, the transmission loss per 100mm of the wiring at 50GHz was smaller than that of sample B27. More specifically, in samples B1 to B25, the transmission loss per 100mm of the wiring at 50GHz was less than 7dB. In sample B26, the transmission loss per 100mm of the wiring at 50GHz was greater than that of sample B27. It can be seen from this that according to the multilayer printed wiring board 300, good high-frequency characteristics can be obtained.
[0091] Sample B26 can be bent with a bending radius of 0.5 mm or more. As the thickness T1 decreases, the high-frequency characteristics decrease (the transmission loss of the wiring increases). On the other hand, as the thickness T1 decreases, the bendability improves.
[0092] The samples with thickness T1 of 170 μm or less (samples B1 to B3, B5, B7, B9, and B18 to B25) among samples B1 to B25, i.e., samples that can be bent with a bending radius of 0.5 mm or more, also have lower transmission loss per 100 mm of wiring at 50 GHz than sample B27. It can be seen that the multilayer printed wiring board 300 can achieve both good high frequency characteristics and good bendability.
[0093] In order to evaluate the bendability of samples B7 and B15, a mandrel test specified in JIS K5600-5 was performed. The mandrel test was performed 10 times with a mandrel diameter of 2 mm. The mandrel test was performed in such a way that the strip line became a bend portion. After the mandrel test was performed 10 times with a mandrel diameter of 2 mm, a probe was brought into contact with the pad of the strip line arranged at the end of the multilayer printed wiring board to determine whether the strip line was broken.
[0094]
[0095] As shown in Table 4, in Sample B7 and Sample B15, after the mandrel test was performed 10 times with a mandrel diameter of 2 mm, the strip line was not broken. This shows that the multilayer printed wiring board 300 can ensure the bendability.
[0096] The embodiments disclosed this time should be considered in all respects as illustrative and non-restrictive. The scope of the present invention is indicated by the claims rather than the embodiments described above, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0097] Description of Reference Numerals
[0098] 10 insulating layer; 10a first main surface; 10b second main surface; 10c through hole; 11 polyimide layer; 12 fluororesin layer; 12a, 12b fluororesin layer; 20 first copper foil; 21 first wiring; 21a pad portion; 30 second copper foil; 31 second wiring; 31a pad portion; 40 conductor layer; 50 bonding layer; 100 printed wiring board substrate; 200, 201, 202 printed wiring board; 300 multilayer printed wiring board; T1, T2, T3 thickness.
Claims
1. A printed wiring board substrate, comprising: Insulation layer; and The first copper foil and the second copper foil, The insulating layer has a first main surface and a second main surface which is a surface opposite to the first main surface. The insulating layer has a plurality of polyimide layers and a plurality of fluororesin layers, The total number of the plurality of polyimide layers and the number of the plurality of fluororesin layers is 5 or more, Each of the plurality of polyimide layers and each of the plurality of fluororesin layers are alternately stacked in a thickness direction of the insulating layer, One of the plurality of fluororesin layers serves as the outermost layer on the first main surface side, that is, the first outermost layer. Another one of the plurality of fluororesin layers serves as the outermost layer on the second main surface side, that is, the second outermost layer. The thickness of the first outermost layer and the thickness of the second outermost layer are 1.0 μm or more and 50 μm or less, The value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer is 0.95 or less, The first copper foil and the second copper foil are disposed on the first main surface and the second main surface, respectively.
2. The printed wiring board substrate according to claim 1, The plurality of fluororesin layers are formed of at least one selected from the group consisting of tetrafluoroethylene-hexafluoropropylene copolymer, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, and polytetrafluoroethylene.
3. The printed wiring board substrate according to claim 1 or 2, The plurality of polyimide layers are formed of polyimide having a relative dielectric constant of 2 or more and 4 or less.
4. The printed wiring board substrate according to any one of claims 1 to 3, The first copper foil and the second copper foil are formed of electrolytic copper foil.
5. The printed wiring board substrate according to any one of claims 1 to 3, The first copper foil and the second copper foil are formed of rolled copper foil.
6. The printed wiring board substrate according to any one of claims 1 to 5, The thermal expansion coefficient of the insulating layer is greater than or equal to 16.0 ppm / K and less than or equal to 100 ppm / K.
7. The printed wiring board substrate according to any one of claims 1 to 6, The thickness of the insulating layer is less than 170 μm.
8. A printed wiring board comprising: Insulation layer; and a first wiring and a second wiring, The insulating layer has a first main surface and a second main surface which is a surface opposite to the first main surface. The insulating layer has a plurality of polyimide layers and a plurality of fluororesin layers, The total number of the plurality of polyimide layers and the number of the plurality of fluororesin layers is 5 or more, Each of the plurality of polyimide layers and each of the plurality of fluororesin layers are alternately stacked in a thickness direction of the insulating layer, One of the plurality of fluororesin layers serves as the outermost layer on the first main surface side, that is, the first outermost layer. Another one of the plurality of fluororesin layers serves as the outermost layer on the second main surface side, that is, the second outermost layer. The thickness of the first outermost layer and the thickness of the second outermost layer are 1.0 μm or more and 50 μm or less, The value obtained by dividing the total thickness of the plurality of polyimide layers by the thickness of the insulating layer is 0.95 or less, The first wiring and the second wiring are arranged on the first main surface and the second main surface, respectively.
9. The printed wiring board according to claim 8, The transmission loss per 100 mm of the first wiring at 50 GHz and the transmission loss per 100 mm of the second wiring at 50 GHz are 7 dB or less.
10. A multilayer printed wiring board, A plurality of printed wiring boards are provided. Each of the plurality of printed wiring boards is the printed wiring board according to claim 8 or 9.